Spherical copper powder for conductive paste as well as preparation method and application of spherical copper powder

By directly reacting the copper source with the reducing agent, the formation of copper oxide is avoided, and the uniform dispersion and uniform particle size preparation of spherical copper powder is achieved, which solves the problems of low spherical degree and poor particle size uniformity in the prior art, and simplifies production Process and reduce costs.

CN119057074APending Publication Date: 2024-12-03WUHE PILOT PHOTOELECTRIC MATERIALS CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411308732.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-19
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing liquid phase chemical reduction method for preparing spherical copper powder has problems such as low spherical morphology, poor particle size uniformity and complex production process, resulting in high production costs and low yields.

Method used

By mixing and heating the reducing agent, dispersant and pH adjusting agent, a reaction base liquid is formed and reacted directly with the copper source to avoid the Cu2+ forming copper oxide process, and control the reaction conditions to achieve the nucleation and growth of Cu nuclei. Prepare spherical copper powder with uniform dispersion and uniform size.

Benefits of technology

It realizes efficient preparation of spherical copper powder for conductive paste, with narrow particle size distribution and good dispersion, simplifies the production process, reduces production costs, and is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The invention provides spherical copper powder for conductive paste and a preparation method and application of the spherical copper powder. According to the preparation method, a copper source solution is added into a reaction base solution of a reducing agent, a dispersing agent and a pH regulator, and Cu < 2 + > is directly reduced into copper powder without being subjected to the process of generating cuprous oxide. Along with the addition of the copper source solution, the concentration of Cu < 2 + > gradually reaches the critical nucleation concentration, and at the moment, a large number of Cu crystal nuclei are formed in the reaction system. Meanwhile, due to the fact that a large amount of Cu < 2 + > is reduced, the concentration is rapidly reduced to the critical supersaturation concentration required by nucleation, nucleation does not occur in a reaction system under the condition, and crystal grains enter a growth stage. The nucleation process and the growth process of Cu crystal grains can be carried out separately, and a model of explosion nucleation and slow growth is met, so that the copper powder which is uniform in dispersion, uniform in size and narrow in particle size distribution can be prepared.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of conductive material preparation, and in particular relates to spherical copper powder for conductive paste and a preparation method and application thereof. Background Art

[0002] Micro-nano spherical copper powder refers to copper metal powder particles with high purity (≥99.5%), regular particle shape (spherical or approximately spherical) and certain chemical activity with a particle size distribution concentrated between 0.2~10 μm. Copper powder is widely used in many different fields because of its good electrical and thermal conductivity. On the one hand, copper powder can be used as the main raw material for preparing silver-coated copper powder. At present, with the growing market demand for ultrafine silver-coated copper powder, especially in the context of dual carbon, the rapid development of perovskite / silicon heterojunction stacked solar cells, the development of ultrafine silver-coated copper powder can not only meet the requirements of photovoltaic slurry, but also have huge cost competitive advantages. Silver-coated copper powder is generally prepared on the basis of ultrafine copper powder products. The quality of ultrafine copper powder will directly affect the performance of the final silver-coated copper. On the other hand, copper powder with high purity, good dispersibility, small particle size, narrow particle size distribution and good electrical conductivity is a good material for preparing MLCC electrodes. With the continuous expansion of the MLCC market, the demand for copper powder for MLCC terminal electrodes has been driven. However, due to the high surface activity and easy oxidation and deterioration of micro-nano copper powder, its production, preparation and storage are very difficult. At present, domestic copper powder for MLCC electrodes mainly relies on imports. Therefore, it is of great practical significance to prepare and produce an ultrafine copper powder with high purity, good dispersibility, narrow particle size distribution and good conductivity.

[0003] At present, the main methods for preparing spherical copper powder are liquid phase chemical reduction method, physical vapor deposition method, etc. Compared with the vapor deposition method, the equipment is complex and the energy consumption is high; the liquid phase chemical reduction method can control the morphology and particle size of copper powder, the production cost is low, and it is suitable for mass production. However, the copper powder prepared by the existing liquid phase reduction method has problems such as low sphericity, poor particle size uniformity, and long production process. Patent CN116021029 provides a method for preparing micro-nano spherical copper powder, which includes the steps of copper powder reduction, solid-liquid separation, copper powder cleaning, airflow drying, and grading treatment. However, this preparation method has the following defects: (1) The post-processing is complicated, airflow drying and sorting are required, and the yield is low (2) The airflow drying and sorting equipment has a complex structure and high production cost. Summary of the invention

[0004] In view of this, the object of the present invention is to provide a spherical copper powder for conductive paste and a preparation method and application thereof. The spherical copper powder for conductive paste prepared according to the preparation method is evenly dispersed and uniform in size.

[0005] To achieve this object, the present invention adopts the following technical solutions: In a first aspect, the present invention provides a method for preparing spherical copper powder for conductive paste, comprising the following steps: S1: mixing and heating a reducing agent, a dispersant and a pH adjusting agent to obtain a reaction base liquid, and controlling the pH of the reaction base liquid to be between 6 and 12; S2: Mixing the reaction base liquid and the copper source and reacting them to obtain spherical copper powder for conductive paste.

[0006] Preferably, the reducing agent is selected from any one or more of hydrazine hydrate, formaldehyde, ferrous sulfate, ascorbic acid or glucose.

[0007] Preferably, the dispersant is selected from any one or more of polyvinyl pyrrolidone, polyvinyl alcohol, polyethylene imine, oleic acid or sodium citrate.

[0008] Preferably, the pH adjuster is selected from any one or more of ammonia water, sodium hydroxide, ammonium carbonate, dilute nitric acid, dilute sulfuric acid, hydrochloric acid or acetic acid.

[0009] Preferably, the copper source is selected from any one or more of copper sulfate pentahydrate, anhydrous copper sulfate, copper acetate, copper nitrate, basic copper carbonate or copper chloride.

[0010] Preferably, the mass ratio of the dispersant to the copper in the copper source is (1-10):1.

[0011] Preferably, the molar ratio of the reducing agent to the copper in the copper source is (1-3):1.

[0012] Preferably, the heating temperature is 30-80°C.

[0013] Preferably, step S1 is: mixing and heating a reducing agent and a dispersant to obtain a reaction base liquid, mixing the reaction base liquid with a pH regulator, and controlling the pH of the reaction base liquid to be between 6 and 12.

[0014] Preferably, the oxygen content of the reaction bottom solution obtained in step S1 is below 20 mg / L.

[0015] Preferably, after the reaction in step S2 is completed, the obtained product is mixed with the coating liquid.

[0016] Preferably, the coating liquid is selected from any one or more of oleic acid, benzotriazole or stearic acid.

[0017] Preferably, the product and the coating liquid are mixed under stirring conditions, and the mixing time is 5 to 30 minutes.

[0018] Preferably, after the reaction in step S2 is completed, the solid-liquid separation is performed, and the obtained product is washed until the conductivity of the liquid is ≤10 μs / cm, and then dried to obtain spherical copper powder for conductive paste.

[0019] In a second aspect, the present invention provides a spherical copper powder for conductive paste prepared according to the above preparation method, wherein the particle size of the spherical copper powder for conductive paste is 100-6000 nm.

[0020] In a third aspect, the present invention provides a conductive material, which includes the spherical copper powder for conductive paste.

[0021] Compared with the prior art, the present invention has the following beneficial effects: The present invention provides a method for preparing spherical copper powder for conductive paste. The method comprises adding a copper source solution to a reaction base liquid of a reducing agent, a dispersant and a pH adjusting agent. 2+ It does not need to go through the process of generating cuprous oxide, but is directly reduced to copper powder. With the addition of copper source solution, Cu 2+ The concentration gradually reaches the critical nucleation concentration, at which point a large number of Cu nuclei will form in the reaction system. 2+ A large amount of reduction causes the concentration to drop rapidly to the critical supersaturation concentration required for nucleation. Under this condition, nucleation no longer occurs in the reaction system, and the grains enter the growth stage. The nucleation and growth processes of Cu grains can be carried out separately, which conforms to the model of "explosive nucleation and slow growth", so that copper powder with uniform dispersion, uniform size and narrow particle size distribution can be prepared.

[0022] The preparation method provided by the invention has simple steps and high efficiency, and is conducive to realizing industrialization or industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 is a SEM image of the copper powder obtained in Example 1; Figure 2 is a SEM image of the copper powder obtained in Example 2; Figure 3 is a SEM image of the copper powder obtained in Example 3; Figure 4 is a SEM image of the copper powder obtained in Example 4; Figure 5 is a SEM image of the copper powder obtained in Example 5; Figure 6 This is the SEM image of the copper powder obtained in Comparative Example 1. DETAILED DESCRIPTION

[0024] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] The present invention provides a method for preparing spherical copper powder for conductive paste, comprising the following steps: S1: mixing and heating a reducing agent, a dispersant and a pH adjusting agent to obtain a reaction base liquid, and controlling the pH of the reaction base liquid to be greater than 6, preferably between 6 and 12; S2: Mixing the reaction base liquid and the copper source and reacting them to obtain spherical copper powder for conductive paste.

[0026] According to the present invention, firstly, the reducing agent, dispersant and pH adjusting agent are mixed and heated to obtain a reaction base liquid. Wherein, the reducing agent is selected from any one or more of hydrazine hydrate, formaldehyde, ferrous sulfate, ascorbic acid or glucose; the dispersant is selected from any one or more of polyvinyl pyrrolidone, polyvinyl alcohol, polyethyleneimine, oleic acid or sodium citrate, preferably sodium citrate; the pH adjusting agent is selected from any one or more of ammonia water, sodium hydroxide, ammonium carbonate, dilute nitric acid, dilute sulfuric acid, hydrochloric acid or acetic acid. It should be noted that the pH adjusting agent includes both acidic substances and alkaline substances. When used in specific applications, it is adjusted in time according to the acidity or alkalinity of the reducing agent.

[0027] In some embodiments of the present invention, the reducing agent, dispersant and pH regulator are preferably mixed and heated to 30-80°C, preferably 40-70°C, and then kept warm to obtain a reaction base liquid. The reducing agent and dispersant are preferably mixed and heated to 30-80°C and then kept warm to obtain a reaction base liquid, which is then mixed with a pH regulator to control the pH of the reaction base liquid to be between 6 and 12. It should be noted that the pH value of the reaction base liquid will affect the reducing property of the reducing agent. When the pH value is low, the reducing ability of the reducing agent is insufficient; when the pH value is high, Cu 2+ With OH - Combined to generate Cu(OH)2, copper hydroxide is easily hydrolyzed into impurities such as copper oxide, which affects the purity of the reaction product. Therefore, the present invention preferably has a pH of 6 to 12 for the reaction base liquid. The mixing is preferably carried out under stirring conditions. In the present invention, the present invention preferably introduces a protective gas into the reaction system to remove oxygen, such as nitrogen, and controls the oxygen content of the reaction base liquid to below 20 mg / L, preferably below 18 mg / L, and then adds a copper source. This allows the reaction system to form a low-oxygen environment and reduce the possibility of copper powder being oxidized. The present invention has no particular limitation on the flow rate of the protective gas. In some embodiments of the present invention, 2 to 4 mL / min is preferred.

[0028] Then, according to the present invention, the reaction bottom liquid is mixed and reacted with a copper source. The mixing and reaction are preferably carried out under stirring conditions, the reaction temperature is carried out at the above-mentioned insulation temperature, and the reaction time is 1 to 5 h, preferably 2 to 4 h. Wherein, the copper source is selected from any one or more of copper sulfate pentahydrate, anhydrous copper sulfate, copper acetate, copper nitrate, basic copper carbonate or copper chloride. In some embodiments of the present invention, the mass of the dispersant in the reaction droplet is more than 1 times the mass of the copper source. Specifically, the mass ratio of the dispersant in the reaction droplet to the copper in the copper source is preferably (1 to 10): 1, more preferably (1.5 to 5): 1; specifically, the molar ratio of copper in the reducing agent and the copper source is preferably (1 to 3): 1, more preferably (2 to 3): 1.

[0029] The present invention preferably controls the amount of the above dispersant and reducing agent because the amount of the dispersant affects the morphology of the product. When the amount of the dispersant is large, the sphericity of the product is higher and the dispersibility is better. 2+ The molar ratio affects the reaction time and product particle size. Generally, the amount of reducing agent used needs to be more than the theoretical amount.

[0030] It should be noted that the present invention can obtain spherical copper powder with uniform particle size and excellent dispersibility through the combination of the above raw materials.

[0031] In some preferred embodiments of the present invention, after the reaction in step S2 is completed, the obtained product is preferably mixed with a coating liquid, and the coating liquid is selected from any one or more of oleic acid, benzotriazole or stearic acid, preferably oleic acid. The mixing is carried out under stirring conditions, and the mixing time is 5 to 30 minutes, preferably 10 to 20 minutes.

[0032] This step can not only inhibit the oxidation of copper powder during the subsequent cleaning and drying process, but also will not interfere with the preparation and synthesis of copper powder. Compared with the solution of adding a coating agent during post-treatment such as copper powder drying, this process is simpler and more convenient.

[0033] In some embodiments of the present invention, after the reaction is completed, solid-liquid separation is preferably performed to obtain wet copper powder, which is washed with pure water for more than 2 times, preferably 2 to 3 times, until the conductivity of the liquid is ≤10 µs / cm to ensure the purity of the copper powder, and then the wet copper powder is dried, preferably in a vacuum drying oven, at 60 to 120°C for 3 to 5 h, preferably at 80 to 100°C for 3.5 to 4 h, to obtain the target product.

[0034] In summary, in some specific embodiments of the present invention, the preparation method of the spherical copper powder for conductive paste is as follows: A 5L glass beaker is selected as a reaction container, and a reducing agent, a dispersant and pure water are added thereto in sequence to form a solution as a reaction base solution; a copper source and water are mixed to form a copper source solution; a coating agent and water are mixed to form a coating agent solution; The reaction vessel is installed in a water bath, the temperature is set to a specific value between 30 and 80 °C, and a stirring device and a ventilation device are installed; the coating agent solution, the copper source solution and the reaction base solution are heated to the corresponding set values ​​and then kept warm; the stirrer above the reaction vessel is turned on, the stirring speed is controlled at 300 to 500 rpm, and an appropriate amount of ammonia water is added to the reaction base solution to adjust the pH to the target range; nitrogen gas with a flow rate of 2 to 4 mL / min is introduced into the reaction base solution to reduce the dissolved oxygen content of the solution to 20 mg / L; after 10 to 30 min, the prepared copper source solution is introduced into the reaction vessel to mix it with the reducing solution and start the reaction. During the reaction, the temperature is kept constant at the set °C, and the nitrogen flow rate is maintained at 2 to 4 mL / min; after 2 to 5 h, the coating agent solution is added to the mixed reaction solution, and the reaction is continued for 5 to 30 min. min; stop the reaction, close the nitrogen valve, stirrer and constant temperature water bath, and take out the reaction vessel; after solid-liquid separation of the mixture in the reaction vessel, continue to wash the solid wet powder with pure water for 3 to 4 times until the conductivity of the supernatant is ≤10 µs / cm; then put the wet powder into a vacuum drying oven, set the temperature to 60~120℃, and dry it to obtain the target product-copper powder.

[0035] The preparation method provided by the present invention adds a copper source solution to the reaction base liquid of a reducing agent, a dispersant and a pH regulator, and Cu 2+ It does not need to go through the process of generating cuprous oxide, but is directly reduced to copper powder. With the addition of copper source solution, Cu 2+ The concentration gradually reaches the critical nucleation concentration, at which point a large number of Cu nuclei will form in the reaction system. 2+ A large amount of reduction causes the concentration to drop rapidly to the critical supersaturation concentration required for nucleation. Under this condition, nucleation no longer occurs in the reaction system, and the grains enter the growth stage. The nucleation and growth processes of Cu grains can be carried out separately, which conforms to the model of "explosive nucleation and slow growth", so that copper powder with uniform dispersion, uniform size and narrow particle size distribution can be prepared.

[0036] In the present invention, the particle size of the product is related to factors such as the type of reducing agent and the type of copper source used. According to SEM characterization, for the same reducing agent and copper source, the spherical copper powder for the conductive paste prepared by the preparation method of the present invention is evenly dispersed, has a uniform particle size, and has a narrow particle size distribution (e.g. Figures 1 to 5 As shown). According to calculation, the particle size can be 100~6000 nm.

[0037] The present invention also provides a conductive material, which comprises spherical copper powder for conductive paste prepared by the above preparation method.

[0038] In order to further illustrate the present invention, the following examples are provided for detailed description. The experimental raw materials used in the following examples of the present invention are all common commercially available products. Example 1

[0039] A 5L glass beaker was selected as a reaction container, and 131.2g of ascorbic acid, 50g of polyvinyl pyrrolidone and 2kg of pure water were added thereto in sequence to form a solution as a reaction base liquid; 187.5g of copper sulfate pentahydrate and 250g of water were mixed to form a 3mol / L copper source solution; 1g of benzotriazole and 50g of water were mixed to form a coating agent solution; the reaction container was installed in a water bath, the temperature was set to 70°C, and a stirring device and a ventilation device were installed; the coating agent solution, the copper source solution and the reaction base liquid were heated to 70°C respectively and then kept warm; the stirrer above the reaction container was turned on, the stirring speed was controlled at 300rpm, and an appropriate amount of ammonia water was added to the reaction base liquid to adjust the pH to 9; a flow was introduced into the reaction base liquid The nitrogen gas was added at a rate of 2 mL / min to reduce the dissolved oxygen content of the solution to 20 mg / L; after 10 minutes, the prepared copper source solution was introduced into the reaction vessel to mix with the reducing solution and start the reaction. During the reaction, the temperature was kept constant at 70°C and the nitrogen flow rate was maintained at 2 mL / min; after 2 hours, the coating agent solution was added to the mixed reaction solution and the reaction was continued for 10 minutes; the reaction was stopped, the nitrogen valve, the stirrer and the constant temperature water bath were closed, and the reaction vessel was taken out; after the mixture in the reaction vessel was separated from the solid and liquid, the solid wet powder was washed with pure water for 3 to 4 times until the conductivity of the supernatant was ≤10µs / cm; the wet powder was then placed in a vacuum drying oven, the temperature was set to 80°C, and copper powder was obtained after drying for 3 hours. Example 2

[0040] A 5L glass beaker was used as the reaction vessel, and 143.25g of formaldehyde (40%), 50g of polyvinyl pyrrolidone and 2kg of pure water were added to the beaker in sequence to form a solution as the reaction base solution; 187.5g of copper sulfate pentahydrate and 500g of water were mixed to form a 1.5mol / L copper source solution; 20g of oleic acid ethanol solution (oleic acid concentration was 1.7%) and 50g of water were added to form a coating agent solution; the reaction vessel was placed in a water bath and the temperature was set to 70 ℃, and install the stirring device and ventilation device; heat the coating agent solution, copper source solution and reaction base solution to 70℃ respectively and then keep warm; turn on the stirrer above the reaction container, control the stirring speed at 300rpm, and add an appropriate amount of sodium hydroxide to the reaction base solution to adjust the pH to 12; introduce nitrogen gas with a flow rate of 2mL / min into the reaction base solution to reduce the dissolved oxygen content of the solution to 20mg / L; after 10min, introduce the prepared copper source solution into the reaction container, mix it with the reducing solution, start the reaction, and the reaction During the process, the temperature was kept constant at 70°C, and the nitrogen flow rate was maintained at 2 mL / min. After 2 hours, the coating agent solution was added to the mixed reaction solution, and the reaction was continued for 10 minutes. The reaction was stopped, the nitrogen valve, the stirrer and the constant temperature water bath were closed, and the reaction vessel was taken out. After the mixture in the reaction vessel was separated from the solid and liquid, the solid wet powder was washed with pure water for 3 to 4 times until the conductivity of the supernatant was ≤10µs / cm. The wet powder was then placed in a vacuum drying oven, the temperature was set to 80°C, and copper powder was obtained after drying for 3 hours. Example 3

[0041] A 5L glass beaker was used as the reaction vessel, and 70.5g of hydrazine hydrate (80%), 50g of polyvinyl pyrrolidone and 2kg of pure water were added to the beaker in sequence to form a solution as the reaction base solution; 187.5g of copper sulfate pentahydrate and 500g of water were mixed to form a 1.5mol / L copper source solution; 20g of oleic acid ethanol solution (oleic acid concentration was 1.7%) and 50g of water were added to form a coating agent solution; the reaction vessel was placed in a water bath and the temperature was set to 65 ℃, and install the stirring device and ventilation device; heat the coating agent solution, copper source solution and reaction base solution to 65℃ respectively and then keep warm; turn on the stirrer above the reaction container, control the stirring speed at 300rpm, and add an appropriate amount of ammonia water to the reaction base solution to adjust the pH to 9; introduce nitrogen gas with a flow rate of 2mL / min into the reaction base solution to reduce the dissolved oxygen content of the solution to 20mg / L; after 10min, introduce the prepared copper source solution into the reaction container, mix it with the reducing solution, start the reaction, and the reaction is During the process, the temperature was kept constant at 65°C, and the nitrogen flow rate was maintained at 2 mL / min. After 2 hours, the coating agent solution was added to the mixed reaction solution, and the reaction was continued for 10 minutes. The reaction was stopped, the nitrogen valve, the stirrer and the constant temperature water bath were closed, and the reaction vessel was taken out. After the mixture in the reaction vessel was separated into solid and liquid, the solid wet powder was washed with pure water for 3 to 4 times until the conductivity of the supernatant was ≤10µs / cm. The wet powder was then placed in a vacuum drying oven, the temperature was set to 80°C, and copper powder was obtained after drying for 3 hours. Example 4

[0042] A 5L glass beaker was used as a reaction vessel, and 477g of ferrous sulfate heptahydrate, 100g of sodium citrate and 2kg of pure water were added to the beaker in sequence to form a solution as a reaction base solution; 150g of cuprous chloride and 400g of water were mixed to form a 0.15mol / L copper source solution; 20g of oleic acid ethanol solution (oleic acid concentration was 1.7%) and 50g of water were added to form a coating agent solution; the reaction vessel was placed in a water bath and the temperature was set to 60 ℃, and install the stirring device and ventilation device; heat the coating agent solution, copper source solution and reaction base solution to 60℃ respectively and then keep warm; turn on the stirrer above the reaction container, control the stirring speed at 300rpm, and add an appropriate amount of ammonia water to the reaction base solution to adjust the pH to 6; introduce nitrogen gas with a flow rate of 2mL / min into the reaction base solution to reduce the dissolved oxygen content of the solution to 20mg / L; after 10min, introduce the prepared copper source solution into the reaction container at one time to mix it with the reducing solution instantly, start the reaction, and react During the reaction, the temperature was kept constant at 60°C and the nitrogen flow rate was maintained at 2 mL / min. After 2 hours, the coating agent solution was added to the mixed reaction solution and the reaction was continued for 10 minutes. The reaction was stopped, the nitrogen valve, the stirrer and the constant temperature water bath were closed, and the reaction vessel was taken out. After the mixture in the reaction vessel was separated into solid and liquid, the solid wet powder was washed with pure water for 3 to 4 times until the conductivity of the supernatant was ≤10µs / cm. The wet powder was then placed in a vacuum drying oven, the temperature was set to 80°C, and copper powder was obtained after drying for 3 hours. Example 5

[0043] A 5L glass beaker was selected as a reaction container, and 218.3g of ascorbic acid, 100g of sodium citrate and 2kg of pure water were added thereto in sequence to form a solution as a reaction base liquid; 187.5g of copper sulfate pentahydrate and 250g of water were mixed to form a 3mol / L copper source solution; 1g of benzotriazole and 50g of water were mixed to form a coating agent solution; the reaction container was installed in a water bath, the temperature was set to 70°C, and a stirring device and a ventilation device were installed; the coating agent solution, the copper source solution and the reaction base liquid were heated to 70°C respectively and then kept warm; the stirrer above the reaction container was turned on, the stirring speed was controlled at 300rpm, and an appropriate amount of ammonia water was added to the reaction base liquid to adjust the pH to 8; nitrogen gas with a flow rate of 2mL / min was introduced into the reaction base liquid to reduce the dissolved oxygen content of the solution to 20mg / L; after 10min, the prepared copper source solution was introduced into the reaction container to mix it with the reducing solution, and the reaction was started. During the process, the temperature was kept constant at 70°C, and the nitrogen flow rate was maintained at 2 mL / min. After 2 hours, the coating agent solution was added to the mixed reaction solution, and the reaction was continued for 10 minutes. The reaction was stopped, the nitrogen valve, the stirrer and the constant temperature water bath were closed, and the reaction vessel was taken out. After the mixture in the reaction vessel was separated from the solid and liquid, the solid wet powder was washed with pure water for 3 to 4 times until the conductivity of the supernatant was ≤10µs / cm. The wet powder was then placed in a vacuum drying oven, the temperature was set to 80°C, and the copper powder was obtained after drying for 3 hours.

[0044] The SEM images of the copper powders obtained in the above examples 1 to 5 are as follows: Figures 1 to 5 shown.

[0045] Comparative Example 1 A 5L glass beaker was used as the reaction vessel, and 187.5g of copper sulfate pentahydrate and 1500g of water were added to the beaker to prepare a 0.15mol / L copper source reaction base solution; 218.3g of ascorbic acid, 100g of sodium citrate and 1kg of pure water were mixed to prepare a solution as an additive solution; 20g of oleic acid ethanol solution (oleic acid concentration was 1.7%) and 50g of water were added to prepare a coating agent solution; the reaction vessel was placed in a water bath and the temperature was set to 60 ℃, and install the stirring device and ventilation device; heat the coating agent solution, copper source solution and reaction base solution to 60℃ respectively and then keep warm; turn on the stirrer above the reaction container, control the stirring speed at 300rpm, and add appropriate amount of ammonia water to the reaction base solution to adjust the pH to 8; introduce nitrogen gas with a flow rate of 2mL / min into the reaction base solution to reduce the dissolved oxygen content of the solution to 20mg / L; after 10 minutes, introduce the prepared reducing agent and other additives into the reaction container at one time to mix them with the copper source solution instantly to start the reaction During the reaction, the temperature was kept constant at 60°C and the nitrogen flow rate was maintained at 2 mL / min. After 2 hours, the coating agent solution was added to the mixed reaction solution and the reaction was continued for 10 minutes. The reaction was stopped, the nitrogen valve, the stirrer and the constant temperature water bath were closed, and the reaction vessel was taken out. After the mixture in the reaction vessel was separated into solid and liquid, the solid wet powder was washed with pure water for 3 to 4 times until the conductivity of the supernatant was ≤10µs / cm. The wet powder was then placed in a vacuum drying oven, the temperature was set to 80°C, and copper powder was obtained after drying for 3 hours.

[0046] The SEM images of the copper powder obtained in Comparative Example 1 are as follows: Figure 6 As shown, it can be seen that the copper powder agglomerates.

[0047] Performance Testing The test method is as follows: The oxygen content and carbon content are measured by infrared absorption method; the morphology is tested by field emission scanning electron microscopy; the yield refers to the ratio of the mass of copper powder obtained after drying to the theoretical mass of copper powder.

[0048] The test results are shown in Table 1 below: Table 1

[0049] Combination Figures 1 to 6 As can be seen from Table 1, the powders prepared with reducing solution, dispersing solution, etc. as base liquids have a spherical morphology, good dispersibility, and carbon and oxygen contents are both less than 2500 ppm, excellent oxidation resistance, high yield, and meet the requirements of mass production of products. In Comparative Example 1, the copper powder prepared by the method of using copper source solution as base liquid and adding reducing agent and dispersing agent later has irregular morphology and powder agglomeration.

[0050] The above description of the disclosed embodiments enables those skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A method for preparing spherical copper powder for conductive paste, characterized in that: The following steps are involved: S1: mixing and heating a reducing agent, a dispersant and a pH adjusting agent to obtain a reaction base liquid, and controlling the pH of the reaction base liquid to be between 6 and 12; S2: Mixing the reaction base liquid and the copper source and reacting them to obtain spherical copper powder for conductive paste.

2. The preparation method according to claim 1, characterized in that: The reducing agent is selected from any one or more of hydrazine hydrate, formaldehyde, ferrous sulfate, ascorbic acid or glucose; The dispersant is selected from any one or more of polyvinyl pyrrolidone, polyvinyl alcohol, polyethylene imine, oleic acid or sodium citrate; The pH regulator is selected from any one or more of ammonia water, sodium hydroxide, ammonium carbonate, dilute nitric acid, dilute sulfuric acid, hydrochloric acid or acetic acid; The copper source is selected from any one or more of copper sulfate pentahydrate, anhydrous copper sulfate, copper acetate, copper nitrate, basic copper carbonate or copper chloride.

3. The preparation method according to claim 1 or 2, characterized in that: The mass ratio of the dispersant to the copper in the copper source is (1-10):1; The molar ratio of the reducing agent to the copper in the copper source is (1-3):

1.

4. The preparation method according to any one of claims 1 to 3, characterized in that The heating temperature is 30-80°C.

5. The preparation method according to any one of claims 1 to 4, characterized in that Step S1 is: mixing and heating a reducing agent and a dispersant to obtain a reaction base liquid, and mixing the reducing agent and a dispersant to control the pH of the reaction base liquid to be between 6 and 12; The oxygen content of the reaction bottom solution obtained in step S1 is below 20 mg / L.

6. The preparation method according to any one of claims 1 to 5, characterized in that After the reaction in step S2 is completed, the obtained product is mixed with the coating liquid; The coating liquid is selected from any one or more of oleic acid, benzotriazole or stearic acid.

7. The preparation method according to claim 6, characterized in that: The product and the coating liquid are mixed under stirring conditions, and the mixing time is 5 to 30 minutes.

8. The preparation method according to any one of claims 1 to 7, characterized in that After the reaction in step S2 is completed, the solid and liquid are separated, and the obtained product is washed until the conductivity of the liquid is ≤10 μs / cm, and then dried to obtain spherical copper powder for conductive paste.

9. The spherical copper powder for conductive paste prepared by the preparation method according to any one of claims 1 to 8, characterized in that: The particle size of the spherical copper powder for the conductive paste is 100-6000 nm.

10. A conductive material, characterized in that: The invention comprises spherical copper powder for conductive paste prepared by the preparation method according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Preparation method of micro-nano spherical copper powder

    CN116021029A