Polishing apparatus, polishing method, and wafer

By using air film and multi-region pressure design in the polishing device, the problem of uneven stress on the edge of the top silicon layer is solved, and uniform removal of the edge of the top silicon layer is achieved, and the performance of the wafer is improved.

CN119057676APending Publication Date: 2024-12-03TIANJIN HUANYAO NEW MATERIAL TECHNOLOGY CO LTD
View PDF 15 Cites 0 Cited by

Patent Information

Application Number
CN202411390940.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-30
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

During the polishing process of the wafer, the edges of the top silicon layer are subjected to uneven stress, resulting in uneven edge removal, affecting the performance of the wafer.

Method used

By adopting a polishing device, by providing an air film on the caster, the force range of the air film includes a first area and a second area, the pressure of the first area is slightly greater than the second area, and combined with a slope and a multi-region pressure partition design, Ensure uniformity of the applied pressure at the edge of the top silicon layer.

Benefits of technology

The uniform removal of the edge of the top silicon layer is achieved, and the performance of the wafer is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119057676A_ABST
    Figure CN119057676A_ABST
Patent Text Reader

Abstract

The invention discloses a polishing device, a polishing method and a wafer, and the polishing device comprises a polishing head which is provided with an air film on one side facing a substrate, so as to transmit pressure to the substrate through the air film; the force application range of the gas film comprises a first area and a second area, and the first area is arranged around the second area; wherein the first area has a first pressure P1; the second region has a second pressure P2 satisfying: P1gt; p2. According to the polishing device, the polishing method and the wafer provided by the invention, the edge removal uniformity of the top silicon layer can be improved, so that the use performance of the wafer is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of semiconductor manufacturing technology, and in particular to a polishing device, a polishing method and a wafer. Background Art

[0002] At present, the preparation of wafers mainly includes oxygen injection isolation technology, intelligent stripping technology and bonding thinning technology. Among them, bonding thinning technology is a process of thinning the device layer substrate after bonding the support substrate and the device layer substrate. It has attracted attention due to its simple process and low cost. Before thinning, it is necessary to use a grinding process to remove the unbonded part of the edge of the device layer substrate to form a width. During polishing, the top silicon layer will be unevenly stressed at the edge due to the width, which will further lead to uneven edge removal, which will directly affect the performance of the wafer. Summary of the invention

[0003] The purpose of the present application is to provide a polishing device, a polishing method and a wafer, which can improve the uneven force on the edge of the top silicon layer, achieve uniform removal of the edge of the top silicon layer, and improve the performance of the wafer.

[0004] The present application provides a polishing device, comprising:

[0005] A polishing head, wherein an air film is provided on a side of the polishing head facing the substrate so as to transmit pressure to the substrate through the air film;

[0006] The force application range of the air film includes a first area and a second area, and the first area is arranged around the second area;

[0007] The first region has a first pressure P 1 The second region has a second pressure P 2 , satisfy: P 1 >P 2 .

[0008] In some embodiments, the first region is provided with a slope, the slope has a first inclined surface, and a first angle α is formed between the first inclined surface and an extension direction of the lateral direction of the polishing head, satisfying: 5°≤α≤70°.

[0009] In some embodiments, the slope has a bottom surface extending along the transverse direction, and the bottom surface has a first length L that satisfies: 2 mm ≤ L ≤ 15 mm.

[0010] In some embodiments, the first region has a second inclined surface on a side facing the substrate; an extension direction of the second inclined surface and an extension direction of the lateral direction of the polishing head have a second angle β, satisfying: 5°≤β≤70°.

[0011] In some embodiments, the force application range of the air film further includes a third region, and the third region is arranged around the first region; the third region has a third pressure P 3 , satisfy: P 2 <P 1 ≤P 3 .

[0012] In some embodiments, the second region includes a first sub-region, a second sub-region, and a third sub-region; the second sub-region is disposed around the first sub-region; and the third sub-region is disposed around the second sub-region.

[0013] In some embodiments, the first sub-region has a fourth pressure P 4 , the second sub-region has a fifth pressure P 5 , the third sub-region has a sixth pressure P 6 , at least one of the following conditions is met:

[0014] (a)P 4 <P 5 <P 6 ;

[0015] (b)P 4 <P 5 ≤P 6 ;

[0016] (c)P 4 ≤P 5 <P 6 ;

[0017] (d)P 4 ≤P 5 ≤P 6 ;

[0018] (e)P 4 <P 5 And P 5 =P 6 ;

[0019] (f)P 4 =P 5 And P 5 <P 6 .

[0020] In some embodiments, the polishing device further comprises a polishing table; the polishing head has a first rotation speed V 1 , the polishing table has a second rotation speed V 2 , meet: 1 rpm ≤|V 1 -V 2 |≤10 rev / min.

[0021] Accordingly, the present application also provides a polishing method, comprising:

[0022] Providing a polishing head, wherein an air film is provided on a side of the polishing head facing the substrate;

[0023] transmitting pressure to the substrate through the air film, wherein the force application range of the air film includes a first area and a second area, and the first area is arranged around the second area;

[0024] The first region has a first pressure P 1 The second region has a second pressure P 2 , satisfy: P 1 >P 2 .

[0025] In some embodiments, the method is used for polishing a wafer including the substrate, wherein the wafer includes an oxide layer and a top silicon layer, wherein the oxide layer is located on a side of the substrate, and the top silicon layer is located on a side of the oxide layer away from the substrate;

[0026] A side of the substrate away from the oxide layer is adsorbed onto the gas film to polish the top silicon layer.

[0027] In some embodiments, the wafer has a first polishing area and a second polishing area, the first polishing area is arranged around the second polishing area, the first polishing area is arranged corresponding to the first area; the second polishing area is arranged corresponding to the second area.

[0028] In some embodiments, the wafer has a step, and the step is located in the first polishing area; the step has a width W, satisfying: 0.5 mm≤W≤4 mm.

[0029] In some embodiments, the step of polishing the top silicon layer comprises:

[0030] contacting the top silicon layer with a polishing table;

[0031] removing at least a portion of the top silicon layer located in the first polishing area;

[0032] At least a portion of the top silicon layer located in the second polishing area is removed.

[0033] In some embodiments, the blasting head has a first rotation speed V 1 ; The polishing table has a second speed V 2 , meet: 1 rpm ≤|V 1 -V 2 |≤10 rev / min.

[0034] In some embodiments, the top silicon layer in the first polishing area has a first removal amount D1 , the top silicon layer located in the second polishing area has a second removal amount D 2 , satisfying: 0≤|D 1 -D 2 |≤0.5μm.

[0035] In some embodiments, the first removal amount D 1 and the second removal amount D 2 , satisfying: 3.5μm≤D 1 ≤5μm and 3.5μm≤D 2 ≤5μm.

[0036] In some embodiments, along the lateral direction of the polishing head, the first polishing area has a second length M that satisfies: 4 mm ≤ M ≤ 20 mm.

[0037] Correspondingly, the present application also provides a wafer, including a wafer polished by the polishing device as described above; or, including a wafer polished by the polishing method as described above.

[0038] The beneficial effects of this application are:

[0039] The present application provides a polishing device, a polishing method and a wafer, wherein the polishing device comprises: a polishing head, an air film is provided on a side of the polishing head facing the substrate, so as to transmit pressure to the substrate through the air film; the force application range of the air film comprises a first area and a second area, and the first area is arranged around the second area; wherein the first area has a first pressure P 1 The second region has a second pressure P 2 , satisfy: P 1 >P 2 The present application provides a polishing device, a polishing method and a wafer, which divides the gas film into zones and controls the first pressure P in the first zone. 1 Slightly greater than the second pressure P in the second region 2 , which can improve the uniformity of the top silicon layer edge removal, thereby improving the performance of the wafer. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 A schematic diagram of the structure of the wafer provided for this application;

[0041] Figure 2 A schematic diagram of the structure after a wafer is polished using an existing polishing device;

[0042] Figure 3 A schematic diagram of the structure of the polishing device provided in this application;

[0043] Figure 4A schematic diagram of the structure of the air film in the polishing device provided in this application;

[0044] Figure 5 for Figure 4 The first cross-sectional view along line AB;

[0045] Figure 6 for Figure 5 A zoomed-in view of the middle slope;

[0046] Figure 7 is a schematic diagram of the decomposition of the force applied to the first inclined surface;

[0047] Figure 8 for Figure 4 The second cross-sectional view along line AB;

[0048] Fig. 9 for Figure 8 A magnified view of the second inclined surface;

[0049] Fig.10 A flow chart of the polishing method provided for this application;

[0050] Fig.11 A schematic diagram of the structure of a wafer provided in the present application being polished in a polishing device;

[0051] Fig.12 This is a schematic diagram of the structure of the wafer provided in this application before and after polishing by the polishing device.

[0052] In the accompanying drawings, the components represented by the reference numerals are as follows:

[0053] 10. Polishing head; 11. Polishing head; 12. Air film; 121. First area; 122. Second area; 1221. First sub-area; 1222. Second sub-area; 1223. Third sub-area; 123. Third area; 13. Slope; 131. First inclined surface; 132. Bottom surface; 14. Second inclined surface; 20. Polishing table; 30. Wafer; 31. First polishing area; 32. Second polishing area; 33. Step; 301. Substrate; 302. Oxide layer; 303. Top silicon layer. DETAILED DESCRIPTION

[0054] The technical solution of the present application will be described clearly and completely below in conjunction with the embodiments and drawings of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present application. The various embodiments of the present application may exist in the form of a range; it should be understood that the description in the form of a range is only for convenience and simplicity, and should not be understood as a rigid limitation on the scope of the present application; therefore, it should be considered that the range description has specifically disclosed all possible sub-ranges and single values ​​within the range. For example, it should be considered that the range description from 1 to 6 has specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which are applicable regardless of the range. In addition, whenever a numerical range is indicated in this article, it is meant to include any quoted numbers (fractions or integers) within the indicated range.

[0055] like Figure 1-Figure 2 As shown, the wafer 30 includes a substrate 301, an oxide layer 302 and a top silicon layer 303. The oxide layer 302 is located on one side of the substrate 301; the top silicon layer 303 is located on a side of the oxide layer 302 away from the substrate 301. The wafer 30 includes a silicon-on-insulator wafer.

[0056] During the polishing process of the wafer 30 to be polished, the polishing head 11 contacts the substrate 301 and applies pressure, and the pressure is then transferred to the top silicon layer 303 through the substrate 301. The top silicon layer 303 is subjected to uneven force at the edge, resulting in uneven removal of the edge of the top silicon layer 303. Figure 2 .

[0057] In some embodiments, the wafer 30 has a first polishing area 31 and a second polishing area 32 ; the first polishing area 31 is disposed around the second polishing area 32 .

[0058] Specifically, the first polishing area 31 and the second polishing area 32 may be arranged in concentric circles.

[0059] In some embodiments, the wafer 30 has a step 33 , and the step 33 is located in the first polishing area 31 ; the step 33 has a width W, which satisfies: 0.5 mm≤W≤4 mm.

[0060] Specifically, the width W may include a range consisting of one or two of 0.5mm, 1mm, 1.5mm, 2mm, 2.5mm, 3mm, 3.5mm, and 4mm. It is worth noting that the value of the width W is only given for example, and as long as it is within the range of 0.5mm≤W≤4mm, it falls within the scope of protection of this application.

[0061] The present application provides a polishing device, which can improve the uneven force on the edge of the top silicon layer 303 during the polishing process, so as to achieve uniform removal of the edge of the top silicon layer 303.

[0062] like Figure 3-Figure 9 As shown, a polishing device includes: a polishing head 11 and an air film 12, wherein the air film 12 is located on a side of the polishing head 11 facing a substrate 301, so as to transmit pressure to the substrate 301 through the air film 12; the force application range of the air film 12 includes a first area 121 and a second area 122, wherein the first area 121 is arranged around the second area 122; wherein the first area 121 has a first pressure P 1 The second region 122 has a second pressure P 2 , satisfy: P 1 >P 2 .

[0063] Specifically, the first area 121 and the second area 122 may be arranged in concentric circles. The polishing head 11 and the air film 12 constitute a polishing head 10 of the polishing device.

[0064] In this application, the first pressure P of the first area 121 is controlled 1 Slightly greater than the second pressure P of the second region 122 2 , it can be achieved that the pressure applied to the first polishing area 31 is slightly greater than the pressure applied to other areas of the top silicon layer 303, that is, the pressure applied to the area where the step 33 is located is slightly greater than the pressure applied to other areas of the top silicon layer 303, which can improve the uniformity of edge removal of the top silicon layer 303, thereby obtaining a top silicon layer 303 with uniform film thickness.

[0065] In some embodiments, the first region 121 is provided with a slope 13, the slope 13 has a first inclined surface 131, and a first angle α is formed between the first inclined surface 131 and the extension direction of the transverse direction X of the polishing head 11, satisfying: 5°≤α≤70°. The longitudinal direction Y of the polishing head 11 intersects with the transverse direction X, and specifically, the longitudinal direction Y is perpendicular to the transverse direction X.

[0066] Specifically, the first angle α may include a range consisting of one or two of 5°, 10°, 15°, 20°, 25°, 30°, 35°, 40°, 45°, 50°, 55°, 60°, 65°, and 70°. It is worth noting that the value of the first angle α is only given as an example, and as long as it is within the range of 5°≤α≤70°, it falls within the scope of protection of this application.

[0067] like Figure 7 As shown in the figure, when the force applied by the air film 12 to the first inclined surface 131 is F, F is decomposed along the transverse direction X and the longitudinal direction Y. It can be seen that the first force in the transverse direction X is F 1 , satisfying: F 1= Fsinα; The second force in the longitudinal direction Y is F 2 , satisfying: F 2 = Fcosα. That is, the second force F is applied to the first polishing area 31 2 , satisfying: F 2 < F. Specifically, the transverse direction X is perpendicular to the longitudinal direction Y.

[0068] Therefore, in this application, by providing a ramp 13 in the first region 121 and controlling the first angle α between the extension direction of the first inclined surface 131 and the transverse direction X of the polishing head 11, satisfying: 5° ≤ α ≤ 70°, the force F applied to the ramp 13 by the air film 12 can be decomposed, so that the force applied to the first polishing area 31 can be slightly greater than the force applied to other areas of the top silicon layer 303. That is, the pressure applied to the area where the step 33 is located is slightly greater than the pressure applied to other areas of the top silicon layer 303, which can improve the uniformity of the edge removal of the top silicon layer 303, and thus obtain a top silicon layer 303 with uniform film thickness.

[0069] In some embodiments, the ramp 13 has a bottom surface 132 extending along the transverse direction X, and the bottom surface 132 has a first length L, satisfying: 2 mm ≤ L ≤ 15 mm.

[0070] It can be understood that the bottom surface 132 is in contact with the substrate 301. The first length L of the bottom surface 132 should be less than or equal to the first width L of the first region 121 along the transverse direction X 1 .

[0071] Specifically, the first length L may include a value within the range composed of one or both of 2 mm, 5 mm, 8 mm, 10 mm, 12 mm, and 15 mm. It should be noted that the value of the first length L is only given exemplarily, and as long as it is within the range of 2 mm ≤ L ≤ 15 mm, it falls within the scope of protection of this application.

[0072] By decomposing the force F applied to the first inclined surface 131, the force applied to the first polishing area 31 can be made slightly greater than the force applied to other areas of the top silicon layer 303, which can improve the uniformity of the edge removal of the top silicon layer 303, and thus obtain a top silicon layer 303 with uniform film thickness.

[0073] As Figure 8-Figure 9 shown, in some embodiments, the side of the first region 121 facing the substrate 301 has a second inclined surface 14; the extension direction of the second inclined surface 14 and the extension direction of the transverse direction X of the polishing head 11 have a second angle β, satisfying: 5° ≤ β ≤ 70°.

[0074] It can be understood that there is a gap (not shown in the figure) between the second inclined surface 14 and the substrate 301.

[0075] Specifically, the second angle β may include a range consisting of one or two of 5°, 10°, 15°, 20°, 25°, 30°, 35°, 40°, 45°, 50°, 55°, 60°, 65°, and 70°. It is worth noting that the value of the second angle β is only given as an example, and as long as it is within the range of 5°≤β≤70°, it falls within the scope of protection of this application.

[0076] Similarly, if the force applied by the air film 12 to the second inclined surface 14 is F, F is decomposed along the transverse direction X and the longitudinal direction Y. It can be seen that the first force in the transverse direction X is F 1 , satisfying: F 1 =Fsinβ; the second force in the longitudinal direction Y is F 2 , satisfying: F 2 =Fcosβ. That is, the second force F is applied to the first polishing area 31. 2 , satisfying: F 2 <F。

[0077] The present application sets a second bevel 14 in the first area 121 and controls the second angle β of the second bevel 14 to satisfy: 5°≤β≤70°. The force F applied by the air film 12 to the second bevel 14 can be decomposed, so that the force applied to the first polishing area 31 can be slightly greater than the force applied to other areas of the top silicon layer 303. The uniformity of edge removal of the top silicon layer 303 can be improved, thereby obtaining a top silicon layer 303 with uniform film thickness.

[0078] In some embodiments, the force application range of the air film 12 also includes a third region 123, and the third region 123 is arranged around the first region 121; the third region 123 has a third pressure P 3 , satisfy: P 2 <P 1 ≤P 3 .

[0079] Specifically, the third area 123 and the first area 121 may be arranged in concentric circles. The third area 123 is a retaining ring of the air film 12. The air film 12 located in the third area 123 covers both ends of the wafer 30 to fix the wafer 30 for polishing.

[0080] In this application, the first pressure P of the first area 121 is controlled 1 , the second pressure P of the second region 122 2 , the third pressure P of the third region 123 3 , satisfy: P 2 <P 1 ≤P 3, the wafer 30 can be fixed and polished, and the uniformity of edge removal of the top silicon layer 303 can be improved, thereby obtaining a top silicon layer 303 with uniform film thickness.

[0081] In some embodiments, the second region 122 includes a first sub-region 1221 , a second sub-region 1222 , and a third sub-region 1223 ; the second sub-region 1222 is disposed around the first sub-region 1221 ; and the third sub-region 1223 is disposed around the second sub-region 1222 .

[0082] Specifically, the first sub-region 1221 , the second sub-region 1222 , and the third sub-region 1223 may be arranged in concentric circles.

[0083] The present application realizes partition polishing of the wafer 30 by setting the second area 122 as the first sub-area 1221, the second sub-area 1222 and the third sub-area 1223; and the second sub-area 1222 is set around the first sub-area 1221; the third sub-area 1223 is set around the second sub-area 1222, so as to better polish the wafer 30.

[0084] In some embodiments, the first sub-region 1221 has a fourth pressure P 4 , the second sub-region 1222 has a fifth pressure P 5 , the third sub-region 1223 has a sixth pressure P 6 , satisfies at least one of the following conditions: (a) P 4 <P 5 <P 6 ; (b) P 4 <P 5 ≤P 6 ; (c) P 4 ≤P 5 <P 6 ; (d) P 4 ≤P 5 ≤P 6 ; (e)P 4 <P 5 And P 5 =P 6 ; (f) P 4 =P 5 And P 5 <P 6 .

[0085] In this application, the fourth pressure P of the first sub-region 1221 is controlled 4 , the fifth pressure P of the second sub-region 1222 5 , the sixth pressure P of the third sub-region 1223 6 , satisfies at least one of the following conditions: (a) P4 <P 5 <P 6 ; (b) P 4 <P 5 ≤P 6 ; (c) P 4 ≤P 5 <P 6 ; (d) P 4 ≤P 5 ≤P 6 ; (e)P 4 <P 5 And P 5 =P 6 ; (f) P 4 =P 5 And P 5 <P 6 , partition polishing of the wafer 30 can be achieved, so that the wafer 30 can be polished better.

[0086] In some embodiments, the polishing device further comprises a polishing table 20; the polishing head 11 has a first rotation speed V 1 , the polishing table 20 has a second rotation speed V 2 , meet: meet: 1 rpm ≤ |V 1 -V 2 |≤10 rev / min.

[0087] It can be understood that the polishing table 20 and the polishing head 11 have the same rotation direction.

[0088] During the polishing process, the wafer 30 is placed on the polishing table 20 by being sucked by the air film 12, and the pressure applied to the placed wafer 30 is controlled by the air film 12, and the polishing head 11 is controlled to have a first rotation speed V 1 , the polishing table 20 has a second rotation speed V 2 , control 1 rpm≤|V 1 -V 2 |≤10 rpm, there is a speed difference between the polishing head 11 and the polishing table 20, and a stable flow of polishing liquid is applied to perform mechanical chemical polishing.

[0089] In some embodiments, the first pressure P 1 , satisfying: 3Psi≤P 1 ≤7Psi; Second pressure P 2 , satisfying: 1Psi≤P 2 ≤4.5Psi; third pressure P 3 , satisfying: 4Psi≤P 3 ≤9Psi.

[0090] Specifically, the first pressure P 1It can be a range consisting of one or two of 3Psi, 3.5Psi, 4Psi, 4.5Psi, 5Psi, 5.5Psi, 6Psi, 6.5Psi, and 7Psi. It is worth noting that the first pressure P 1 The value is given for example only. 1 Within the range of ≤7Psi, it belongs to the scope of protection of this application.

[0091] Specifically, the second pressure P 2 It can be a range consisting of one or two of 1Psi, 1.50Psi, 2Psi, 2.5Psi, 3Psi, 3.5Psi, 4Psi, and 4.5Psi. It is worth noting that the second pressure P 2 The value is given for example only. 2 In the range of ≤4.5Psi, it belongs to the scope of protection of this application.

[0092] Specifically, the third pressure P 3 It can be a range consisting of one or two of 4Psi, 5Psi, 6Psi, 7Psi, 8Psi, and 9Psi. It is worth noting that the third pressure P 3 The value is given for example only. 3 In the range of ≤9Psi, it belongs to the protection scope of this application.

[0093] In this application, the first pressure P of the first area 121 is controlled 1 , the second pressure P of the second region 122 2 , the third pressure P of the third region 123 3 , satisfy: P 2 <P 1 ≤P 3 , the wafer 30 can be fixed and polished, and the uniformity of edge removal of the top silicon layer 303 can be improved, thereby obtaining a top silicon layer 303 with uniform film thickness.

[0094] In some embodiments, along the transverse direction X, the first region 121 has a first width L 1 , meet: 9mm≤L 1 ≤15mm; the second region 122 has a second width L 2 , meet: 85mm≤L 2 ≤91mm; the third region 123 has a third width L 3 , meet: 17mm≤L 3 ≤23mm.

[0095] Specifically, the first width L 1It can be a range of one or two of 9mm, 10mm, 11mm, 12mm, 13mm, 14mm, and 15mm. It is worth noting that the first width L 1 The value is given only as an example. 1 Anything within the range of ≤15mm falls within the scope of protection of this application.

[0096] Specifically, the second width L 2 It can be a range of one or two of 85mm, 86mm, 87mm, 88mm, 89mm, 90mm, and 91mm. It is worth noting that the second width L 2 The value is given only as an example. 2 Anything within the range of ≤91mm falls within the scope of protection of this application.

[0097] Specifically, the third width L 3 It can be a range consisting of one or two of 17mm, 18mm, 19mm, 20mm, 21mm, 22mm, and 23mm. It is worth noting that the third width L 3 The value is given for example only. 2 Anything within the range of ≤23mm falls within the scope of protection of this application.

[0098] In some embodiments, along the lateral direction X, the first sub-region 1221 has a fourth width L 4 , meet: 47mm≤L 4 ≤53mm; the second sub-region 1222 has a fifth width L 5 , meet: 22mm≤L 5 ≤28mm; the third sub-region 1223 has a sixth width L 6 , meet: 20mm≤L 6 ≤26mm.

[0099] Specifically, the fourth width L 4 It can be a range consisting of one or two of 47mm, 48mm, 49mm, 50mm, 51mm, 52mm, and 53mm. It is worth noting that the fourth width L 4 The value is given for example only. 4 Anything within the range of ≤53mm falls within the scope of protection of this application.

[0100] Specifically, the fifth width L 5 It can be a range consisting of one or two of 22mm, 23mm, 24mm, 25mm, 26mm, 27mm, and 28mm. It is worth noting that the fifth width L5 The value is given only as an example. 2 Anything within the range of ≤28mm falls within the scope of protection of this application.

[0101] Specifically, the sixth width L 6 It can be a range consisting of one or two of 20mm, 21mm, 22mm, 23mm, 24mm, 25mm, and 26mm. It is worth noting that the sixth width L 6 The value is given only as an example. 6 Within the range of ≤26, it belongs to the scope of protection of this application.

[0102] In some embodiments, the fourth pressure P 4 , meet: 2.60Psi≤P 4 ≤2.68Psi; Fifth pressure P 5 , satisfying: 2.69Psi≤P 5 ≤2.70Psi; Sixth pressure P 6 , satisfying: 2.71Psi≤P 6 ≤2.85Psi.

[0103] Specifically, the fourth pressure P 4 It can be a range consisting of one or two of 2.60Psi, 2.61Psi, 2.62Psi, 2.63Psi, 2.64Psi, 2.65Psi, 2.66Psi, 2.67Psi, and 2.68Psi. It is worth noting that the fourth pressure P 4 The value is given for example only. 4 In the range of ≤2.68Psi, it belongs to the protection scope of this application.

[0104] Specifically, the fifth pressure P 5 It can be in the range of 2.69Psi, 2.70Psi or both. It is worth noting that the fifth pressure P 5 The value is given for example only. 4 The range of ≤2.70Psi belongs to the protection scope of this application.

[0105] Specifically, the sixth pressure P 6It can be a range consisting of one or two of 2.71Psi, 2.72Psi, 2.73Psi, 2.74Psi, 2.75Psi, 2.76Psi, 2.77Psi, 2.78Psi, 2.79Psi, 2.8Psi, 2.81Psi, 2.82Psi, 2.83Psi, 2.84Psi, and 2.85Psi. It is worth noting that the sixth pressure P 6 The value is given for example only. 6 In the range of ≤2.85Psi, it belongs to the protection scope of this application.

[0106] like Figure 10-12 As shown, accordingly, the present application also provides a polishing method, using the polishing device as described above, comprising:

[0107] Step S101 : providing a polishing head 11 , and providing an air film 12 on a side of the polishing head 11 facing the substrate 301 .

[0108] Step S102: The pressure is transmitted to the substrate 301 through the gas film 12. The force application range of the gas film 12 includes the first area 121 and the second area 122. The first area 121 is arranged around the second area 122. The first area 121 has a first pressure P 1 The second region 122 has a second pressure P 2 , satisfy: P 1 >P 2 .

[0109] In this application, the first pressure P of the first area 121 is controlled 1 Slightly greater than the second pressure P of the second region 122 2 , it can be achieved that the pressure applied to the first polishing area 31 is slightly greater than the pressure applied to other areas of the top silicon layer 303, that is, the pressure applied to the area where the step 33 is located is slightly greater than the pressure applied to other areas of the top silicon layer 303, which can improve the uniformity of edge removal of the top silicon layer 303, thereby obtaining a top silicon layer 303 with uniform film thickness.

[0110] In some embodiments, step S103 is used to polish a wafer 30 including a substrate 301 , wherein the wafer 30 includes an oxide layer 302 and a top silicon layer 303 , wherein the oxide layer 302 is located on a side of the substrate 301 , and the top silicon layer 303 is located on a side of the oxide layer 302 away from the substrate 301 .

[0111] Step S104 : adsorbing a side of the substrate 301 away from the oxide layer 302 onto the gas film 12 to polish the top silicon layer 303 .

[0112] During the polishing process, the side of the substrate 301 away from the oxide layer 302 is adsorbed on the gas film 12, and pressure is transmitted to the substrate 301 through the gas film 12 to adsorb and fix the wafer 30 to be polished to polish the top silicon layer 303.

[0113] In some embodiments, the first polishing area 31 is disposed corresponding to the first region 121 ; and the second polishing area 32 is disposed corresponding to the second region 122 .

[0114] In the present application, the first polishing area 31 is set correspondingly to the first region 121, and the second polishing area 32 is set correspondingly to the second region 122. Since the first region 121 has a first pressure P 1 , the second region 122 has a second pressure P 2 , satisfy: P 1 >P 2 , the force applied to the first polishing area 31 can be slightly greater than the force applied to the second polishing area 32 of the top silicon layer 303, thereby improving the uniformity of edge removal of the top silicon layer 303, thereby obtaining a top silicon layer 303 with uniform film thickness.

[0115] In some embodiments, the step of polishing the top silicon layer 303 includes:

[0116] Step S1041 : making the top silicon layer 303 contact with the polishing platform 20 .

[0117] Step S1042 : removing at least a portion of the top silicon layer 303 located in the first polishing area 31 .

[0118] Step S1043 : removing at least a portion of the top silicon layer 303 located in the second polishing area 32 .

[0119] It is understandable that by bringing the top silicon layer 303 into contact with the polishing platform 20 and polishing the top silicon layer 303 , at least a portion of the top silicon layer 303 in the first polishing area 31 and at least a portion of the top silicon layer 303 in the second polishing area 32 can be removed.

[0120] In some embodiments, the blasting head 11 has a first rotation speed V 1 ; The polishing table 20 has a second speed V 2 , meet: 1 rpm ≤|V 1 -V 2 |≤10 rpm. It is understandable that the polishing table 20 and the polishing head 10 have the same rotation direction.

[0121] During the polishing process, the wafer 30 to be polished is placed on the polishing table 20 through the air film 12, and the top silicon layer 303 is in contact with the polishing table 20, and the polishing head 11 is controlled to have a first rotation speed V 1 , the polishing table 20 has a second rotation speed V 2, control 1 rpm≤|V 1 -V 2 |≤10 rpm, there is a speed difference between the polishing head 11 and the polishing table 20, and a stable flow of polishing liquid is applied to perform mechanical chemical polishing on the top silicon layer 303.

[0122] like Fig.12 As shown, in some embodiments, the top silicon layer 303 located in the first polishing area 31 has a first removal amount D 1 , the top silicon layer 303 located in the second polishing area 32 has a second removal amount D 2 , satisfy: satisfy: 0≤|D 1 -D 2 |≤0.5μm.

[0123] It can be understood that the top silicon layer 303 located in the first polishing area 31 has a first removal amount D 1 , the top silicon layer 303 located in the second polishing area 32 has a second removal amount D 2 , satisfying: 0≤|D 1 -D 2 |≤0.5μm, achieving uniform removal of the edge of the top silicon layer 303, thereby obtaining a top silicon layer 303 with uniform film thickness.

[0124] In some embodiments, the first removal amount D 1 , satisfying: 3.5μm≤D 1 ≤5μm; Second removal amount D 2 , satisfying: 3.5μm≤D 2 ≤5μm.

[0125] Specifically, the first removal amount D 1 The range may include one or two of 3.5 μm, 3.8 μm, 4 μm, 4.2 μm, 4.5 μm, and 5 μm. It is worth noting that the first removal amount D 1 The values ​​are given for example only. 1 The range of ≤5μm belongs to the protection scope of this application.

[0126] Specifically, the second removal amount D 2 The range may include one or two of 3.5 μm, 3.8 μm, 4 μm, 4.2 μm, 4.5 μm, and 5 μm. It is worth noting that the second removal amount D 2 The values ​​are given for example only. 2 The range of ≤5μm belongs to the protection scope of this application.

[0127] In some embodiments, along the transverse direction X of the polishing head 11 , the first polishing area 31 has a second length M that satisfies: 4 mm≤M≤20 mm.

[0128] It can be understood that the second length M of the first polishing area 31 should be greater than or equal to the width W.

[0129] Specifically, the second length M may include a range consisting of one or two of 4mm, 8mm, 12mm, 15mm, 17mm, and 20mm. It is worth noting that the value of the second length M is only given as an example, and as long as it is within the range of 4mm≤W≤20mm, it falls within the scope of protection of this application.

[0130] The polishing device provided in the present application was used to polish five wafer 30 samples with widths W of 0.5 mm, 1.5 mm, 2.5 mm, 3 mm, and 4 mm, respectively. The forces applied to the first polishing area 31 and the second polishing area 32 during polishing were measured, and the amount of removal of the top silicon layer 303 located in the first polishing area 31 and the second polishing area 32 after polishing was measured. The results are shown in Table 1.

[0131] Table 1

[0132]

[0133] Correspondingly, the present application also provides a wafer 30, including the wafer 30 polished by the polishing device as described above; or, including the wafer 30 polished by the polishing method as described above.

[0134] The present application provides a wafer 30 which is obtained by polishing using the polishing device as described above, or by polishing using the polishing method as described above, wherein the edge of the top silicon layer 303 is removed uniformly, thereby improving the performance of the wafer 30 .

[0135] The above is a detailed introduction to a polishing device provided by the present application. Specific examples are used in this article to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the method of the present application and its core idea; at the same time, for technical personnel in this field, based on the idea of ​​the present application, there will be changes in the specific implementation method and application scope. In summary, the content of this specification should not be understood as a limitation on the present application.

Claims

1. A polishing device, characterized in that: Comprising: A polishing head (11), on one side of the polishing head (11) facing the substrate (301), there is an air film (12) for transmitting pressure to the substrate (301) through the air film (12); The force application range of the air film (12) includes a first region (121) and a second region (122), and the first region (121) is arranged around the second region (122); Wherein, the first region (121) has a first pressure P1; the second region (122) has a second pressure P2, satisfying: P1 > P2.

2. The polishing device according to claim 1, characterized in that: The first region (121) is provided with a slope (13), the slope (13) has a first inclined surface (131), and there is a first included angle α between the extending direction of the first inclined surface (131) and the transverse direction (X) of the polishing head (11), satisfying: 5° ≤ α ≤ 70°.

3. The polishing device according to claim 2, characterized in that: The slope (13) has a bottom surface (132) extending along the transverse direction (X), and the bottom surface (132) has a first length L, satisfying: 2 mm ≤ L ≤ 15 mm.

4. The polishing device according to claim 1, characterized in that: One side of the first region (121) facing the substrate (301) has a second inclined surface (14); the extending direction of the second inclined surface (14) and the extending direction of the transverse direction (X) of the polishing head (11) have a second included angle β, satisfying: 5° ≤ β ≤ 70°.

5. The polishing device according to claim 1, characterized in that: The force application range of the air film (12) further includes a third region (123), and the third region (123) is arranged around the first region (121); the third region (123) has a third pressure P3, satisfying: P2 < P1 ≤ P3.

6. The polishing device according to claim 1, characterized in that: The second region (122) includes a first sub-region (1221), a second sub-region (1222) and a third sub-region (1223); the second sub-region (1222) is arranged around the first sub-region (1221); the third sub-region (1223) is arranged around the second sub-region (1222).

7. The polishing device according to claim 6, characterized in that: The first sub-region (1221) has a fourth pressure P4, the second sub-region (1222) has a fifth pressure P5, and the third sub-region (1223) has a sixth pressure P6, satisfying at least one of the following conditions: (a) P4 < P5 < P6; (b) P4 < P5 ≤ P6; (c) P4 ≤ P5 < P6; (d) P4 ≤ P5 ≤ P6; (e) P4 < P5 and P5 = P6; (f) P4 = P5 and P5 < P6.

8. The polishing device according to claim 1, characterized in that: The polishing device further includes a polishing table (20); the polishing head (11) has a first rotation speed V1, and the polishing table (20) has a second rotation speed V2, satisfying: 1 revolution per minute ≤ |V1 - V2| ≤ 10 revolutions per minute.

9. A polishing method, characterized in that: Comprising: Providing a polishing head (11), on one side of the polishing head (11) facing the substrate (301), there is an air film (12); Transmitting pressure to the substrate (301) through the air film (12), the force application range of the air film (12) includes a first region (121) and a second region (122), and the first region (121) is arranged around the second region (122); The first region (121) has a first pressure P1; the second region (122) has a second pressure P2, satisfying: P1>P2.

10. The polishing method according to claim 9, characterized in that: Used for polishing a wafer (30) comprising the substrate (301), the wafer (30) comprising an oxide layer (302) and a top silicon layer (303), the oxide layer (302) being located on a side of the substrate (301), and the top silicon layer (303) being located on a side of the oxide layer (302) away from the substrate (301); A side of the substrate (301) away from the oxide layer (302) is adsorbed onto the gas film (12) to polish the top silicon layer (303).

11. The polishing method according to claim 10, characterized in that: The wafer (30) comprises a first polishing area (31) and a second polishing area (32); the first polishing area (31) is arranged around the second polishing area (32); the first polishing area (31) is arranged corresponding to the first area (121); and the second polishing area (32) is arranged corresponding to the second area (122).

12. The polishing method according to claim 11, characterized in that: The wafer (30) has a step (33), and the step (33) is located in the first polishing area (31); the step (33) has a width W, which satisfies: 0.5 mm ≤ W ≤ 4 mm.

13. The polishing method according to claim 11, characterized in that: The step of polishing the top silicon layer (303) comprises: bringing the top silicon layer (303) into contact with a polishing table (20); removing at least a portion of the top silicon layer (303) located in the first polishing area (31); At least a portion of the top silicon layer (303) located in the second polishing area (32) is removed.

14. The polishing method according to claim 13, characterized in that: The polishing head (11) has a first rotation speed V1; the polishing table (20) has a second rotation speed V2, which satisfies: 1 rpm≤|V1-V2|≤10 rpm.

15. The polishing method according to claim 13, characterized in that: The top silicon layer (303) located in the first polishing area (31) has a first removal amount D1, and the top silicon layer (303) located in the second polishing area (32) has a second removal amount D2, satisfying: 0≤|D1-D2|≤0.5μm.

16. The polishing method according to claim 15, characterized in that: The first removal amount D1 and the second removal amount D2 satisfy: 3.5 μm≤D1≤5 μm and 3.5 μm≤D2≤5 μm.

17. The polishing method according to claim 11, characterized in that: Along the transverse direction (X) of the polishing head (11), the first polishing area (31) has a second length M, which satisfies: 4mm≤M≤20mm.

18. A wafer, characterized in that: It includes a wafer polished by the polishing device as described in any one of claims 1-8; or, it includes a wafer polished by the polishing method as described in any one of claims 9-17.

Citation Information

Patent Citations

  • Adjustment of polishing rates during substrate polishing with predictive filters

    CN105765707A

  • Control method and system for adjusting polishing pressure according to life cycle of consumables

    CN108908063A

  • Polishing pressure control method, device and equipment for wafer polishing

    CN110193776A

  • Wafer polishing head, system thereof, and method using the same

    CN113134786A

  • Method for improving CMP thickness uniformity of thin film

    CN113436960A