Preparation method of transition metal atom doped two-dimensional bismuth oxide nanosheet
The preparation of high-quality transition metal atom doped two-dimensional bismuth oxide nanosheets through the dual-temperature CVD method solves the problems of poor crystallinity and expensive preparation in the prior art, and realizes the high-quality preparation and controllability of nanosheets. Promotes its application in the field of two-dimensional transistor devices.
Patent Information
- Application Number
- CN202310642364.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-01
- Publication Date
- 2024-12-03
AI Technical Summary
The prior art is difficult to prepare high-quality transition metal atom doped two-dimensional Bi2O3 nanosheets, which limits their application in the field of two-dimensional transistor devices, especially due to poor crystallinity and expensive preparation methods and are not suitable for large-scale production.
Using the dual-temperature CVD method, Bi2O3 powder and NaCl particles are uniformly mixed, placed in a quartz boat, argon and Ar/O2 mixed gas are introduced, and the gas pressure and temperature are adjusted to achieve transition metal atom doping of two-dimensional bismuth oxide nanosheets. Preparation.
A high-quality two-dimensional rectangular nanosheet was successfully prepared, with a maximum size of up to 60μm, a controllable thickness, good crystallinity, large nucleation density and good stability. It is suitable for the application of two-dimensional transistor devices and promotes transition metal atom doping. Miscellaneous Bi2O3 is widely used in the fields of electronics and optoelectronics.
Smart Images

Figure CN119059555A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of nanomaterials and relates to a method for preparing a transition metal atom-doped two-dimensional bismuth oxide nanosheet. Background Art
[0002] Two-dimensional materials represented by graphene, such as boron nitride (h-NB), transition metal chalcogenides (TMDCs), black phosphorus (BP), indium selenide (InSe), bismuth selenide (Bi 2 O 2 Two-dimensional materials such as Se) have a rich series of physical and chemical properties, including atomic-level thickness, adjustable band gap, no dangling bonds on the surface, ultra-high carrier mobility and excellent electrostatic tunability. They are considered to be one of the most promising channel materials for the silicon-based sub-10 nanometer semiconductor process in the post-Moore era. Two-dimensional metal oxide semiconductor materials have been found to have both high electron-hole carrier mobility and ultra-high air stability, becoming one of the hot research directions in the field of two-dimensional semiconductor materials recently. Among them, Bi 2 O 3 Metal oxide semiconductor materials represented by have excellent physical and chemical properties, electrical properties, high air stability and simple preparation. They are mainly used in optoelectronics, catalysis and energy fields. 2 O 3 The application of two-dimensional transistor electronics is still scarce, so the development of high-performance transition metal atom-doped two-dimensional Bi 2 O 3 Semiconductor materials are of great significance for future applications in electronic devices.
[0003] The researchers mainly used solution precipitation, microwave-assisted, thermal evaporation deposition, atomic layer deposition (ALD), liquid metal stripping and CVD to prepare Bi 2 O 3 The morphology of zero-dimensional nanoparticles, one-dimensional nanowires, one-dimensional nanorods, one-dimensional nanohooks, three-dimensional nanoflowers, etc., and its application in many fields such as photocatalysis and solar cells has been studied. 2 O 3 The material cannot obtain high crystalline quality Bi on a two-dimensional scale 2 O 3 Crystals cannot be expanded to the research and application of two-dimensional transistor devices, limiting their application in the field of electronics. Reference 1 uses atomic layer deposition (ALD) technology to prepare Bi 2 O 3 The Bi film prepared by this method 2 O 3The film has poor crystallinity and the equipment is expensive, which is not suitable for large-scale preparation of bismuth oxide nanosheets (YDShen, YWLi, WMLi, JZZhang, ZGHu, and JHChu, Growth of Bi 2 O 3 Ultrathin Films by AtomicLayer Deposition,J.Phys.Chem.C,2012,116,3449-3456). Reference 2 synthesized V-doped Bi by hydrothermal method. 2 O 3 Three-dimensional nanoflower structure. The bismuth oxide prepared by this method is used for the reduction of carbon dioxide and is not suitable for the application of electronic devices (ZHANG G, ZHENG X, CUI X, et al. Doping of Vanadium into Bismuth OxideNanoparticles for Electrocatalytic CO 2 Reduction[J].ACS Applied NanoMaterials, 2022, 5(10):15465-72). Reference 3 prepared Sm-doped Bi by coprecipitation method. 2 O 3 Nanoparticles, the samples prepared by this method have needle-like morphology, poor crystallinity, and are only used as warm light sources, lacking application in the field of electronics (DIVYAJ, SHIVARAMU NJ, ROOS WD, et al. Synthesis, surface and photoluminescence properties of Sm 3+ dopedα-Bi 2 O 3 [J].Journal of Alloys and Compounds,2021,854:157221).
[0004] So far, transition metal atom-doped Bi has been prepared by CVD method. 2 O 3 There are no reports of two-dimensional semiconductor materials. Summary of the invention
[0005] The purpose of the present invention is to provide a method for preparing transition metal atom-doped two-dimensional bismuth oxide nanosheets.
[0006] The technical solution for achieving the purpose of the present invention is as follows:
[0007] The preparation method of transition metal atom-doped two-dimensional bismuth oxide nanosheets comprises the following steps:
[0008] Place a two-dimensional monolayer transition metal sulfide or transition metal selenide on a high temperature resistant quartz plate and place it in the second temperature zone. 2 O 3 The powder and NaCl particles were placed in a quartz boat and mixed evenly, and then placed in the first temperature zone as the precursor powder. Argon gas was introduced to remove the residual air in the tube. The first temperature zone was heated to 840-870°C and kept warm for 10-60 min. The second temperature zone was heated to 400-550°C and kept warm for 10-60 min. Ar and O were introduced at the same time. 2 Mixed gas, Ar:O 2 The flow rate ratio is 140-200 sccm:1-60 sccm, and O 2 The amount of input is not 0, and the gas pressure in the tube furnace chamber is adjusted to 100-200 Pa. The precursor powder volatilized and diffused in the first temperature zone is transferred to the second temperature zone in the gas phase, causing a chemical reaction and re-nucleation and growth to obtain transition metal atom-doped two-dimensional bismuth oxide nanosheets.
[0009] The transition metal atoms described in the present invention are tungsten (W), molybdenum (Mo), vanadium (V), chromium (Cr), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), niobium (Nb), palladium (Pd), cadmium (Cd) and other transition metal atoms. In the specific implementation of the present invention, W and Mo are representative examples.
[0010] Preferably, the transition metal sulfide is WS 2 or MoS 2 , transition metal selenide is WSe 2 or MoSe 2 .
[0011] Preferably, Bi 2 O 3 The mass ratio of powder to NaCl particles is 100-200 mg:0.5-3 mg.
[0012] Preferably, the first temperature zone is heated to 850° C. and kept warm for 20 min; the second temperature zone is heated to 450° C. and kept warm for 20 min.
[0013] Preferably, the heating rate is 20°C / min.
[0014] Preferably, Ar:O 2 The flow rate ratio is 120sccm:30sccm.
[0015] Preferably, the gas pressure in the tube furnace chamber is adjusted to 150Pa.
[0016] Compared with the prior art, the present invention has the following advantages:
[0017] The preparation method of the present invention is simple, and for the first time, high-quality two-dimensional rectangular nanosheets are prepared, with a maximum size of 60 μm and a minimum thickness of 1 nm. The transition metal atom-doped bismuth oxide nanosheets prepared by the present invention have the advantages of high nucleation density, good stability, controllable thickness and size, and good crystallinity. It not only enriches the family of two-dimensional semiconductor nanomaterials, but also provides material support for its application research in two-dimensional transistor devices, and is expected to promote the transition metal atom-doped Bi 2 O 3 Semiconductor materials are widely used in electronics, optoelectronics and other fields. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 Schematic diagram of the preparation method of transition metal atom-doped two-dimensional bismuth oxide nanosheets;
[0019] Figure 2 For a two-dimensional monolayer WS grown on a sapphire substrate 2 OM diagram;
[0020] Figure 3 HREM image of a single rectangular two-dimensional W-doped bismuth oxide nanosheet prepared in Example 1;
[0021] Figure 4 TEM diffraction pattern of the two-dimensional W-doped bismuth oxide nanosheet prepared in Example 1;
[0022] Figure 5 OM image of the appearance and size of a single crystal of a two-dimensional W-doped bismuth oxide nanosheet prepared in Example 1;
[0023] Figure 6 This is an atomic force microscope image (AFM) of the two-dimensional W-doped bismuth oxide nanosheet prepared in Example 1;
[0024] Figure 7 Raman spectra of two-dimensional W-doped bismuth oxide nanosheets of different thicknesses prepared in Example 1;
[0025] Figure 8 This is an XPS graph of the two-dimensional W-doped bismuth oxide nanosheets prepared in Example 1;
[0026] Fig. 9 This is the EDS element distribution diagram of the two-dimensional W-doped bismuth oxide nanosheet prepared in Example 1;
[0027] Fig.10 UV-Vis-NIR of the two-dimensional W-doped bismuth oxide nanosheets prepared in Example 1;
[0028] Fig.11 The two-dimensional W-doped bismuth oxide nanosheets prepared in Example 2 and the two-dimensional monolayer WS used 2 OM diagram;
[0029] Fig.12 OM image of the two-dimensional W-doped bismuth oxide nanosheet prepared in Example 3;
[0030] Fig.13 OM image of the two-dimensional W-doped bismuth oxide nanosheet prepared in Example 4;
[0031] Fig.14 This is the nucleation density map of the two-dimensional W-doped bismuth oxide nanosheet OM prepared in Example 5;
[0032] Fig.15 OM nucleation density diagram of the two-dimensional W-doped bismuth oxide nanosheet prepared in Comparative Example 1;
[0033] Fig.16 For two-dimensional MoS grown on sapphire substrate 2 OM image of the film;
[0034] Fig.17 This is the nucleation density map of the two-dimensional Mo-doped bismuth oxide nanosheet OM prepared in Example 6;
[0035] Fig.18 This is a Raman spectrum (Raman) of the two-dimensional Mo-doped bismuth oxide nanosheets prepared in Example 6;
[0036] Fig.19 For WS 2 and MoS 2 Raman spectrum of . DETAILED DESCRIPTION
[0037] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. After reading the present invention, various equivalent forms of modifications to the present invention by those skilled in the art all fall within the scope defined by the claims attached to this application.
[0038] In the following embodiments: a two-dimensional single-layer WS 2 The preparation method is based on the existing method, which can be found in the literature (YANG W, MU Y, CHEN X, et al. CVD growth of large-area monolayer WS 2film on sapphire throughtuning substrate environment and its application for high-sensitive strain sensor[J].Discover Nano,2023,18(1):13.), specifically: select a dual-temperature zone CVD tube furnace, weigh 1.0g of S powder and put it into a quartz boat to the heating center of the upstream first temperature zone, and then weigh the purity of 99.99% WO 3 100 mg of powder and 1 mg of NaCl solid particles were evenly mixed and placed in a quartz boat to the heating center of the second temperature zone downstream. A 1 cm × 1 cm cut sapphire substrate was placed at the heating center of the second temperature zone downstream. The temperature of the heating center of the first temperature zone upstream was set to 110-130 ° C, and the temperature of the heating center of the second temperature zone downstream was set to 940-960 ° C. It was ensured that the S source and the W source were evaporated at the same time. 140-160 sccm of pure argon was introduced as a transport carrier gas to obtain a two-dimensional single-layer WS 2 .
[0039] 2D MoS 2 The film was prepared by the existing method, which can be referred to in the literature (SINGH A, MOUN M, SHARMA M, et al. NaCl-assisted substrate dependent 2D planar nucleated growth of MoS 2 [J]. Applied Surface Science, 2021, 538: 148201.), specifically: select a dual-temperature zone CVD tube furnace, weigh 1.0g of S powder and put it into a quartz boat to the heating center of the upstream first temperature zone, and then weigh the purity of 99.99% MoO 3 30 mg of powder was placed in a quartz boat at the heating center of the second temperature zone downstream. A 1 cm × 1 cm cut sapphire substrate was placed at the heating center of the second temperature zone downstream. The temperature of the heating center of the first temperature zone upstream was set to 110-130 ° C, and the temperature of the heating center of the second temperature zone downstream was set to 700-750 ° C. The S source and the Mo source were evaporated at the same time. 140-160 sccm of pure argon was introduced as a carrier gas to obtain MoS 2 film.
[0040] Example 1
[0041] (1) Select a two-dimensional single-layer WS with a size of 100 to 120 μm 2 The sample is loaded on a high temperature resistant quartz plate and placed in the heating center of the second temperature zone of the CVD tube furnace;
[0042] (2) Take Bi with a purity of 99.99% 2 O 3 Powder and NaCl granules with a purity of 99.99%, weighing Bi with an electronic balance 2 O 3 150 mg of powder and 3 mg of NaCl particles were evenly mixed in a quartz boat and then placed in the heating center of the second temperature zone of a CVD tube furnace;
[0043] (3) Clean the CVD tube furnace with pure Ar carrier gas, turn on the mechanical pump to evacuate the tube furnace, and then introduce Ar gas for flushing. Repeat the cleaning three times to achieve the purpose of cleaning the residual air;
[0044] (4) Set the CVD heating curve. The first temperature zone is set at room temperature of 25°C and heated to 850°C in 43 minutes, and kept at this temperature for 30 minutes; the second temperature zone is set at room temperature of 25°C and heated to 450°C in 43 minutes, and kept at this temperature for 30 minutes;
[0045] (5) Set the carrier gas flow rate and pressure. Introduce a mixed carrier gas with a ratio of Ar:O 2 =120:30 (sccm) The pressure value in the furnace is adjusted to 120Pa through the pressure detection equipment and the gas valve knob. After the pressure value and its flow rate are stable, the equipment is started to carry out experimental growth preparation;
[0046] (6) After the experimental heating reaction is completed, the mechanical pump and the air inlet valve are turned off. After naturally cooling to room temperature, the sample is taken out for characterization and testing to obtain a two-dimensional W-doped bismuth oxide nanosheet.
[0047] The single layer WS used in the two-dimensional W-doped bismuth oxide nanosheet prepared in Example 1 2 The OM diagram is as follows: Figure 2 HRTEM image of a single two-dimensional rectangular W-doped bismuth oxide prepared in Example 1, as shown Figure 3 The TEM diffraction pattern of the two-dimensional rectangular W-doped bismuth oxide nanosheet prepared in Example 1 is as shown in FIG. Figure 4 The appearance and size of a single crystal of a two-dimensional rectangular W-doped bismuth oxide nanosheet prepared in Example 1 are shown in the OM image. Figure 5 The atomic force microscope (AFM) image of the two-dimensional rectangular W-doped bismuth oxide nanosheet prepared in Example 1 is shown in FIG. Figure 6 As shown in FIG. 1 , the crystal thickness reaches the atomic scale, which is about 8 nm. The Raman spectrum (Raman) analysis of the two-dimensional rectangular W-doped bismuth oxide nanosheets prepared in Example 1 shows that Figure 7 As shown, 257~307cm -1 It is an octahedral WO 6 The stretching vibration mode of the Bi-O bond and the bending vibration mode of the Bi-O bond are 796-825 cm -1A belonging to the antisymmetric and symmetric OWO g The XPS element valence bond analysis diagram of the two-dimensional rectangular W-doped bismuth oxide nanosheet prepared in Example 1 is as follows: Figure 8 As shown, they are the main peaks of Bi 4f orbital photoelectrons, W 4f orbital photoelectrons, and O 1s orbital photoelectrons, respectively, which illustrate that the valence state of Bi is +3, W is +6, and the formation of Bi-O and WO valence bonds, proving that the prepared sample is a two-dimensional Bi 7.89 W 0.11 O 12.16 The EDS element distribution diagram of the two-dimensional rectangular W-doped bismuth oxide nanosheets prepared in Example 1 is as follows: Fig. 9 As shown in FIG. 1 , it can be seen that the Bi, W, and O elements are evenly distributed on the nanosheets. The UV-Vis-NIR image of the two-dimensional rectangular W-doped bismuth oxide rectangular nanosheets prepared in Example 1 is shown in FIG. Fig.10 As shown, its semiconductor band gap value is 2.57eV.
[0048] Example 2
[0049] Similar to Example 1, except that the two-dimensional single-layer WS is selected in step (1) of Example 1. 2 The size is 160-200μm.
[0050] Example 2 Preparation of two-dimensional rectangular W-doped bismuth oxide nanosheets and two-dimensional single-layer WS 2 The OM diagram is as follows: Fig.11 As shown in the figure, it can be seen that the edge size of the largest two-dimensional rectangular W-doped bismuth oxide nanosheet is about 40 μm, and the average size is larger than that of Example 1, indicating that the two-dimensional single layer WS 2 The size of will affect the synthesis size of two-dimensional rectangular W-doped bismuth oxide nanosheets, playing a key role in providing auxiliary raw materials.
[0051] Example 3
[0052] Similar to Example 1, except that the insulation time of the second temperature zone in step (4) of Example 1 is adjusted to 10 minutes.
[0053] OM image of a single two-dimensional rectangular W-doped bismuth oxide nanosheet prepared in Example 3, as shown Fig.12 As shown in the figure, it can be seen that the diameter of the nanosheets is about 15 μm, the thickness is significantly thinner and the average size is smaller than that of Example 1.
[0054] Example 4
[0055] Similar to Example 1, except that the insulation time of the second temperature zone in step (2) of Example 1 is adjusted to 60 minutes.
[0056] OM image of the two-dimensional rectangular W-doped bismuth oxide nanosheet prepared in Example 4, as shown in Fig.13 As shown in the figure, it can be seen that the diameter of the two-dimensional nanosheet is about 50 μm, it appears as an irregular rectangle and the thickness increases significantly, and the size increases.
[0057] Example 5
[0058] Similar to Example 1, except that the carrier gas flow rate Ar in step (5) of Example 1 is regulated: 2 =100:50(sccm).
[0059] The OM nucleation density diagram of the two-dimensional rectangular W-doped bismuth oxide nanosheets prepared in Example 5 is as follows: Fig.14 As shown in the figure, it can be seen that the nucleation density of the obtained two-dimensional rectangular W-doped bismuth oxide nanosheets is reduced and the size is small. The comparison shows that adjusting the carrier gas flow ratio will affect the nucleation density of the two-dimensional material.
[0060] Comparative Example 1
[0061] Similar to Example 1, except that the pressure in step (5) of Example 1 is regulated to 300 Pa.
[0062] The OM nucleation growth diagram of the circular nanosheets prepared in Comparative Example 1 is as follows: Fig.15 As shown, it can be seen that when the pressure increases, the two-dimensional rectangular W-doped bismuth oxide nanosheets are small and less dense, and appear irregularly shaped.
[0063] Example 6
[0064] Bismuth oxide is doped with Mo as a transition metal atom, similar to Example 1, except that the single layer WS in step (1) of Example 1 is 2 Replace with MoS 2 The film was grown by adjusting the temperature of the second temperature zone in step (4) of Example 1 to 400° C. and maintaining the temperature for 30 minutes.
[0065] The nucleation density diagram of the two-dimensional rectangular Mo-doped bismuth oxide nanosheet OM prepared in Example 6 is as follows: Fig.17 As shown, the 2D rectangular Mo-doped bismuth oxide nanosheets have high density but small size. Fig.18 The Raman spectrum of the nanosheets obtained by doping bismuth oxide with Mo can be judged to have a chemical formula of Bi 2 MoO 6 , because the MoS used 2 The Mo concentration in the film is very high, which is beneficial to the alloying of bismuth oxide.
[0066] It can be seen from the above embodiments and comparative examples that the preparation method provided by the present invention is simple to operate. By adjusting the growth parameters, two-dimensional rectangular W-doped bismuth oxide nanosheets with different thicknesses, different sizes and good crystallinity can be obtained. 2 The size and pressure environment are the key factors affecting the preparation of two-dimensional rectangular W-doped bismuth oxide nanosheets. The two-dimensional rectangular W-doped bismuth oxide nanosheets prepared by this technology have high nucleation density, regular shape, high crystal quality, and good chemical stability. At the same time, the type of parent material is changed, and MoS 2 The film increases the concentration of Mo, which can cause alloying of bismuth oxide, which fully demonstrates that the method of the present invention is applicable to the situation of doping two-dimensional bismuth oxide with multiple types of transition metal atoms, not limited to W and Mo elements, but can be further expanded to include the doping of transition metal atoms such as vanadium (V), chromium (Cr), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), niobium (Nb), palladium (Pd), and cadmium (Cd).
[0067] The above is only a preferred embodiment of the present invention, and does not limit the present invention in any form. It should be pointed out that for those skilled in the art, it is obvious that the present invention is not limited to the details of the above exemplary embodiments, but also includes the scope of applicable situations that the innovative method of the present invention can expand, and the present invention can be implemented in other specific forms without departing from the spirit or basic features of the present invention. Therefore, no matter from which point of view, the embodiments should be regarded as exemplary and non-restrictive, and the scope of the present invention is defined by the attached claims rather than the above description, so it is intended to include all changes within the meaning and scope of the equivalent elements of the claims. Any figure mark in the claims should not be regarded as limiting the claims involved. At the same time, for those of ordinary skill in the art, without departing from the precursor of the principle of the present invention, several improvements and modifications can be made, and these improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing transition metal atom-doped two-dimensional bismuth oxide nanosheets, characterized in that: The following steps are involved: A two-dimensional monolayer transition metal sulfide or transition metal selenide is placed on a high-temperature resistant quartz plate and loaded in the second temperature zone. Bi2O3 powder and NaCl particles are placed in a quartz boat and evenly mixed and placed in the first temperature zone as precursor powder. Argon gas is introduced to remove residual air in the tube. The first temperature zone is heated to 840-870°C and kept warm for 10-60 min. The second temperature zone is heated to 400-550°C and kept warm for 10-60 min. At the same time, a mixed gas of Ar and O2 is introduced, and the flow rate ratio of Ar:O2 is 140-200sccm:1-60sccm, and the amount of O2 introduced is not 0. The gas pressure in the tube furnace chamber is adjusted to 100-200 Pa, and the precursor powder volatilized and diffused in the first temperature zone is gas-phase transferred to the second temperature zone, a chemical reaction occurs, and re-nucleation and growth are obtained to obtain transition metal atom-doped two-dimensional bismuth oxide nanosheets.
2. The preparation method according to claim 1, characterized in that: The transition metal atom is tungsten, molybdenum, vanadium, chromium, iron, cobalt, nickel, copper, niobium, palladium or cadmium.
3. The preparation method according to claim 1, characterized in that The transition metal sulfide is WS2 or MoS2, and the transition metal selenide is WSe2 or MoSe2.
4. The preparation method according to claim 1, characterized in that The mass ratio of Bi2O3 powder and NaCl particles is 100~200 mg:0.5~3 mg.
5. The preparation method according to claim 1, characterized in that The first temperature zone was heated to 850 °C and kept at this temperature for 20 min; the second temperature zone was heated to 450 °C and kept at this temperature for 20 min.
6. The preparation method according to claim 1, characterized in that The heating rate is 20 ℃ / min.
7. The preparation method according to claim 1, characterized in that The flow rate ratio of Ar:O2 is 120 sccm:30 sccm.
8. The preparation method according to claim 1, characterized in that Adjust the gas pressure in the tube furnace chamber to 150 Pa.
9. Transition metal atom-doped two-dimensional bismuth oxide nanosheets prepared according to the preparation method according to any one of claims 1 to 8.