Method for enhancing binding force of metal film on glass surface
By using Bessel laser to form a concentric ring microstructure on the glass surface, the problem of insufficient bonding force of the metal film on the glass surface is solved, significantly improving the binding force and avoiding the metal film falling off, achieving higher accuracy and speed.
Patent Information
- Application Number
- CN202410968009.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-12-03
AI Technical Summary
The prior art cannot effectively enhance the bonding force of the metal film on the glass surface, resulting in the problem that the metal layer is prone to layering, curling and falling off on the glass surface.
The physical characteristics of the Bessel laser multi-side lobes are used to form a microstructure of concentric rings on the glass surface, increasing the contact area between the glass and the metal film, and enhancing friction through the groove and burr structure to improve binding force.
The bonding force of the metal film on the glass surface is significantly improved, and the metal film is avoided from falling off. Compared with traditional CNC programming processing, the accuracy is higher and the speed is faster.
Smart Images

Figure CN119059743A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of chip packaging, and in particular to a method for enhancing the bonding force of a metal film on a glass surface. Background Art
[0002] As Moore's Law continues to reach its limit, advanced integrated packaging technology has gradually entered people's field of vision. Traditional integrated packaging technology is limited by the processing of organic substrates, and has problems such as low wiring density and low space utilization. With the development of packaging technology, silicon adapters with through-silicon via structures have been widely studied and applied. The integrated packaging structure using silicon adapters is called 2.5D packaging. During the packaging process, a layer of metal film is required on both sides of the silicon adapter to achieve better electrical and thermal performance. However, silicon substrates have problems such as complex processes, high costs, and severe signal loss. Therefore, glass adapters with through-glass vias have become a new research hotspot. Compared with silicon adapters, glass adapters have the advantages of low signal loss, large size, low cost, and simple process. However, due to the smooth surface of the glass and poor bonding with the metal film, there are problems of metal layer delamination, curling, and shedding.
[0003] At present, the methods commonly used for coating metal films on glass surfaces include magnetron sputtering coating and electrochemical coating, specifically:
[0004] 1. Magnetron sputtering coating: Magnetron sputtering technology is a kind of physical vapor deposition technology. Its principle is to use the target material as the target cathode, use argon ions to bombard the target material, produce cathode sputtering, and then sputter the target atoms onto the workpiece to form a deposition layer. As an important coating technology, magnetron sputtering coating technology has the advantages of fast deposition speed, high precision, good film quality, and a wide range of substrate applications. However, there are problems such as low target material utilization and poor film-substrate bonding.
[0005] 2. Electrochemical plating: Electrochemical plating is a method of forming a film layer by depositing metal ions in an electrolyte on a substrate through an electrochemical reaction. Specifically, this method involves placing the workpiece to be plated as a cathode in an electrolyte containing the metal ions to be plated. After power is turned on, the metal ions obtain electrons at the cathode and are reduced to metal atoms and deposited on the cathode workpiece to form a metal coating. Compared with magnetron sputtering coating technology, electrochemical plating technology has the advantages of mature process, high production efficiency, and a variety of materials, but it also has the problem of low film-base bonding on smooth substrate surfaces.
[0006] Although both electrochemical coating and magnetron sputtering coating can form metal films on the glass surface, they cannot overcome the problem of low bonding strength of the metal film on the glass surface. Therefore, there is an urgent need for a method that can effectively improve the bonding strength of the metal film on the glass surface. Summary of the invention
[0007] The purpose of the present invention is to propose a method for enhancing the bonding strength of a metal film on a glass surface, utilizing the physical properties of multiple side lobes of a Bessel laser to form a concentric ring microstructure on the glass surface, thereby enhancing the bonding strength of the metal film on the glass surface to overcome the shortcomings of the prior art.
[0008] To achieve this object, the present invention adopts the following technical solutions:
[0009] A method for enhancing the bonding strength of a metal film on a glass surface comprises the following steps:
[0010] A. Clean and dry the glass;
[0011] B. Determine the processing point and processing path of laser processing on the glass surface in step A;
[0012] C. According to the processing path, focusing the Bessel beam on the glass surface of step B, and laser processing the processing point to form a microstructure on the glass surface; wherein the Bessel beam is a pulsed laser;
[0013] D. placing the glass in step C in an etching solution for etching;
[0014] E. Clean and dry the glass in step D.
[0015] Preferably, the laser power of the Bessel beam is 1-40 W, and the pulse width of the Bessel beam is 290-6000 fs.
[0016] Preferably, the distance between two adjacent processing points is smaller than the spot diameter of the Bessel light beam.
[0017] Preferably, in step C, the number of pulses of the Bessel beam for laser processing any one of the processing points is 1 to 9.
[0018] Preferably, step D further comprises:
[0019] D. After repeating step C1 to 500 times, place the glass in an etching solution for etching.
[0020] Preferably, in step D, the etching solution comprises hydrofluoric acid and auxiliary acid, and in terms of mass percentage, the content of the hydrofluoric acid is 5-20%, and the content of the auxiliary acid is 1-20%.
[0021] Preferably, the auxiliary acid includes any one or more combinations of hydrochloric acid, nitric acid and sulfuric acid.
[0022] Preferably, the wavelength of the Bessel light beam is 1030 nm.
[0023] Preferably, the cleaning steps of step A and step E both include: cleaning the glass with acetone, anhydrous ethanol and deionized water in sequence.
[0024] Preferably, the glass includes any one of soda-lime glass, aluminosilicate glass, quartz glass, borosilicate glass and lead silicate glass.
[0025] The technical solution provided by the present invention may include the following beneficial effects:
[0026] 1. By utilizing the physical characteristics of the multiple side lobes of the Bessel laser, a concentric ring microstructure is formed on the glass surface. The above microstructure can increase the contact area between the glass and the metal film and increase the bonding force of the glass surface to the metal film.
[0027] 2. The microstructure of the concentric rings can exert a force directed toward the center of the rings on the film through the grooves when deformation occurs, increasing the friction between the groove sidewalls and the metal film, thereby preventing the film from falling off.
[0028] 3. Compared with traditional CNC programming processing, the use of Bessel beam can process concentric ring structures in a single time with higher precision and faster speed. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 It is a schematic diagram of the light intensity distribution of the Bessel light beam in the present invention.
[0030] Figure 2 It is a processing schematic diagram of a method for enhancing the bonding strength of a metal film on a glass surface according to the present invention.
[0031] Figure 3 It is a schematic diagram of the microstructure of the present invention.
[0032] Figure 4 It is a schematic diagram of the concentric ring interference of the present invention. DETAILED DESCRIPTION
[0033] A method for enhancing the bonding strength of a metal film on a glass surface comprises the following steps:
[0034] A. Clean and dry the glass;
[0035] B. Determine the processing point and processing path of laser processing on the glass surface in step A;
[0036] C. According to the processing path, focusing the Bessel beam on the glass surface of step B, and laser processing the processing point to form a microstructure on the glass surface; wherein the Bessel beam is a pulsed laser;
[0037] D. placing the glass in step C in an etching solution for etching;
[0038] E. Clean and dry the glass in step D.
[0039] In order to enhance the bonding strength of the glass surface to the metal film, this technical solution proposes an effective bonding strength enhancement method, using Bessel laser (light intensity distribution diagram as shown in Figure 1 The physical characteristics of multiple side lobes form a microstructure of concentric rings on the glass surface, such as Figure 2 As shown, the above microstructure can increase the contact area between the glass and the metal film, and enhance the bonding force of the glass surface to the metal film.
[0040] At the same time, when the Bessel beam acts on the glass surface, pits and burrs will be formed on the groove surface of the microstructure, forming a barb-like structure, such as Figure 3 When the metal film is completely filled into the groove, the metal film and the pits and burrs in the groove will form a riveting effect and a hook chain effect, so that when it is subjected to external force, the metal film and the hole wall of the groove are broken by shear force, making the bonding strength stronger.
[0041] Furthermore, due to the different thermal expansion and contraction properties of glass and metal film, and under the same temperature change, the deformation of the metal film is greater than that of the glass. Therefore, during use, the film-base bonding force may decrease due to changes in ambient temperature, and even the metal film may fall off. However, the microstructure formed by processing concentric rings can apply a force pointing to the center of the ring to the film through the groove when deformation occurs, increase the friction between the groove sidewall and the metal film, and thus avoid the film from falling off. Furthermore, compared with traditional CNC programming processing, the use of Bessel beams can process concentric ring structures in a single time, with higher precision and faster speed.
[0042] Therefore, the method for enhancing the bonding strength of the metal film on the glass surface proposed in this solution can significantly increase the bonding strength of the glass surface to the metal film and promote the application of the glass transfer plate.
[0043] It should be noted that in the drying steps of step A and step E, a vacuum drying oven or high-pressure gas blowing may be used for drying, which is not limited here.
[0044] To further illustrate, the laser power of the Bessel beam is 1-40 W, and the pulse width of the Bessel beam is 290-6000 fs.
[0045] It should be noted that the laser power and pulse width of the Bessel beam will directly affect the diameter and number of the concentric ring microstructures. Therefore, in order to further enhance the bonding strength of the glass surface to the metal film, this scheme also optimizes the above two parameters.
[0046] It is further explained that the distance between two adjacent processing points is smaller than the spot diameter of the Bessel light beam.
[0047] Furthermore, in order to further enhance the bonding strength of the glass surface to the metal film, the present solution also makes the distance between two adjacent processing points smaller than the spot diameter of the Bessel beam, so that interference occurs between the adjacent concentric rings formed. When interference occurs, some grooves of different rings will cross, thus forming Figure 4 The structure shown above can increase the contact area between the metal film and the glass surface, and further enhance the bonding strength.
[0048] To further illustrate, in step C, the number of pulses of the Bessel beam for laser processing any of the processing points is 1 to 9.
[0049] It should be noted that the pulse number refers to the number of times the pulsed Bessel laser continuously processes a certain processing point.
[0050] To further illustrate, step D also includes:
[0051] D. After repeating step C1 to 500 times, place the glass in an etching solution for etching.
[0052] It should be noted that the number of laser processing times will affect the groove width and depth of the concentric ring structure. If the number of laser processing times exceeds 500 times, laser ablation will produce a large amount of sediment, increasing the difficulty of subsequent etching, resulting in residual sediment and affecting the bonding strength between the metal film and the glass substrate.
[0053] Preferably, after repeating step C 500 times, a groove with a depth of 70 μm, a top width of 20 μm, and a bottom width of 8 μm can be obtained.
[0054] To further illustrate, in step D, the etching solution includes hydrofluoric acid and auxiliary acid, and in terms of mass percentage, the content of the hydrofluoric acid is 5-20%, and the content of the auxiliary acid is 1-20%.
[0055] The etching step can eliminate debris and impurities adhering to the surface of the glass concentric ring structure due to laser processing. In a preferred embodiment of the present technical solution, the etching solution is a mixed solution of hydrofluoric acid and auxiliary acid. Compared with the existing alkaline etching solution, the reaction rate of the mixed solution of hydrofluoric acid is faster, which can effectively improve the etching efficiency.
[0056] It should be noted that in the etching step, etching can be assisted by one or more of ultrasonic, stirring, and rotation.
[0057] To further illustrate, the auxiliary acid includes any one or more combinations of hydrochloric acid, nitric acid and sulfuric acid.
[0058] To further illustrate, the wavelength of the Bessel light beam is 1030 nm.
[0059] To further illustrate, the cleaning steps of step A and step E both include: cleaning the glass with acetone, anhydrous ethanol and deionized water in sequence.
[0060] In another preferred embodiment of the present technical solution, the cleaning step can use acetone, anhydrous ethanol and deionized water to clean the glass in sequence. Preferably, ultrasonic wave can also be applied to assist cleaning.
[0061] It should be noted that in step A, acetone and anhydrous ethanol are used to remove oil and stains on the glass surface, and deionized water is used to remove residual acetone and anhydrous ethanol. In step E, acetone and anhydrous ethanol are used to remove residual etching solution on the glass surface, and deionized water is used to remove residual acetone and anhydrous ethanol.
[0062] To further illustrate, the glass includes any one of soda-lime glass, aluminosilicate glass, quartz glass, borosilicate glass and lead silicate glass.
[0063] The technical solution of the present invention is further illustrated below through specific implementation methods.
[0064] Example 1
[0065] A. Clean the soda lime glass with acetone, anhydrous ethanol and deionized water in sequence, and use ultrasonic waves to assist in the cleaning process; then dry it in a vacuum drying oven;
[0066] B. Determine the processing points and processing path of laser processing on the glass surface in step A; wherein the distance between two adjacent processing points is 40 μm, and the processing path is a zigzag shape;
[0067] C. According to the processing path, the glass surface of step B is focused by a Bessel beam, and the processing point is laser processed to form a microstructure on the glass surface; wherein the Bessel beam is a pulsed laser with a repetition frequency of 100 kHz and a wavelength of 1030 nm; the laser power of the Bessel beam is 20 W, the pulse width is 1000 fs, and the number of pulses of the Bessel beam for laser processing any processing point is 1;
[0068] D. placing the glass in step C in an etching solution and etching for 10 minutes; wherein the etching solution comprises hydrofluoric acid and nitric acid, and in terms of mass percentage, the content of hydrofluoric acid is 10%, and the content of nitric acid is 10%;
[0069] E. Clean the soda-lime glass in step D with acetone, anhydrous ethanol and deionized water in sequence, and use ultrasonic wave to assist in the cleaning process; then dry it in a vacuum drying oven.
[0070] Example 2
[0071] A. Clean the quartz glass with acetone, anhydrous ethanol and deionized water in sequence, and use ultrasonic waves to assist in the cleaning process; then dry it in a vacuum drying oven;
[0072] B. Determine the processing points and processing path of laser processing on the glass surface in step A; wherein the distance between two adjacent processing points is 50 μm, and the processing path is a “U” shape;
[0073] C. According to the processing path, the glass surface of step B is focused by a Bessel beam, and the processing point is laser processed to form a microstructure on the glass surface; wherein the Bessel beam is a pulsed laser with a repetition frequency of 100 kHz and a wavelength of 1030 nm; the laser power of the Bessel beam is 40 W, the pulse width is 500 fs, and the number of pulses of the Bessel beam for laser processing any processing point is 6;
[0074] D. Place the glass in step C in an etching solution and etch for 15 minutes; wherein the etching solution comprises hydrofluoric acid and sulfuric acid, and in terms of mass percentage, the content of hydrofluoric acid is 15% and the content of sulfuric acid is 5%;
[0075] E. Clean the quartz glass in step D with acetone, anhydrous ethanol and deionized water in sequence, and use ultrasonic wave to assist in the cleaning process; then dry it in a vacuum drying oven.
[0076] Example 3
[0077] A. Cleaning the aluminosilicate glass with acetone, anhydrous ethanol and deionized water in sequence, and using ultrasonic waves to assist in the cleaning process; and then drying it in a vacuum drying oven;
[0078] B. Determine the processing points and processing path of laser processing on the glass surface in step A; wherein the distance between two adjacent processing points is 20 μm, and the processing path is a zigzag shape;
[0079] C. According to the processing path, the glass surface of step B is focused by a Bessel beam, and the processing point is laser processed to form a microstructure on the glass surface; wherein the Bessel beam is a pulsed laser with a repetition frequency of 100 kHz and a wavelength of 1030 nm; the laser power of the Bessel beam is 30 W, the pulse width is 4000 fs, and the number of pulses of the Bessel beam for laser processing any processing point is 1;
[0080] D. Place the glass in step C in an etching solution and etch for 25 minutes; wherein the etching solution comprises hydrofluoric acid and hydrochloric acid, and in terms of mass percentage, the content of hydrofluoric acid is 5%, and the content of hydrochloric acid is 15%;
[0081] E. Clean the aluminosilicate glass in step D with acetone, anhydrous ethanol and deionized water in sequence, and use ultrasonic waves to assist in the cleaning process; then dry it in a vacuum drying oven.
[0082] Metal films of the same thickness and type were plated on the glass surfaces of Examples 1-3 and the surface of untreated soda-lime glass with a smooth surface. The bonding strength of the above-mentioned glasses to the metal films was tested respectively using conventional testing methods in the art. The results are shown in Table 1 below.
[0083] Table 1 Binding strength of Examples 1-3 and smooth glass to metal film
[0084]
[0085] It can be seen from the test results in Table 1 that the glass treated by the method of the present technical solution has effectively improved bonding strength to the metal film compared to the unprocessed glass.
[0086] The technical principle of the present invention is described above in conjunction with specific embodiments. These descriptions are only for explaining the principle of the present invention and cannot be interpreted as limiting the scope of protection of the present invention in any way. Based on the explanations herein, those skilled in the art can associate other specific implementations of the present invention without paying creative labor, and these methods will fall within the scope of protection of the present invention.
Claims
1. A method for enhancing the bonding strength of a metal film on a glass surface, characterized in that: The following steps are involved: A. Clean and dry the glass; B. Determine the processing point and processing path of laser processing on the glass surface in step A; C. According to the processing path, focusing the Bessel beam on the glass surface of step B, and laser processing the processing point to form a microstructure on the glass surface; wherein the Bessel beam is a pulsed laser; D. placing the glass in step C in an etching solution for etching; E. Clean and dry the glass in step D.
2. A method for enhancing the bonding strength of a metal film on a glass surface according to claim 1, characterized in that: The laser power of the Bessel beam is 1-40W, and the pulse width of the Bessel beam is 290-6000fs.
3. The method for enhancing the bonding strength of a metal film on a glass surface according to claim 1, characterized in that: The distance between two adjacent processing points is smaller than the spot diameter of the Bessel light beam.
4. The method for enhancing the bonding strength of a metal film on a glass surface according to claim 1, characterized in that: In step C, the number of pulses of the Bessel beam for laser processing any one of the processing points is 1 to 9.
5. The method for enhancing the bonding strength of a metal film on a glass surface according to claim 1, characterized in that: Step D also includes: D. After repeating step C1 to 500 times, place the glass in an etching solution for etching.
6. The method for enhancing the bonding strength of a metal film on a glass surface according to claim 1, characterized in that: In step D, the etching solution includes hydrofluoric acid and auxiliary acid, and in terms of mass percentage, the content of the hydrofluoric acid is 5-20%, and the content of the auxiliary acid is 1-20%.
7. The method for enhancing the bonding strength of a metal film on a glass surface according to claim 6, characterized in that: The auxiliary acid includes any one or more combinations of hydrochloric acid, nitric acid and sulfuric acid.
8. The method for enhancing the bonding strength of a metal film on a glass surface according to claim 1, characterized in that: The wavelength of the Bessel beam is 1030 nm.
9. The method for enhancing the bonding strength of a metal film on a glass surface according to claim 1, characterized in that: The cleaning steps of step A and step E both include: cleaning the glass with acetone, anhydrous ethanol and deionized water in sequence.
10. The method for enhancing the bonding strength of a metal film on a glass surface according to claim 1, characterized in that: The glass includes any one of soda-lime glass, aluminosilicate glass, quartz glass, borosilicate glass and lead silicate glass.
Citation Information
Patent Citations
Method for producing regular texture structure on glass surface
CN107322167A
Laser processing optimization method and system of Bessel beams
CN109530913A
Method and device for compositely welding glass by double laser beams
CN111302609A
Laser cutting method and system for ground glass
CN115159828A
Femtosecond laser processing system and method based on Bessel beam
CN116851909A