Hydroxylated lignin composite cement solidified soil admixture and preparation method thereof

By combining hydroxylated lignin with γ-(2,3-epoxypropoxy)propyltrimethoxysilane and soil particles, combined with the antibacterial effect of silver-loaded zeolite particles, the dosage of industrial waste residue-type curing agent is solved. The problem of high energy consumption of Yamato cement improves the strength and durability of the cured soil, reduces transportation costs and improves the efficiency of waste soil resource utilization.

CN119059756AActive Publication Date: 2024-12-03POWERCHINA HUADONG ENG CORP LTD +1
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411555791.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-11-04
Publication Date
2024-12-03
Estimated Expiration
2044-11-04

AI Technical Summary

Technical Problem

The existing industrial waste slag-type curing agent is added large, which increases transportation costs and is highly regional, limiting its promotion and application in engineering. It also has high energy consumption and large carbon emissions, resulting in the resource utilization of slag soil. Inefficient.

Method used

Using hydroxylated lignin composite cement-cured soil admixture, lignin increases hydroxyl groups under the action of sodium hydroxide, and γ-(2,3-epoxypropoxy)propyltrimethoxysilane and soil particles. Dehydration and condensation, forming a firm bond, improving the strength and water stability of the solidified soil, and inhibiting microbial degradation through silver-loaded zeolite particles and extending the life of the material.

Benefits of technology

It significantly improves the strength, water stability and durability of the cured soil, reduces the amount of cement used, reduces transportation costs, and improves construction efficiency and material performance through prefabricated and pretreatment optimization.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention discloses a hydroxylated lignin composite cement-solidified soil admixture and a preparation method thereof, and particularly relates to the field of cement-solidified soil admixtures, the hydroxylated lignin composite cement-solidified soil admixture comprises the following components by weight: 10-30 parts of lignin, 10-30 parts of sodium hydroxide, 10-30 parts of gamma-(2, 2, 6-trimethyl-1, 3-pentanediol monoisobutyrate), 10-30 parts of a curing agent, and 10-30 parts of a curing agent. 2 to 6 parts of 1, 3-epoxypropoxy) propyl trimethoxy silane, and 1500 to 1700 parts of water. The admixture prepared by the invention has the effects of improving the cement hydration strength, the cement solidified soil strength and the solidification durability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of cement-solidified soil admixtures, in particular to a hydroxylated lignin composite cement-solidified soil admixture and a preparation method thereof. Background Art

[0002] With the increasing development of infrastructure and underground excavation, large quantities of waste soil are generated. Most of this waste soil has poor engineering properties, posing challenges to its resource utilization. Solidifiers are soil hardeners that can directly bind soil particles or react with clay minerals to form cement at room temperature. Their excellent performance in improving soil properties has led to a widening application range in recent years, including roadbed construction, embankment reinforcement, and unfired bricks. Cement, the most common soil solidifier, is widely used worldwide, particularly in countries such as Japan and Thailand. However, cement production is energy-intensive and produces significant carbon emissions. Consequently, industrial waste residue-based cementitious materials, such as desulfurized gypsum, steel, slag, and fly ash, are being widely researched due to their green, low-carbon, and economic benefits. However, industrial waste residue-based solidifiers have certain drawbacks, including the large dosage required (typically 10%-25% of the dry soil), which significantly increases transportation costs. Furthermore, industrial waste residue is highly regionally distributed and its production is scattered, all of which hinder the widespread application of construction waste residue in engineering projects. Therefore, researching an organic solidifying admixture that can be added in small amounts to reduce the amount of cement used and at the same time improve the performance of solidified soil is of great significance for improving the resource utilization of slag. Summary of the Invention

[0003] In view of the shortcomings of the prior art, the object of the present invention is to provide a hydroxylated lignin composite cement-solidified soil admixture and a preparation method thereof.

[0004] The above-mentioned object of the present invention is achieved through the following technical solutions: A hydroxylated lignin composite cement-solidified soil admixture comprises the following components in parts by weight: 10-30 parts of lignin; 10-30 parts of sodium hydroxide; γ-(2,3-epoxypropoxy)propyltrimethoxysilane 2-6 parts; 1500-1700 parts of water.

[0005] The present invention realizes the effective bonding of γ-(2,3-epoxypropoxy)propyltrimethoxysilane, lignin and soil particles through the following steps, thereby improving the strength and water stability of the solidified soil. First, lignin decomposes under the action of sodium hydroxide, increasing its hydroxyl groups. At the same time, the silicon oxides in the soil particles are corroded under alkaline conditions, also increasing the surface hydroxyl groups. Then, the Si-OH groups of γ-(2,3-epoxypropoxy)propyltrimethoxysilane undergo dehydration condensation with the hydroxyl groups in the soil particles or cement hydration products to form a strong bond. Finally, the epoxy groups of the silane open the ring under alkaline conditions and combine with the hydroxyl groups of the lignin, thereby achieving the connection between the silane and the lignin. Through these reactions, γ-(2,3-epoxypropoxy)propyltrimethoxysilane not only connects the lignin and soil particles together, but also forms an overall structure through the long chain action of the lignin, promotes cement hydration, and significantly improves the strength and water stability of the solidified soil.

[0006] Furthermore, the lignin is partially hydroxylated and pretreated, and the hydroxyl value of the lignin after the hydroxylation pretreatment is 30-60 mg / g.

[0007] Prior hydroxylation of lignin significantly improves its performance in reactions with γ-(2,3-epoxypropoxy)propyltrimethoxysilane and other matrices. First, hydroxylation increases the number of hydroxyl groups in lignin, enhancing its reactivity and making it more susceptible to ring-opening reactions with the epoxy groups in the silane, promoting chemical bonding. Second, the increased number of hydroxyl polar groups strengthens the interfacial bonding between lignin, the silane, and cement or soil particles, improving the overall structure of the material. Furthermore, hydroxylation enhances lignin's water solubility and dispersibility, ensuring its uniform distribution within the cement or soil matrix, thereby enhancing cementitious properties. By increasing the number of hydroxyl groups, lignin reacts with more γ-(2,3-epoxypropoxy)propyltrimethoxysilane, forming a more stable three-dimensional network structure that helps improve the strength and water stability of cement-stabilized soils. Improved dispersibility and reactivity also promote cement hydration, further increasing its ultimate strength. Furthermore, hydroxylation reduces the interference of impurities in lignin with the cement hydration reaction, ensuring its more efficient contribution to the reaction, thereby improving the overall performance and durability of the material.

[0008] Furthermore, the invention also comprises 0.5-1.5 parts of silver-loaded zeolite particles.

[0009] Furthermore, the D50 particle size of the silver-loaded zeolite particles is 100-500 μm.

[0010] The introduction of silver-loaded zeolite particles not only effectively inhibits harmful bacteria through their antibacterial properties, especially those that degrade and decompose lignin, but also maintains the stability of the solidified material and extends its service life. The antibacterial properties of silver ions in silver-loaded zeolite help reduce the reproduction of microorganisms in the solidified soil and prevent the degradation of material properties due to microbial activity. At the same time, this particle structure synergizes with the cementing system formed by lignin and γ-(2,3-epoxypropoxy)propyltrimethoxysilane to further enhance the stability and strength of cement solidification, allowing the solidified soil to maintain high strength and water stability during long-term use. This admixture not only improves the mechanical properties of cement-solidified soil, but also ensures its durability through its antibacterial effect, effectively avoiding degradation problems caused by microbial erosion.

[0011] Furthermore, the lignin and γ-(2,3-epoxypropoxy)propyltrimethoxysilane are preformed into a preform, and the preform comprises the following components in parts by weight: 10-30 parts of lignin; γ-(2,3-epoxypropoxy)propyltrimethoxysilane 2-6 parts; 20-30 parts of alkali agent; 20-30 parts of acid agent.

[0012] Furthermore, the alkaline agent is selected from sodium carbonate and / or sodium bicarbonate, and the acidic agent is selected from one or more of citric acid, tartaric acid or boric acid.

[0013] Furthermore, the method for preparing the preform includes the following steps: mixing lignin, γ-(2,3-epoxypropoxy)propyltrimethoxysilane, an alkali agent, and an acid agent uniformly and then pressing the mixture into tablets.

[0014] By adopting the above technical solution, the preform is conducive to effectively preventing component reactions caused by moisture or environmental changes during storage and transportation, and is more convenient to use at the construction site. The compressed material is easy to carry, store and place, reducing the operational complexity of traditional liquid or powder admixtures and improving construction efficiency. On the other hand, prefabricating lignin and γ-(2,3-epoxypropoxy)propyltrimethoxysilane into a preform helps to ensure the uniformity of the mixing of lignin and γ-(2,3-epoxypropoxy)propyltrimethoxysilane. The alkali and acid react in water to produce a large number of bubbles. Under the action of the bubbles, the reaction between lignin and γ-(2,3-epoxypropoxy)propyltrimethoxysilane is faster, and lignin can more quickly combine with some of the epoxy groups in γ-(2,3-epoxypropoxy)propyltrimethoxysilane to form a prepolymer. As a result, after the admixture is mixed with cement and soil, the admixture can quickly take effect, more evenly and quickly promote the water splash of cement, and make the soil particles more quickly and firmly bonded. Furthermore, the reaction of the alkali and acid in water to produce a large number of bubbles will also promote the uniform dispersion of the silver-loaded zeolite particles, and a trace amount of γ-(2,3-epoxypropoxy)propyltrimethoxysilane will also be mixed with the silver-loaded zeolite particles under the action of the bubbles. During the solidification process of the admixture and the soil, the silver-loaded zeolite particles that have adsorbed a trace amount of γ-(2,3-epoxypropoxy)propyltrimethoxysilane are more evenly dispersed in the solidified soil and are more firmly and stably disposed.

[0015] Furthermore, the lignin is pretreated before being preformed with γ-(2,3-epoxypropoxy)propyltrimethoxysilane to form a preform, and the pretreatment includes the following steps: A1: Mix lignin and saturated glucose solution evenly and heat to evaporate the water into syrup; A2: Add the syrup to a sealed container and pressurize to 30-40 atmospheres, then cool to room temperature; A3: Grind the cooled syrup solids into granules.

[0016] Furthermore, the D50 particle size of the particles is no greater than 1 mm.

[0017] On the one hand, pre-treatment of lignin before making it into a preform can improve the reaction activity of lignin. On the other hand, the particles formed by lignin and glucose will also produce a large number of bubbles when encountering water during the disintegration of the preform, and have a certain pressure. These bubbles directly act on the lignin, so that the preform can disintegrate more quickly and accelerate the dispersion of the preform.

[0018] A method for preparing the above-mentioned hydroxylated lignin composite cement-solidified soil admixture comprises the following steps: S1: Mix all components in proportion; S2: Heating is performed by reflux through a condenser, the temperature is controlled at 45-60°C, and the reaction time is 20-40 minutes; S3: After the reaction is completed, the mixture is cooled to room temperature and then stored in liquid form for later use.

[0019] Compared with the prior art, the present invention has the following beneficial effects: The present invention utilizes the decomposition of lignin under the action of sodium hydroxide to increase the hydroxyl group and enhance the binding force with silicon oxides in soil particles. At the same time, the Si-OH group of γ-(2,3-epoxypropoxy)propyltrimethoxysilane dehydrates and condenses with the hydroxyl groups in cement or soil, thereby enhancing the bonding strength of the material. Through the ring-opening reaction of the silane epoxy group and lignin under alkaline conditions, a strong bond is formed between lignin and silane, which further promotes the hydration reaction of cement and improves the mechanical properties of the solidified soil. In addition, the hydroxylation treatment of lignin increases its hydroxyl number and reaction activity, improves the uniform distribution and bonding effect of the material, and thus constructs a stable three-dimensional network structure. The introduction of silver-loaded zeolite particles effectively inhibits the degradation of lignin by microorganisms and extends the service life of the solidified material. The further innovation of the present invention is particularly reflected in the optimized design of the preform and pretreatment. First, by pre-mixing and tableting the lignin, silane coupling agent, alkali agent, and acid agent, the preform effectively avoids component reactions caused by moisture or environmental changes during storage and transportation, ensuring rapid reaction of the components at the construction site. Furthermore, the alkali agent and acid agent react in water to produce bubbles, which accelerate the reaction between lignin and silane epoxy groups, allowing the admixture to act more quickly and evenly in the cement and soil, significantly improving construction efficiency and cement hydration.

[0020] The pretreatment step further enhances the reactivity of the lignin. By mixing it with a glucose solution and pressurizing it to form syrupy particles, this pretreatment not only strengthens the binding between the lignin and the silane but also creates bubbles when the preform disintegrates into water, accelerating its dissolution and dispersion, further improving the admixture's reaction rate and uniformity. Thus, the pretreatment and preform design work together to ensure the admixture's high performance, significantly enhancing the strength, durability, and water stability of the stabilized soil. DETAILED DESCRIPTION

[0021] The present invention is described in detail below with reference to the embodiments.

[0022] Example 1 A hydroxylated lignin composite cement-solidified soil admixture comprises the following components in parts by weight: 20 parts of lignin; 20 parts of sodium hydroxide; 3 parts of γ-(2,3-epoxypropoxy)propyltrimethoxysilane; 1600 parts of water.

[0023] A method for preparing the above-mentioned hydroxylated lignin composite cement-solidified soil admixture comprises the following steps: S1: Mix all components in proportion; S2: heating by condenser reflux, controlling the temperature at 40°C, and the reaction time for 40 minutes; S3: After the reaction is completed, the mixture is cooled to room temperature and then stored in liquid form for later use.

[0024] Example 2 A hydroxylated lignin composite cement-solidified soil admixture comprises the following components in parts by weight: 10 parts of lignin; 10 parts of sodium hydroxide; γ-(2,3-epoxypropoxy)propyltrimethoxysilane 2 parts; 1500 parts of water.

[0025] A method for preparing the above-mentioned hydroxylated lignin composite cement-solidified soil admixture comprises the following steps: S1: Mix all components in proportion; S2: Heating was performed by reflux using a condenser, the temperature was controlled at 45°C, and the reaction time was 20 minutes; S3: After the reaction is completed, the mixture is cooled to room temperature and then stored in liquid form for later use.

[0026] Example 3 A hydroxylated lignin composite cement-solidified soil admixture comprises the following components in parts by weight: 30 parts of lignin; 30 parts of sodium hydroxide; γ-(2,3-epoxypropoxy)propyltrimethoxysilane 6 parts; 1700 parts of water.

[0027] A method for preparing the above-mentioned hydroxylated lignin composite cement-solidified soil admixture comprises the following steps: S1: Mix all components in proportion; S2: heating by condenser reflux, controlling the temperature at 60°C, and the reaction time for 20 minutes; S3: After the reaction is completed, the mixture is cooled to room temperature and then stored in liquid form for later use.

[0028] Example 4 A hydroxylated lignin composite cement-solidified soil admixture comprises the following components in parts by weight: 15 parts of lignin; 15 parts of sodium hydroxide; 4 parts of γ-(2,3-epoxypropoxy)propyltrimethoxysilane; 1600 parts of water.

[0029] A method for preparing the above-mentioned hydroxylated lignin composite cement-solidified soil admixture comprises the following steps: S1: Mix all components in proportion; S2: heating by condenser reflux, controlling the temperature at 50°C, and the reaction time for 30 minutes; S3: After the reaction is completed, the mixture is cooled to room temperature and then stored in liquid form for later use.

[0030] Example 5 A hydroxylated lignin composite cement-solidified soil admixture comprises the following components in parts by weight: 30 parts of lignin; 30 parts of sodium hydroxide; 3 parts of γ-(2,3-epoxypropoxy)propyltrimethoxysilane; 1500 parts of water.

[0031] A method for preparing the above-mentioned hydroxylated lignin composite cement-solidified soil admixture comprises the following steps: S1: Mix all components in proportion; S2: Heating was performed by reflux using a condenser, the temperature was controlled at 60°C, and the reaction time was 40 minutes; S3: After the reaction is completed, the mixture is cooled to room temperature and then stored in liquid form for later use.

[0032] Example 6 A hydroxylated lignin composite cement-solidified soil admixture comprises the following components in parts by weight: 30 parts of lignin; 30 parts of sodium hydroxide; 3 parts of γ-(2,3-epoxypropoxy)propyltrimethoxysilane; 1500 parts of water.

[0033] The lignin is partially hydroxylated and pretreated, and the hydroxyl value of the lignin after the hydroxylation pretreatment is 30 mg / g.

[0034] A method for preparing the above-mentioned hydroxylated lignin composite cement-solidified soil admixture comprises the following steps: S1: Mix all components in proportion; S2: Heating was performed by reflux using a condenser, the temperature was controlled at 60°C, and the reaction time was 40 minutes; S3: After the reaction is completed, the mixture is cooled to room temperature and then stored in liquid form for later use.

[0035] Example 7 A hydroxylated lignin composite cement-solidified soil admixture comprises the following components in parts by weight: 30 parts of lignin; 30 parts of sodium hydroxide; 3 parts of γ-(2,3-epoxypropoxy)propyltrimethoxysilane; 1500 parts of water.

[0036] The lignin is partially hydroxylated and pretreated, and the hydroxyl value of the lignin after the hydroxylation pretreatment is 45 mg / g.

[0037] A method for preparing the above-mentioned hydroxylated lignin composite cement-solidified soil admixture comprises the following steps: S1: Mix all components in proportion; S2: Heating was performed by reflux using a condenser, the temperature was controlled at 60°C, and the reaction time was 40 minutes; S3: After the reaction is completed, the mixture is cooled to room temperature and then stored in liquid form for later use.

[0038] Example 8 A hydroxylated lignin composite cement-solidified soil admixture comprises the following components in parts by weight: 30 parts of lignin; 30 parts of sodium hydroxide; 3 parts of γ-(2,3-epoxypropoxy)propyltrimethoxysilane; 1500 parts of water.

[0039] The lignin is partially hydroxylated and pretreated, and the hydroxyl value of the lignin after the hydroxylation pretreatment is 60 mg / g.

[0040] A method for preparing the above-mentioned hydroxylated lignin composite cement-solidified soil admixture comprises the following steps: S1: Mix all components in proportion; S2: Heating was performed by reflux using a condenser, the temperature was controlled at 60°C, and the reaction time was 40 minutes; S3: After the reaction is completed, the mixture is cooled to room temperature and then stored in liquid form for later use.

[0041] Example 9 A hydroxylated lignin composite cement-solidified soil admixture comprises the following components in parts by weight: 30 parts of lignin; 30 parts of sodium hydroxide; 3 parts of γ-(2,3-epoxypropoxy)propyltrimethoxysilane; 0.5 parts of silver-loaded zeolite particles; 1500 parts of water.

[0042] The lignin is partially hydroxylated and pretreated, and the hydroxyl value of the lignin after the hydroxylation pretreatment is 50 mg / g.

[0043] The D50 particle size of the silver-loaded zeolite particles is 100 μm.

[0044] A method for preparing the above-mentioned hydroxylated lignin composite cement-solidified soil admixture comprises the following steps: S1: Mix all components in proportion; S2: Heating was performed by reflux using a condenser, the temperature was controlled at 60°C, and the reaction time was 40 minutes; S3: After the reaction is completed, the mixture is cooled to room temperature and then stored in liquid form for later use.

[0045] Example 10 A hydroxylated lignin composite cement-solidified soil admixture comprises the following components in parts by weight: 30 parts of lignin; 30 parts of sodium hydroxide; 3 parts of γ-(2,3-epoxypropoxy)propyltrimethoxysilane; 1.5 parts of silver-loaded zeolite particles; 1500 parts of water.

[0046] The lignin is partially hydroxylated and pretreated, and the hydroxyl value of the lignin after the hydroxylation pretreatment is 50 mg / g.

[0047] The D50 particle size of the silver-loaded zeolite particles is 500 μm.

[0048] A method for preparing the above-mentioned hydroxylated lignin composite cement-solidified soil admixture comprises the following steps: S1: Mix all components in proportion; S2: Heating was performed by reflux using a condenser, the temperature was controlled at 60°C, and the reaction time was 40 minutes; S3: After the reaction is completed, the mixture is cooled to room temperature and then stored in liquid form for later use.

[0049] Example 11 A hydroxylated lignin composite cement-solidified soil admixture comprises the following components in parts by weight: 30 parts of lignin; 30 parts of sodium hydroxide; 3 parts of γ-(2,3-epoxypropoxy)propyltrimethoxysilane; 1 part of silver-loaded zeolite particles; 1500 parts of water.

[0050] The lignin is partially hydroxylated and pretreated, and the hydroxyl value of the lignin after the hydroxylation pretreatment is 50 mg / g.

[0051] The D50 particle size of the silver-loaded zeolite particles is 300 μm.

[0052] A method for preparing the above-mentioned hydroxylated lignin composite cement-solidified soil admixture comprises the following steps: S1: Mix all components in proportion; S2: Heating was performed by reflux using a condenser, the temperature was controlled at 60°C, and the reaction time was 40 minutes; S3: After the reaction is completed, the mixture is cooled to room temperature and then stored in liquid form for later use.

[0053] Example 12 A hydroxylated lignin composite cement-solidified soil admixture comprises the following components in parts by weight: 30 parts of lignin; 30 parts of sodium hydroxide; 3 parts of γ-(2,3-epoxypropoxy)propyltrimethoxysilane; 1500 parts of water.

[0054] The lignin is partially hydroxylated and pretreated, and the hydroxyl value of the lignin after the hydroxylation pretreatment is 50 mg / g.

[0055] Lignin and γ-(2,3-epoxypropoxy)propyltrimethoxysilane are preformed into a preform, and the preform comprises the following components in parts by weight: 10 parts of lignin; γ-(2,3-epoxypropoxy)propyltrimethoxysilane 2 parts; 20 parts of alkali agent; 20 parts of acid agent.

[0056] The alkaline agent is sodium bicarbonate, and the acidic agent is citric acid.

[0057] The preparation method of the preform comprises the following steps: mixing lignin, gamma-(2,3-epoxypropoxy)propyltrimethoxysilane, an alkali agent and an acid agent uniformly and then pressing the mixture into tablets.

[0058] A method for preparing the above-mentioned hydroxylated lignin composite cement-solidified soil admixture comprises the following steps: S1: Mix all components in proportion; S2: Heating was performed by reflux using a condenser, the temperature was controlled at 60°C, and the reaction time was 40 minutes; S3: After the reaction is completed, the mixture is cooled to room temperature and then stored in liquid form for later use.

[0059] Example 13 A hydroxylated lignin composite cement-solidified soil admixture comprises the following components in parts by weight: 30 parts of lignin; 30 parts of sodium hydroxide; 3 parts of γ-(2,3-epoxypropoxy)propyltrimethoxysilane; 1 part of silver-loaded zeolite particles; 1500 parts of water.

[0060] The lignin is partially hydroxylated and pretreated, and the hydroxyl value of the lignin after the hydroxylation pretreatment is 50 mg / g.

[0061] The D50 particle size of the silver-loaded zeolite particles is 500 μm.

[0062] Lignin and γ-(2,3-epoxypropoxy)propyltrimethoxysilane are preformed into a preform, and the preform comprises the following components in parts by weight: 10 parts of lignin; γ-(2,3-epoxypropoxy)propyltrimethoxysilane 2 parts; 20 parts of alkali agent; 20 parts of acid agent.

[0063] The alkaline agent is sodium bicarbonate, and the acidic agent is citric acid.

[0064] The preparation method of the preform comprises the following steps: mixing lignin, gamma-(2,3-epoxypropoxy)propyltrimethoxysilane, an alkali agent and an acid agent uniformly and then pressing the mixture into tablets.

[0065] A method for preparing the above-mentioned hydroxylated lignin composite cement-solidified soil admixture comprises the following steps: S1: Mix all components in proportion; S2: Heating was performed by reflux using a condenser, the temperature was controlled at 60°C, and the reaction time was 40 minutes; S3: After the reaction is completed, the mixture is cooled to room temperature and then stored in liquid form for later use.

[0066] Example 14 A hydroxylated lignin composite cement-solidified soil admixture comprises the following components in parts by weight: 30 parts of lignin; 30 parts of sodium hydroxide; 3 parts of γ-(2,3-epoxypropoxy)propyltrimethoxysilane; 1 part of silver-loaded zeolite particles; 1500 parts of water.

[0067] The lignin is partially hydroxylated and pretreated, and the hydroxyl value of the lignin after the hydroxylation pretreatment is 50 mg / g.

[0068] The D50 particle size of the silver-loaded zeolite particles is 500 μm.

[0069] Lignin and γ-(2,3-epoxypropoxy)propyltrimethoxysilane are preformed into a preform, and the preform comprises the following components in parts by weight: 30 parts of lignin; γ-(2,3-epoxypropoxy)propyltrimethoxysilane 6 parts; 30 parts of alkali agent; 30 parts of acid agent.

[0070] The alkaline agent is sodium bicarbonate, and the acidic agent is citric acid.

[0071] The preparation method of the preform comprises the following steps: mixing lignin, gamma-(2,3-epoxypropoxy)propyltrimethoxysilane, an alkali agent and an acid agent uniformly and then pressing the mixture into tablets.

[0072] A method for preparing the above-mentioned hydroxylated lignin composite cement-solidified soil admixture comprises the following steps: S1: Mix all components in proportion; S2: Heating was performed by reflux using a condenser, the temperature was controlled at 60°C, and the reaction time was 40 minutes; S3: After the reaction is completed, the mixture is cooled to room temperature and then stored in liquid form for later use.

[0073] Example 15 A hydroxylated lignin composite cement-solidified soil admixture comprises the following components in parts by weight: 30 parts of lignin; 30 parts of sodium hydroxide; 3 parts of γ-(2,3-epoxypropoxy)propyltrimethoxysilane; 1 part of silver-loaded zeolite particles; 1500 parts of water.

[0074] The lignin is partially hydroxylated and pretreated, and the hydroxyl value of the lignin after the hydroxylation pretreatment is 50 mg / g.

[0075] The D50 particle size of the silver-loaded zeolite particles is 500 μm.

[0076] Lignin and γ-(2,3-epoxypropoxy)propyltrimethoxysilane are preformed into a preform, and the preform comprises the following components in parts by weight: 20 parts of lignin; 4 parts of γ-(2,3-epoxypropoxy)propyltrimethoxysilane; 25 parts of alkali agent; 25 parts of acid agent.

[0077] The alkaline agent is sodium bicarbonate, and the acidic agent is citric acid.

[0078] The preparation method of the preform comprises the following steps: mixing lignin, gamma-(2,3-epoxypropoxy)propyltrimethoxysilane, an alkali agent and an acid agent uniformly and then pressing the mixture into tablets.

[0079] A method for preparing the above-mentioned hydroxylated lignin composite cement-solidified soil admixture comprises the following steps: S1: Mix all components in proportion; S2: Heating was performed by reflux using a condenser, the temperature was controlled at 60°C, and the reaction time was 40 minutes; S3: After the reaction is completed, the mixture is cooled to room temperature and then stored in liquid form for later use.

[0080] Example 16 A hydroxylated lignin composite cement-solidified soil admixture comprises the following components in parts by weight: 30 parts of lignin; 30 parts of sodium hydroxide; 3 parts of γ-(2,3-epoxypropoxy)propyltrimethoxysilane; 1 part of silver-loaded zeolite particles; 1500 parts of water.

[0081] The lignin is partially hydroxylated and pretreated, and the hydroxyl value of the lignin after the hydroxylation pretreatment is 50 mg / g.

[0082] The D50 particle size of the silver-loaded zeolite particles is 500 μm.

[0083] The lignin is first pre-treated, and the pre-treatment comprises the following steps: A1: Mix lignin and saturated glucose solution at a mass ratio of 1:50, then heat and evaporate the water to form a syrup. A2: Add the syrup to a sealed container and pressurize to 40 atmospheres, then cool to room temperature; A3: Grind the cooled syrup solids into granules.

[0084] The D50 particle size of the particles is 0.8 mm.

[0085] Lignin and γ-(2,3-epoxypropoxy)propyltrimethoxysilane are preformed into a preform, and the preform includes the following components in parts by weight: 20 parts of lignin; 4 parts of γ-(2,3-epoxypropoxy)propyltrimethoxysilane; 25 parts of alkali agent; 25 parts of acid agent.

[0086] The alkaline agent is sodium bicarbonate, and the acidic agent is citric acid.

[0087] The preparation method of the preform comprises the following steps: mixing lignin, gamma-(2,3-epoxypropoxy)propyltrimethoxysilane, an alkali agent and an acid agent uniformly and then pressing the mixture into tablets.

[0088] A method for preparing the above-mentioned hydroxylated lignin composite cement-solidified soil admixture comprises the following steps: S1: Mix all components in proportion; S2: Heating was performed by reflux using a condenser, the temperature was controlled at 60°C, and the reaction time was 40 minutes; S3: After the reaction is completed, the mixture is cooled to room temperature and then stored in liquid form for later use.

[0089] Comparative Example The admixture used in Comparative Example 1 is obtained by uniformly mixing the following components in parts by weight: 20 parts of lignin; 20 parts of sodium hydroxide; 1600 parts of water.

[0090] Detection method Curing performance test First, add 7% of the dry weight of the soil to be solidified into cement and dry mix it evenly. The geotechnical properties of the soil are shown in Table 1: The admixture solutions prepared in the Examples and Comparative Examples were then added, and the required amount of water was calculated based on the optimal moisture content at the maximum dry density of the soil. The mixture was then compacted and cured at 25°C for 7 days. The unconfined compressive strength (UCS) of the cured soil was finally tested, and the UCS was further tested after the cured soil was placed in silt for 6 months.

[0091] The test results are shown in Table 2. The control group is soil solidified with cement only.

[0092] Conclusion: The above test results show that the curing performance of cement-cured soil is significantly improved after the admixture prepared by the present invention is added, and when lignin and γ-(2,3-epoxypropoxy)propyltrimethoxysilane are prefabricated into a preform, the antibacterial ability of the silver-loaded zeolite particles is also significantly improved.

[0093] The above description is merely a preferred embodiment of the present invention. The scope of protection of the present invention is not limited to the above embodiment. All technical solutions based on the concept of the present invention are within the scope of protection of the present invention. It should be noted that for those skilled in the art, various improvements and modifications that do not depart from the principles of the present invention should also be considered within the scope of protection of the present invention.

Claims

1. A hydroxylated lignin composite cement-stabilized soil admixture, characterized in that: The composition comprises the following components in parts by weight: 10-30 parts of lignin; 10-30 parts of sodium hydroxide; γ-(2,3-epoxypropoxy)propyltrimethoxysilane 2-6 parts; 1500-1700 parts of water.

2. The hydroxylated lignin composite cement-stabilized soil admixture according to claim 1, characterized in that: The lignin is partially hydroxylated and pretreated, and the hydroxyl value of the lignin after the hydroxylation pretreatment is 30-60 mg / g.

3. The hydroxylated lignin composite cement-stabilized soil admixture according to claim 1, characterized in that: Also included are 0.5-1.5 parts of silver-loaded zeolite particles.

4. The hydroxylated lignin composite cement-stabilized soil admixture according to claim 3, characterized in that: The D50 particle size of the silver-loaded zeolite particles is 100-500 μm.

5. The hydroxylated lignin composite cement-stabilized soil admixture according to claim 4, characterized in that: The lignin and γ-(2,3-epoxypropoxy)propyltrimethoxysilane are preformed into a preform, and the preform includes the following components in parts by weight: 10-30 parts of lignin; γ-(2,3-epoxypropoxy)propyltrimethoxysilane 2-6 parts; 20-30 parts of alkali agent; 20-30 parts of acid agent.

6. The hydroxylated lignin composite cement-stabilized soil admixture according to claim 5, characterized in that: The alkaline agent is selected from sodium carbonate and / or sodium bicarbonate, and the acid agent is selected from one or more of citric acid, tartaric acid or boric acid.

7. The hydroxylated lignin composite cement-stabilized soil admixture according to claim 5, characterized in that: The preparation method of the preform comprises the following steps: lignin, gamma-(2,3-epoxypropoxy)propyltrimethoxysilane, an alkali agent and an acid agent are uniformly mixed and then tabletted.

8. The hydroxylated lignin composite cement-stabilized soil admixture according to claim 5, characterized in that: The lignin is pretreated before being preformed into a preform with γ-(2,3-epoxypropoxy)propyltrimethoxysilane. The following steps are involved: A1: Mix lignin and saturated glucose solution evenly and heat to evaporate water into syrup; A2: Add the syrup into a sealed container and inject 30-40 atmospheres of pressure, then cool to room temperature; A3: The cooled syrup solids are crushed into particles.

9. The hydroxylated lignin composite cement-stabilized soil admixture according to claim 7, characterized in that: The D50 particle size of the particles is no greater than 1 mm.

10. A method for preparing a hydroxylated lignin composite cement-stabilized soil admixture according to any one of claims 1 to 9, characterized in that: The following steps are involved: S1: Mix all components in proportion; S2: heating by reflux of condenser tube, controlling the temperature at 45°C-60°C, and the reaction time at 20-40 minutes; S3: After the reaction is completed, cool to room temperature and keep in liquid form for later use.

Citation Information

Patent Citations

  • Antibacterial cultivation substrate for volvaria volvacea and preparation method of antibacterial cultivation substrate

    CN108812068A

  • Preparation of nano-ion composite muck curing agent

    CN111233369A

  • Soil stabilizer, stabilized soil and method for roadbed backfilling in soft stratum

    CN113072950A

  • Composite sandy soil curing agent and application method thereof

    CN116477874A

  • Method for in-situ modification and curing of lignin-based composite curing agent

    CN117164289A