Preparation method of selenized polyacrylonitrile-based positive electrode material of high-load sodium-selenium battery

By loading SePAN particles on a three-dimensional gel frame composed of MXene and rGO, a high-load sodium selenium battery positive electrode material was prepared, which solved the problems of cycling stability and capacity attenuation of sodium selenium batteries, and achieved high energy density and long cycles Battery performance for life.

CN119059760APending Publication Date: 2024-12-03BEIJING UNIV OF CHEM TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411212108.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The change in the volume of selenium element in sodium selenium batteries during the charge and discharge cycle leads to damage to the electrode structure, and the multi-selenide is easily soluble in organic electrolytes to cause a "shuttle effect", resulting in the loss of active substances and the attenuation of battery capacity, making it difficult to achieve high energy density and long Cycle life.

Method used

The three-dimensional gel frame formed by cross-linking of two-dimensional sheet materials rGO and MXene, loading SePAN particles is loaded, and high-load SePAN/MXene/rGO aerogel is prepared by ultrasonic stirring and hydrothermal treatment, and high-loading SePAN/MXene/rGO aerogel is cut and tableted to obtain high load. The sodium selenium battery cathode material avoids the use of conductive agents and current collectors.

Benefits of technology

The high surface load of SePAN material is achieved, the active Se content can be controlled between 5-10 mg/cm2, and the battery's first discharge capacity reaches 532mAh/g at a current density of 0.1C. The capacity retention rate after 40 cycles is about 93%, which is significantly Improves the energy density and cycle stability of sodium selenium batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119059760A_ABST
    Figure CN119059760A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of electrode materials, in particular to a preparation method of a high-load sodium-selenium battery selenized polyacrylonitrile-based positive electrode material. The invention provides a method for preparing a high-load positive electrode material of a sodium-selenium battery, which comprises the following steps of: mixing selenium powder and polyacrylonitrile, and sintering, so as to obtain black selenized polyacrylonitrile (SePAN for short) powder with uniform particles; carrying out ultrasonic stirring on the powder and a suspension of single-layer graphene oxide and a two-dimensional layered material Ti3C2Tx-MXene, uniformly mixing, carrying out low-temperature hydrothermal treatment to obtain three-dimensional SePAN / MXene / rGO gel, and carrying out freeze drying to obtain the three-dimensional network SePAN / MXene / rGO aerogel uniformly loaded with SePAN; and cutting and tabletting the aerogel to obtain the high-load SePAN-based positive electrode of the sodium-selenium battery. The preparation process is simple, the electrode structure is stable, a conductive agent and a binding agent are not needed, high-activity substance loading can be achieved, and possibility is provided for development of a high-energy sodium-selenium battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of sodium-selenium battery electrode materials, and in particular to the preparation of a sodium-selenium battery high-load selenized polyacrylonitrile-based positive electrode material and its application in the field of sodium-selenium batteries. Background Art

[0002] With the rapid development of new energy vehicles and energy storage industries, the demand for high energy density and low-cost energy storage technologies continues to increase. As a new type of high energy density battery, sodium selenium battery has gradually attracted the attention of researchers in recent years. Sodium selenium battery is a kind of battery that uses metallic sodium (Na) as the negative electrode and selenium (Se) as the positive electrode to store and release energy through electrochemical reactions. As a positive electrode material, selenium has high electronic conductivity, which can make sodium selenium battery have excellent rate performance. Secondly, due to its high density, the volumetric capacity of selenium can reach 3253mAh / cm 3 , the volume occupied is smaller when outputting the same energy, so the battery has a high volume energy density. In addition, compared with high-temperature sodium-sulfur batteries, sodium-selenium batteries can work at room temperature, so they are safer.

[0003] However, the application of sodium-selenium batteries also faces significant challenges. During the charge and discharge cycle of the battery, the volume of the selenium element changes significantly, resulting in the destruction of the electrode structure; in addition, polyselenides are easily soluble in organic electrolytes and cause a "shuttle effect", which causes the loss of active substances and the rapid decay of battery capacity. Covalent selenium-based materials are materials that form selenium-carbon bonds between selenium and organic carbon rings. They have excellent cycle stability when used as the positive electrode of sodium-selenium batteries; Selenized polyacrylonitrile (SePAN) is a typical covalent selenium-based positive electrode material that can effectively suppress the "shuttle effect" problem and has good application development prospects.

[0004] The key to achieving high energy density sodium-selenium batteries is to prepare positive electrode materials with high active material loading. However, due to the limited content of active Se in SePAN, the surface loading of Se in the prepared electrodes under the traditional slurry coating process is less than 1 mg / cm 2 , it is difficult to achieve high surface loading. The present invention uses aerogel formed by cross-linking two-dimensional sheet materials rGO and MXene as a three-dimensional skeleton, which not only achieves a high loading of active substances, but also the excellent conductivity of MXene and rGO makes the electrode no longer need a conductive agent and a current collector, which comprehensively optimizes the energy density and rate performance of the sodium-selenium battery. The active Se content in the high-load selenized polyacrylonitrile electrode prepared by the present invention can be controlled at 5-10 mg / cm 2, which is close to the electrode loading level of commercial lithium-ion batteries, showing great development potential. Therefore, the preparation of high-load SePAN-based positive electrode materials is an important way to achieve high-performance and long cycle life sodium-selenium batteries. Summary of the invention

[0005] The purpose of the present invention is to provide a method for preparing a high-load SePAN-based material for a sodium-selenium battery. By loading SePAN particles on a three-dimensional gel conductive skeleton composed of MXene and rGO, the loading amount of the SePAN material can be controlled, and finally a high-surface-load self-supporting sodium-selenium battery positive electrode is obtained. The positive electrode material used for the sodium-selenium battery has high capacity and excellent cycle performance.

[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0007] (1) Selenium powder and polyacrylonitrile are mixed and sintered to obtain SePAN powder with uniform particles; a single-layer MXene suspension is obtained by a typical lithium fluoride + concentrated hydrochloric acid etching method;

[0008] (2) The prepared SePAN powder, commercial monolayer graphene oxide, and prepared MXene suspension are mixed with a reducing agent, ultrasonically stirred, and heated for reduction, and then washed to obtain SePAN / MXene / rGO gel, which is freeze-dried to obtain SePAN / MXene / rGO aerogel; the heating reduction is carried out under the protection of an inert atmosphere.

[0009] (3) Cutting and pressing the SePAN / MXene / rGO aerogel obtained in step (1) to obtain a high-load SePAN-based positive electrode material for sodium-selenium batteries.

[0010] Preferably, the MXene type in step (1) should be Ti3C2T x or Ti2CT x , concentration is 1-5mg / ml.

[0011] Preferably, the ratio of selenium powder to polyacrylonitrile in step (1) is 2:1-8:1, the sintering temperature is 400-600°C, the heating rate is 2-10°C / min, and the insulation time is 1h-10h.

[0012] Preferably, the reducing agent added in step (1) comprises one of oxalic acid, ascorbic acid and citric acid, and the amount of the reducing agent added is 50-150 mg.

[0013] Preferably, the mass ratio of SePAN powder, graphene oxide and MXene in step (2) is 8:2:1-3:2:1, the stirring time is 0.5-12h, the ultrasonic time is 1-2h, and the inert gas introduced is one of argon, nitrogen and helium.

[0014] Preferably, the reaction container in step (2) should be a cylindrical glass bottle with a diameter of 2-6 cm.

[0015] Preferably, the hydrothermal temperature in step (2) is 60-120° C., the hydrothermal time is 5-15 h, deionized water is used for washing, and the number of washing times is 4-8 times.

[0016] Preferably, the aerogel in step (2) needs to be uniformly cut into different segments after drying in order to control the loading range, the cutting is 0-5 times, the tableting pressure is 5-20 MPa, and the holding time is 1-10 s.

[0017] The present invention provides a method for preparing a high-loaded SePAN-based positive electrode material for a sodium-selenium battery, comprising the following steps: firstly, a typical lithium fluoride+concentrated hydrochloric acid etching method is used to prepare a single-layer MXene suspension so as to cross-link with a single-layer graphene oxide to form a three-dimensional gel skeleton, so as to better load the active substance SePAN on the skeleton; SePAN powder is prepared by mixing selenium powder and polyacrylonitrile and then heating them for reaction, and the heating reaction is carried out under the protection of an inert atmosphere. The SePAN powder, monolayer graphene oxide, MXene suspension and reducing agent prepared above are stirred in a certain proportion, and after being evenly mixed, they are hydrothermally heated at low temperature for a certain period of time to obtain SePAN / MXene / rGO gel. In the process of preparing the gel, ultrasonic stirring is required for a certain period of time to ensure that the three are evenly mixed. The purpose of adding the reducing agent is to reduce the graphene oxide GO to reduced graphene oxide rGO, wherein the mass of graphene oxide is halved in the process of being reduced to reduced graphene oxide. In the present invention, the graphene oxide is weighed according to the mass ratio of the reduced reduced graphene oxide to MXene of 1:1. At this ratio, the two can be cross-linked into a stable gel skeleton and the conductivity of the gel is guaranteed (MXene The material has excellent electrical conductivity). The purpose of hydrothermal treatment is to promote the reduction of graphene oxide and two-dimensional MXene sheets to form a gel. The generated gel needs to be washed with deionized water to remove excess reducing agent. The prepared gel is freeze-dried to obtain SePAN / MXene / rGO aerogel. The purpose of freeze-drying is to remove moisture from the gel and slow down the oxidation of MXene. The aerogel needs to be cut to control the SePAN loading in the target electrode. Finally, the aerogel is pressed to obtain a high-loaded SePAN-based electrode for a sodium-selenium battery. Compared with the traditional coating process, the high-loaded SePAN-based positive electrode material for a sodium-selenium battery prepared by the present invention has a SePAN surface loading of up to 10-20 mg / cm 2 The surface loading of active Se can reach 6-12 mg / cm 2, not easy to pulverize, and the self-supporting electrode gets rid of the use of traditional current collectors, so the volume energy density of the battery is improved. The experimental results show that when the high-load SePAN-based material prepared by the preparation method provided by the present invention is used as the positive electrode of the sodium-selenium battery, the active material Se surface loading is 5.9 mg / cm at a current density of 0.1C (0.05C activated for two cycles). 2 The first discharge capacity is 532 mAh / g (theoretical capacity is 678 mAh / g), and after 40 cycles, it still has 495.1 mAh / g, with a capacity retention rate of about 93%. The SePAN material used in the present invention is simple to prepare, has a stable electrode structure, is green and clean, does not have the "shuttle effect" problem in sodium-selenium batteries, does not require conductive agents and binders, can achieve high active material loading, and provides possibilities for the development of high-energy sodium-selenium batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 This is a thermogravimetric test diagram of SePAN prepared in Example 1 of the present invention;

[0019] Figure 2 This is a SEM image of the SePAN / MXene / rGO aerogel prepared in Example 1 of the present invention;

[0020] Figure 3 HRTEM image of SePAN / MXene / rGO aerogel prepared in Example 1 of the present invention;

[0021] Figure 4 This is a digital image of the high-loaded SePAN / MXene / rGO electrode prepared in Example 1 of the present invention;

[0022] Figure 5 This is a charge and discharge curve diagram of the SePAN / MXene / rGO electrode prepared in Example 1 of the present invention;

[0023] Figure 6 This is the charge-discharge cycle diagram of the SePAN / MXene / rGO electrode prepared in Example 1 of the present invention;

[0024] Figure 7 This is a SEM image of the SePAN / MXene / rGO aerogel prepared in Example 2 of the present invention;

[0025] Figure 8 This is a charge-discharge curve diagram of the high-load SePAN / MXene / rGO electrode prepared in Example 2 of the present invention;

[0026] Fig. 9 This is the charge-discharge cycle diagram of the high-load SePAN / MXene / rGO electrode prepared in Example 2 of the present invention;

[0027] Fig.10 This is a charge-discharge cycle diagram of the high-load SePAN electrode prepared in Comparative Example 1 of the present invention; DETAILED DESCRIPTION

[0028] The technical solutions provided by the present invention are further explained clearly and completely below by means of specific embodiments, but they do not constitute a limitation to the present invention.

[0029] The present invention provides a method for preparing a high-load sodium-selenium battery SePAN-based positive electrode material, comprising the following steps:

[0030] (1) The prepared SePAN powder was mixed evenly with MXene solution, monolayer graphene oxide solution and reducing agent and then hydrothermally heated at low temperature to obtain a three-dimensional SePAN / MXene / rGO gel.

[0031] (2) The gel obtained in step (1) is freeze-dried to obtain SePAN / MXene / rGO aerogel, and the aerogel is cut and pressed into sheets to obtain a high-load SePAN-based positive electrode material.

[0032] In the present invention, unless otherwise specified, all preparation raw materials are commercially available products well known to those skilled in the art.

[0033] In the present invention, the MXene species is preferably Ti3C2T x , the MXene species is preferred because Ti3C2T x It is not easily oxidized and has relatively stable properties.

[0034] In the present invention, the MXene concentration is 1-5 mg / ml, and more preferably 2 mg / ml. The MXene concentration is preferably to maintain the gel morphology while allowing MXene, rGO and SePAN to be better dispersed evenly.

[0035] In the present invention, the ratio of selenium powder to polyacrylonitrile is 2:1-8:1. More preferably, it is 4:1. A high selenium ratio will result in residual selenium, and a low selenium content will result in a low active selenium content. In order to obtain SePAN without elemental selenium and with a high selenium content, a ratio of 4:1 is preferably selected.

[0036] In the present invention, the molecular weight of polyacrylonitrile is preferably 10,000-20,000, more preferably 15,000. A high molecular weight is not conducive to cyclization, while a low molecular weight will result in poor thermal stability of the cyclization product.

[0037] In the present invention, the tube furnace calcination temperature is preferably 400-600°C, more preferably 550°C. A lower calcination temperature will result in residual elemental selenium, and a higher temperature will result in a lower selenium content and a lower loading. 550°C is preferably selected to obtain SePAN without elemental selenium and with a high selenium content. The calcination time is preferably 1-10 hours, more preferably 5-7 hours.

[0038] In the present invention, the reducing agent preferably includes oxalic acid, ascorbic acid, citric acid, and more preferably oxalic acid; the reducing agents are all purchased from Aladdin Pharmaceutical Co., Ltd. In the present invention, the reducing agent can reduce graphene oxide to reduced graphene oxide in a low-temperature hydrothermal process, thereby improving the conductivity of the aerogel skeleton, and the addition of the reducing agent can slow down the oxidation of MXene.

[0039] In the present invention, the mass ratio of SePAN powder, graphene oxide and MXene is preferably 8:2:1-3:2:1, more preferably 8:2:1. The change in ratio leads to the change of the internal pore structure and the final loading of the aerogel. In order to obtain an aerogel with high active material loading and well-developed pores, a ratio of 8:2:1 is preferably selected.

[0040] In the present invention, the stirring time of the mixed dispersion of SePAN / MXene / rGO is preferably 0.5-12h, more preferably 2h; the ultrasonic time is preferably 0-2h, more preferably 1h; too long ultrasonic time will cause the MXene flakes to break and become smaller, and too short ultrasonic time will make it impossible to evenly disperse the graphene oxide.

[0041] In the present invention, the gel reduction process is carried out in an oven at a temperature of 60-120°C for 5-15 hours. More preferably, the reaction time is 10-14 hours and the reaction temperature is 70-100°C. Too long a time or too high a temperature will accelerate the oxidation of MXene. In the present invention, when the reduction reaction conditions are within the above range, it is more conducive to the reduction of graphene oxide and the cross-linking between graphene sheets and MXene sheets.

[0042] In the present invention, the preparation process of the gel is carried out in a closed cylindrical transparent glass bottle with a diameter of 2-6 cm.

[0043] In the process of preparing the reactants, the present invention relates to annealing, ultrasound, stirring and inert atmosphere protection processes. In the present invention, there is no special limitation on the annealing process, and a process well known to those skilled in the art can be used. In the present invention, there is no special limitation on the ultrasonic power and stirring speed, and the purpose is to mix the reactants evenly, and parameters well known to those skilled in the art can be used. After the gel preparation is completed, the present invention will also involve cooling and washing processes. In the present invention, there is no special limitation on the cooling process, and a process well known to those skilled in the art can be used. In the present invention, the washing process is preferably deionized water washing.

[0044] In the present invention, the reduction process is carried out under the protection of an inert atmosphere. The present invention has no particular limitation on the inert atmosphere, and an atmosphere familiar to those skilled in the art may be used. In the present invention, the gas of the inert atmosphere is preferably nitrogen, helium or argon. In the present invention, the inert atmosphere can prevent MXene from being oxidized during the heating reduction process.

[0045] In the present invention, the aerogel is preferably cut 0-5 times, more preferably 1-3 times, during the cutting process; the tableting pressure is preferably 5-20 MPa, more preferably 10-15 MPa. In the present invention, when the cutting times and pressure are within the above ranges, the electrode structure can be stabilized and a high active material loading can be achieved.

[0046] The present invention also provides a sodium-selenium battery SePAN-based positive electrode material prepared by the preparation method described in the above technical solution.

[0047] The present invention has no special limitation on the application method of the high-load SePAN-based positive electrode in the positive electrode material of the sodium-selenium battery. The application method of the carbon material well known to those skilled in the art as the positive electrode material of the sodium-selenium battery can be used.

[0048] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0049] Example 1

[0050] (1) Single-layer Ti3C2T was prepared by the classic lithium fluoride + concentrated hydrochloric acid etching method. x -MXene solution was prepared and diluted to 2 mg / ml. 4 g of selenium powder with a purity greater than 99.9% was mixed with polyacrylonitrile (Mw=15000) and placed in a tube furnace. The mixture was heated to 550°C at a rate of 5°C / min for 6 h. After the reaction, SePAN powder was obtained by natural annealing.

[0051] (2) Take 48 mg of SePAN powder and 3 ml of Ti3C2T x -MXene solution, 12 mg of commercial monolayer graphene oxide, 6 ml of deionized water and 100 mg of oxalic acid were added to a glass bottle, inert gas was introduced and sealed, ultrasonicated for 30 min, stirred for 2 h, and then placed in an oven and hydrothermaled at 70 ° C for 12 h. SePAN / MXene / rGO gel was obtained and washed with deionized water 5 times to remove the remaining oxalic acid.

[0052] (3) The gel obtained in (2) was placed in a freeze dryer and freeze-dried for 72 h to obtain a loose and porous SePAN / MXene / rGO aerogel; the aerogel was evenly cut once, pressed into sheets, and the sheets were cut to obtain a high-load sodium-selenium battery SePAN-based positive electrode material.

[0053] The Se content of the SePAN powder prepared in Example 1 was determined by thermogravimetric analysis, and the TGA graph was as follows: Figure 1 As shown. Figure 1 It can be seen that the content of active substance Se in SePAN is 40.2%.

[0054] The morphology of the SePAN / MXene / rGO aerogel prepared in Example 1 was characterized by scanning electron microscopy, and the SEM image was as follows: Figure 2 As shown. Figure 2 It can be seen that the SePAN spherical particles are uniformly loaded on the three-dimensional skeleton composed of cross-linked MXene and reduced graphene oxide sheets.

[0055] The SePAN / MXene / rGO aerogel prepared in Example 1 was studied using a high-resolution transmission electron microscope, and the HRTEM image of the SePAN / MXene / rGO aerogel prepared in Example 1 was obtained as shown in FIG. Figure 4 As shown. Figure 4 It can be seen that SePAN in the aerogel is mainly a disordered structure, reduced graphene oxide is a short-range ordered structure, and MXene has an obvious crystal structure, which also successfully illustrates the successful preparation of SePAN / MXene / rGO aerogel.

[0056] The pressed high-load SePAN-based positive electrode was weighed using an electronic balance to obtain the SePAN / MXene / rGO high-load electrode prepared in Example 1. The electrode diameter was 8 mm. The Se content was obtained from the reaction ratio and thermogravimetric analysis, and the surface loading of the active substance Se was calculated to be about 8 mg / cm 2 , close to commercial requirements.

[0057] Test Example 1

[0058] The pressed high-load SePAN / MXene / rGO electrode was cut into (8×8) mm 2 The electrode was placed in a vacuum oven and vacuum dried at 60°C for 10 hours, and then immediately transferred to a glove box for standby use. In an argon atmosphere, metallic sodium was used as the counter electrode, and 1M NaClO4 was dissolved in 1L of ethylene carbonate and diethyl carbonate solvent with a volume ratio of 1:1 as the electrolyte. A CR2025 button cell was assembled in an argon atmosphere.

[0059] The assembled CR2025 button battery was subjected to a charge and discharge performance test. The test conditions were: after two cycles of activation at a current density of 0.05C (1C = 678mA / g), a charge and discharge cycle test was performed at 0.1C; the discharge cut-off voltage was 0.5V, and the charge cut-off voltage was 3V.

[0060] Figure 5 The charge-discharge curves of the SePAN-based positive electrode material for sodium-selenium battery prepared in Example 1 at the 1st, 2nd and 30th cycles; Figure 5 It can be seen that the first discharge capacity of the SePAN-based positive electrode material of the sodium-selenium battery described in Example 1 activated at 0.05C is 1195.3 mAh / g, the discharge specific capacity at 0.1C is 532 mAh / g (theoretical specific capacity 678 mAh / g), and the reversible capacity at the 30th cycle is 487.4 mAh / g.

[0061] Figure 6 The charge and discharge cycle diagram of the SePAN-based positive electrode material of the sodium-selenium battery prepared in Example 1 at a current density of 0.1C; Figure 6 It can be seen that the SePAN-based positive electrode material of the sodium-selenium battery described in Example 1 has a 2 At an active material loading of , the first discharge at 0.1C is 532mAh / g, and the capacity is 495.1mAh / g after 40 cycles. The capacity retention rate after 40 cycles is 93%, indicating that the material has both cycle stability and large loading capacity advantages.

[0062] Example 2

[0063] (1) Single-layer Ti3C2T was prepared by the classic lithium fluoride + concentrated hydrochloric acid etching method. x -MXene solution was prepared and diluted to 2 mg / ml. 4 g of selenium powder with a purity greater than 99.9% was mixed with polyacrylonitrile (Mw=15000) and placed in a tube furnace. The mixture was heated to 550°C at a rate of 5°C / min for 6 h. After the reaction, SePAN powder was obtained by natural annealing.

[0064] (2) Take 36 mg of SePAN powder and 6 ml of Ti3C2T x -MXene solution, 24 mg of commercial monolayer graphene oxide, and 100 mg of oxalic acid were placed in a glass bottle, sealed with inert gas, ultrasonicated for 30 min, stirred for 3 h, and then placed in an oven for low-temperature hydrothermal treatment at 70 ° C for 12 h. SePAN / MXene / rGO gel was obtained and washed with deionized water 5 times to remove the remaining oxalic acid.

[0065] (3) The gel obtained in (2) was placed in a freeze dryer and freeze-dried for 72 h to obtain SePAN / MXene / rGO aerogel; the aerogel was evenly cut once, pressed into sheets, and the sheets were cut to obtain SePAN-based positive electrode materials for high-load sodium-selenium batteries.

[0066] Measurement example 2

[0067] The pressed high-load SePAN / MXene / rGO electrode was cut into (8×8) mm 2 The electrode was placed in a vacuum oven and vacuum dried at 60°C for 10 hours, and then immediately transferred to a glove box for standby use. In an argon atmosphere, metallic sodium was used as the counter electrode, and 1M NaClO4 was dissolved in 1L of ethylene carbonate and diethyl carbonate solvent with a volume ratio of 1:1 as the electrolyte. A CR2025 button cell was assembled in an argon atmosphere.

[0068] The assembled CR2025 button battery was subjected to a charge and discharge performance test. The test conditions were: after two cycles of activation at a current density of 0.05C (1C = 678mA / g), a charge and discharge cycle test was performed at 0.1C; the discharge cut-off voltage was 0.5V, and the charge cut-off voltage was 3V.

[0069] Figure 8 The charge-discharge curves of the sodium-selenium battery SePAN-based positive electrode material prepared in Example 2 at a current density of 0.05C (1C = 678mA / g) at the 1st, 2nd and 30th cycles; Figure 8 It can be seen that the active Se surface loading of the SePAN-based positive electrode material for the sodium-selenium battery described in Example 2 is 5 mg / cm at a current density of 0.05C. 2 Under the conditions, the first discharge specific capacity is 782.2mAh / g (theoretical specific capacity 678mAh / g), the discharge platform is 1.35V, and the charging platform is 1.65V, which is a typical capacity platform for sodium-selenium batteries. The discharge capacity in the second cycle is 350mAh / g, and the discharge capacity in the 30th cycle is 361mAh / g.

[0070] Fig. 9 The charge-discharge cycle diagram of the first 30 cycles of the SePAN-based positive electrode material for the sodium-selenium battery prepared in Example 2 of the present invention at a current density of 0.05C (1C = 678mA / g) is shown in FIG. Fig. 9 It can be seen that even at 5 mg / cm 2 Under the loading capacity, the cycle stability of the prepared electrode is still very good, stable at around 350mAh / g. Although the coulombic efficiency in the first cycle is not high, there is almost no capacity attenuation in subsequent cycles.

[0071] Comparative Example 1

[0072] 4 g of selenium powder with a purity greater than 99.9% was mixed evenly with polyacrylonitrile (Mw=15000) and placed in a tube furnace. The mixture was heated to 550°C at a heating rate of 5°C / min for 6 h. After the reaction, the mixture was naturally annealed to obtain SePAN powder.

[0073] Comparative test example 1

[0074] The SePAN powder prepared in Example 1 was mixed with Super P and sodium polyacrylate in a ratio of 8:1:1, and water was used as a dispersant. The mixture was evenly mixed in a homogenizing tank to form a slurry. The slurry was then scraped onto the current collector copper foil, dried in an oven, and cut into (8×8) mm 2 The electrode was placed in a vacuum oven and vacuum dried at 60°C for 10 hours, and then immediately transferred to a glove box for standby use. In an argon atmosphere, sodium metal was used as the counter electrode, and 1 mol of NaClO4 was dissolved in 1L of ethylene carbonate and diethyl carbonate solution with a volume ratio of 1:1 was used as the electrolyte to assemble a CR2025 button cell.

[0075] The assembled CR2025 button battery was subjected to a charge and discharge performance test. The test conditions were: after two cycles of activation at a current density of 0.05C (1C = 678mA / g), a charge and discharge cycle test was performed at 0.1C; the discharge cut-off voltage was 0.5V, and the charge cut-off voltage was 3V.

[0076] Fig.10 This is the positive electrode of a sodium-selenium battery prepared by conventional coating technology using pure SePAN positive electrode material in comparative example 1 of the present invention. Under the condition of a current density of 0.05C (1C = 678mA / g), the charge-discharge cycle diagram for the first 40 cycles is shown in the figure. Fig.10 It can be seen that at 6.5 mg / cm 2 Under the loading condition, the prepared large-load electrode has poor cycle stability. This may be because the traditional coating process causes the electrode structure to be too dense, the utilization rate of active materials is low, and the electrode piece is powdered, resulting in insufficient cycle stability.

[0077] It can be seen from the above experimental results that the high-load SePAN-based positive electrode material prepared by the preparation method provided by the present invention has a high capacity retention rate and energy density when used as the positive electrode of a sodium-selenium battery.

[0078] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a high-load sodium-selenium battery selenized polyacrylonitrile-based positive electrode material, the steps of which are as follows: (1) A single-layer MXene suspension is obtained by a typical lithium fluoride + concentrated hydrochloric acid etching method; (2) mixing selenium powder and polyacrylonitrile and sintering them to obtain selenized polyacrylonitrile (SePAN) powder with uniform particles; (3) mixing the above SePAN powder with commercial graphene oxide, MXene suspension, and a reducing agent, stirring the mixture evenly by ultrasonication, introducing an inert gas, heating, and washing to obtain a SePAN / MXene / rGO gel, and freeze-drying the obtained gel to obtain a SePAN / MXene / rGO aerogel; (4) The aerogel obtained above is cut and pressed into sheets to obtain the high-load SePAN-based positive electrode material for sodium-selenium batteries.

2. A method for preparing a high-loaded SePAN-based positive electrode material for sodium-selenium batteries according to claim 1, characterized in that: The MXene in step (1) is Ti3C2T x or Ti2CT x , concentration is 1-5mg / ml.

3. A method for preparing a high-loaded SePAN-based positive electrode material for sodium-selenium batteries according to claim 1, characterized in that: In the step (2), the ratio of selenium powder to polyacrylonitrile is 2:1-8:1, the sintering temperature is 400-600°C, the heating rate is 2-10°C / min, and the insulation time is 1h-10h.

4. A method for preparing a high-loaded SePAN-based positive electrode material for sodium-selenium batteries according to claim 1, characterized in that: In the step (2), the purity of selenium powder should be greater than 99.9%, and the molecular weight of polyacrylonitrile should be between 10,000 and 20,000.

5. A method for preparing a high-loaded SePAN-based positive electrode material for sodium-selenium batteries according to claim 1, characterized in that: In the step (3), the mass ratio of SePAN powder, graphene oxide and MXene is 8:2:1-3:2:1, the stirring time is 0.5-12h, the ultrasonic time is 0-2h, and the inert gas introduced is one of argon, nitrogen and helium.

6. A method for preparing a high-load SePAN-based positive electrode material for sodium-selenium batteries according to claim 1, characterized in that: The reducing agent added in step (3) includes one of oxalic acid, ascorbic acid and citric acid, and the amount of the reducing agent added is 50-150 mg.

7. A method for preparing a high-loaded SePAN-based positive electrode material for sodium-selenium batteries according to claim 1, characterized in that: The heating temperature in step (3) is 60-120° C., and deionized water should be used for washing, with the washing times being 4-8 times and the washing time being 5-24 hours.

8. A method for preparing a high-loaded SePAN-based positive electrode material for sodium-selenium batteries according to claim 1, characterized in that: The reaction vessel in step (3) should be a cylindrical glass bottle with a diameter of 2-6 cm.

9. A method for preparing a high-load SePAN-based positive electrode material for sodium-selenium batteries according to claim 1, characterized in that: In the step (4), the aerogel needs to be evenly cut into different sections after drying in order to control the loading range, the cutting is 0-5 times, the tableting pressure is 5-20 MPa, and the holding time is 1-10 s.

10. The highly loaded SePAN-based material according to any one of claims 1 to 9, characterized in that: The target material is used as a positive electrode material for a sodium-selenium battery.