Phosphogypsum concrete as well as preparation method and application thereof
Through the combination of modified regenerated aggregate and a mixed binder of various resins, the insufficient strength and durability of phosphogypsum concrete are solved, and its water permeability and mechanical properties are improved. It is suitable for high-speed slope protection and dam slope protection.
Patent Information
- Application Number
- CN202411250485.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-12-03
AI Technical Summary
Phosphate gypsum concrete is prone to cracks, insufficient strength, poor durability, poor connection stability and drainage problems during use, resulting in the impact of structural stability and service life.
Use modified regenerated aggregates, mixed binders of various resins and cement with specific ratios and other raw materials, soak the regenerated aggregates through the modified liquid A and liquid B to form a uniform three-dimensional pore structure, which improves water permeability and mechanical strength. And improve performance through vibration press molding and kiln maintenance.
It significantly improves the water permeability, compressive strength and fold resistance of phosphogypsum concrete, ensuring that high mechanical properties are maintained after freeze-thaw cycle, and is suitable for high-speed slope protection and dam slope protection.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of concrete, and in particular relates to phosphogypsum concrete, a preparation method and application thereof. Background Art
[0002] Phosphogypsum concrete is a common hexagonal block precast concrete product, mainly used in ground paving, slope protection, soil and water conservation and other projects. Their design is based on the hexagonal geometry, which can provide good structural stability and space efficiency because the hexagons can be seamlessly spliced without gaps.
[0003] There are some technical problems that may affect the performance and service life of phosphogypsum concrete during its use. (1) Cracks: Phosphogypsum concrete may develop cracks during the production process or after a period of use. This may be caused by improper proportions of concrete mixtures, insufficient curing or environmental factors (such as temperature changes). (2) Insufficient strength: If the concrete mix is not appropriate or the quality of the materials used is poor, the compressive strength of the hexagonal blocks may not meet the design requirements. (3) Durability issues: If the hexagonal blocks are exposed to harsh environments, such as marine environments with high salinity or areas with frequent freeze-thaw cycles, they may suffer from corrosion, peeling and other problems. (4) Connection stability: The connection stability between the hexagonal blocks is crucial to the safety of the overall structure. If the connection is improper, it may lead to a decrease in the stability of the entire structure. (5) Construction quality issues: Improper operations during construction, such as uneven placement and insufficient mortar filling, may cause structural problems. (6) Drainage problems: If the hexagonal blocks are used for slope protection or riverbed paving, improper drainage design may cause water accumulation, which in turn affects the stability and service life of the structure.
[0004] Phosphogypsum concrete is generally used for high-speed slope protection and dam slope protection. Traditional phosphogypsum concrete is made without adding fine aggregate or only adding a small amount of fine aggregate, and pores are naturally formed by coarse aggregate and cement. In actual use, due to the poor uniformity of pore formation, the drainage effect of the blocks is poor, water is easily accumulated, and its mechanical properties are not ideal. In the prior art, hectorite is added to concrete. Hectorite is added to water and can expand rapidly to form a hydrogel with good thixotropy, dispersibility, suspension and thickening properties. After drying, connected three-dimensional pores are formed on the surface of the concrete, which can absorb water and seep water, and has good water permeability and water retention. However, the strength grade of the phosphogypsum concrete prepared by this method cannot meet the market requirements.
[0005] Therefore, there is an urgent need for a phosphogypsum concrete with good water permeability and water retention and high strength grade. Summary of the invention
[0006] The purpose of the present invention is to provide phosphogypsum concrete, a preparation method and application thereof.
[0007] In order to achieve the above-mentioned purpose, the present invention provides the following technical scheme: a phosphogypsum concrete, comprising the following raw materials in parts by weight: 250-300 parts of modified recycled aggregate, 500-570 parts of crushed stone, 100-140 parts of natural rock, 200-260 parts of pebbles, 380-400 parts of cement, 500-550 parts of natural sand, 210-260 parts of blast furnace slag, 60-120 parts of silica fume, 10-50 parts of fly ash, 40-90 parts of mullite, 300-350 parts of binder, 150-170 parts of curing agent and 500-580 parts of water.
[0008] Furthermore, the preparation method of the modified recycled aggregate is: (1) Crushing and screening the waste concrete to remove impurities, improve the aggregate shape, and remove the hardened cement stone attached to the surface of the aggregate to obtain recycled aggregate; (2) The recycled aggregate is completely immersed in the modified liquid A for 2-3 days, the solid and liquid are separated, and the water is naturally dried to obtain the silane-modified recycled aggregate; (3) The recycled aggregate is completely immersed in the modified liquid B for 2-3 days, the solid and liquid are separated, and the water is naturally dried to obtain the modified recycled aggregate.
[0009] Further, γ-mercaptopropyltrimethoxysilane and water were mixed at a volume ratio of 1:(8-10) to prepare a modified liquid A.
[0010] Furthermore, hexadecyltrimethylammonium bromide and water are mixed in a volume ratio of 1:(12-15) to prepare a modified liquid B.
[0011] Furthermore, the particle size of the recycled aggregate is 5-20 mm, of which particles with a particle size of less than 10 mm account for 30-35%, particles with a particle size of ≥10 mm and less than 15 mm account for 15-20%, and the remainder are particles with a particle size of ≥15 mm.
[0012] When preparing phosphogypsum concrete, using recycled aggregate as raw material is conducive to the reuse of resources, but the pores formed by using recycled aggregate have poor uniformity, resulting in poor drainage effect of blocks. The present invention can improve the water permeability coefficient of phosphogypsum concrete by adding modified recycled aggregate and cooperating with the raw materials. Because γ-mercaptopropyltrimethoxysilane penetrates the micropores of recycled aggregate, siloxane crosslinking is formed on the surface of recycled aggregate and coated on the surface, hexadecyltrimethylammonium bromide is adsorbed on the surface of recycled aggregate pores, and in the mixing process with other components, it plays a certain dispersing and lubricating role, which helps to improve the interaction between aggregate and cement paste, improve the fluidity of the mixture, and then improve the uniformity of mixing between raw materials, so that the concrete surface forms connected three-dimensional pores, and has good water permeability. At the same time, the thiol group has hydrophobicity, and hexadecyltrimethylammonium bromide contains a long-chain hydrophobic alkyl chain, which can reduce the hydrophilicity of aggregate, effectively prevent water from entering the interior of aggregate, and reduce the water absorption of foam concrete waste.
[0013] Furthermore, the cement is ordinary Portland cement with a strength grade of 42.5 MPa.
[0014] Furthermore, the binder is selected from one or more of silicone resin, epoxy resin E-51, and modified epoxy resin.
[0015] Furthermore, the preparation method of the modified epoxy resin is: 16-18 parts by weight of polyether diol, 5 parts by weight of diphenylmethane diisocyanate, and 0.15-0.02 parts by weight of an organic bismuth catalyst are mixed, heated to 70-75°C, reacted for 3-5 hours, cooled to room temperature, 1-3 parts by weight of propylene glycol and 3-5 parts by weight of trimethylolpropane are added and stirred evenly to obtain a polyurethane prepolymer, and 100 parts by weight of epoxy resin E-44 are continued to be added, reacted for 3-5 hours, and the epoxy resin is modified.
[0016] Furthermore, the weight average molecular weight of the polyether diol is 1000-3000.
[0017] Furthermore, the organic silicone resin has an epoxy value of 0.03-0.08 and is purchased from Sanmu Group with a brand name of SMH-30.
[0018] Furthermore, the curing agent is CYDHD-593.
[0019] Furthermore, the binder is a mixture of silicone resin, epoxy resin E-51, and modified epoxy resin in a mass ratio of 1: (1.2-1.5): (0.6-0.8).
[0020] The present invention selects a variety of different raw materials such as modified recycled aggregates, natural sand, silica fume, etc., and can improve the permeability of phosphogypsum concrete through compounding. However, the compressive strength and folding strength of phosphogypsum concrete under certain conditions are not ideal. The present invention attempts to add conventional epoxy resin to the concrete system, but the improvement effect is not ideal. The present invention can improve the compressive strength and folding strength of phosphogypsum concrete by adding a binder prepared by mixing multiple resins into the raw materials. The binder used in the present invention can make the point contact between the raw materials more continuous, thereby enhancing the mechanical strength of the concrete. And when the binder is mixed with silicone resin, epoxy resin E-51, and modified epoxy resin in a specific ratio, the concrete hexagon can still maintain a high mechanical strength after multiple freeze-thaw cycles.
[0021] The present invention also provides a method for preparing the phosphogypsum concrete. The method for preparing the phosphogypsum concrete comprises the following steps: putting the raw materials into a mixer and stirring them evenly, pouring them into a mold, performing vibration pressing and molding, demolding after molding, and sending the raw materials to a curing kiln for curing.
[0022] Furthermore, the curing conditions are: temperature of 13-15°C, relative humidity of 97±1%, and curing time of 28 days.
[0023] The invention also provides application of the phosphogypsum concrete.
[0024] Compared with the prior art, the advantages and beneficial effects of the present invention are: 1. The present invention compounds a variety of raw materials to work synergistically, so that the prepared phosphogypsum concrete has good water permeability, high compressive strength and high flexural strength, and can be used for high-speed slope protection and dam slope protection.
[0025] 2. The present invention can improve the water permeability of phosphogypsum concrete by adding modified recycled aggregates and cooperating with the raw materials. At the same time, the thiol group is hydrophobic, and hexadecyltrimethylammonium bromide contains a long-chain hydrophobic alkyl chain, which can reduce the hydrophilicity of the aggregate, effectively prevent water from entering the interior of the aggregate, and reduce the water absorption of the foam concrete waste.
[0026] 3. The present invention can improve the compressive strength and folding strength of phosphogypsum concrete by adding a plurality of resins to the raw materials. The binder used in the present invention can make the point contact between the raw materials more continuous, thereby enhancing the mechanical strength of the concrete. And when the binder is mixed with silicone resin, epoxy resin E-51 and modified epoxy resin in a specific ratio, the concrete hexagon can still maintain a high mechanical strength after multiple freeze-thaw cycles. DETAILED DESCRIPTION
[0027] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0028] Epoxy resin E-51 and epoxy resin E-44 were purchased from Shandong Pinshang New Materials Co., Ltd.
[0029] Example 1 The present embodiment provides a phosphogypsum concrete, comprising the following raw materials in parts by weight: 280 parts of modified recycled aggregate, 550 parts of crushed stone, 120 parts of natural rock, 240 parts of pebbles, 390 parts of cement, 530 parts of natural sand, 230 parts of blast furnace slag, 100 parts of silica fume, 30 parts of fly ash, 60 parts of mullite, 310 parts of binder, 160 parts of curing agent, and 540 parts of water.
[0030] The preparation method of modified recycled aggregate is as follows: (1) Crushing and screening the waste concrete to remove impurities, improve the aggregate shape, and remove the hardened cement stone attached to the surface of the aggregate to obtain recycled aggregate; (2) γ-mercaptopropyltrimethoxysilane and water are mixed in a volume ratio of 1:9 to prepare a modified liquid A. The recycled aggregate is completely immersed in the modified liquid A for 2 days, the solid and liquid are separated, and the water is naturally dried to obtain silane-modified recycled aggregate; (3) Hexadecyltrimethylammonium bromide and water were mixed in a volume ratio of 1:13 to prepare a modified liquid B. The recycled aggregate was completely immersed in the modified liquid B for 3 days, the solid and liquid were separated, and the water was naturally dried to obtain a modified recycled aggregate.
[0031] The particle size of the recycled aggregate is 5-20 mm, of which particles with a particle size of less than 10 mm account for 32%, particles with a particle size of ≥10 mm and less than 15 mm account for 17%, and the remainder are particles with a particle size of ≥15 mm.
[0032] The cement is ordinary Portland cement with a strength grade of 42.5MPa.
[0033] The adhesive is a mixture of silicone resin, epoxy resin E-51 and modified epoxy resin in a mass ratio of 1:1.4:0.7.
[0034] The preparation method of the modified epoxy resin is as follows: 17 parts by weight of polyether diol, 5 parts by weight of diphenylmethane diisocyanate, and 0.17 parts by weight of an organic bismuth catalyst are mixed, heated to 72°C, reacted for 4 hours, cooled to room temperature, 2 parts by weight of propylene glycol and 4 parts by weight of trimethylolpropane are added and stirred evenly to obtain a polyurethane prepolymer, and 100 parts by weight of epoxy resin E-44 are continuously added and reacted for 4 hours to obtain a modified epoxy resin.
[0035] The weight average molecular weight of the polyether diol is 1000-3000.
[0036] Organic silicon resin, epoxy value 0.03-0.08. Purchased from Sanmu Group, brand: SMH-30.
[0037] The curing agent is CYDHD-593. Brand: Baling Petrochemical.
[0038] The preparation method of phosphogypsum concrete is as follows: put the raw materials into a mixer and mix them evenly, pour them into a mold, vibrate and press them into shape, demold them after shaping, and send them to a curing kiln for curing. The curing conditions are: temperature is 14°C, relative humidity is 97±1%, and curing time is 28 days.
[0039] Example 2 The present embodiment provides a phosphogypsum concrete, comprising the following raw materials in parts by weight: 250 parts of modified recycled aggregate, 500 parts of crushed stone, 100 parts of natural rock, 200 parts of pebbles, 380 parts of cement, 500 parts of natural sand, 210 parts of blast furnace slag, 60 parts of silica fume, 10 parts of fly ash, 40 parts of mullite, 300 parts of binder, 150 parts of curing agent, and 500 parts of water.
[0040] The preparation method of modified recycled aggregate is: (1) Crushing and screening the waste concrete to remove impurities, improve the aggregate shape, and remove the hardened cement stone attached to the surface of the aggregate to obtain recycled aggregate; (2) γ-mercaptopropyltrimethoxysilane and water are mixed in a volume ratio of 1:8 to prepare a modified liquid A. The recycled aggregate is completely immersed in the modified liquid A for 2 days, the solid and liquid are separated, and the water is naturally dried to obtain silane-modified recycled aggregate; (3) Hexadecyltrimethylammonium bromide and water were mixed in a volume ratio of 1:12 to prepare a modified liquid B. The recycled aggregate was completely immersed in the modified liquid B for 2 days, the solid and liquid were separated, and the water was naturally dried to obtain a modified recycled aggregate.
[0041] The particle size of the recycled aggregate is 5-20 mm, of which particles with a particle size of less than 10 mm account for 30%, particles with a particle size of ≥10 mm and less than 15 mm account for 15%, and the remainder are particles with a particle size of ≥15 mm.
[0042] The cement is ordinary Portland cement with a strength grade of 42.5MPa.
[0043] The adhesive is a mixture of silicone resin, epoxy resin E-51 and modified epoxy resin in a mass ratio of 1:1.2:0.6.
[0044] The preparation method of the modified epoxy resin is as follows: 16 parts by weight of polyether diol, 5 parts by weight of diphenylmethane diisocyanate, and 0.15 parts by weight of an organic bismuth catalyst are mixed, heated to 70°C, reacted for 3 hours, cooled to room temperature, 1 part by weight of propylene glycol and 3 parts by weight of trimethylolpropane are added and stirred evenly to obtain a polyurethane prepolymer, and 100 parts by weight of epoxy resin E-44 are continuously added and reacted for 3 hours to obtain a modified epoxy resin.
[0045] The weight average molecular weight of the polyether diol is 1000-3000.
[0046] Organic silicon resin, epoxy value 0.03-0.08. Purchased from Sanmu Group, brand: SMH-30.
[0047] The curing agent is CYDHD-593. Brand: Baling Petrochemical.
[0048] The preparation method of phosphogypsum concrete is as follows: put the raw materials into a mixer and mix them evenly, pour them into a mold, vibrate and press them into shape, demold them after shaping, and send them to a curing kiln for curing. The curing conditions are: temperature is 13°C, relative humidity is 97±1%, and curing time is 28 days.
[0049] Example 3 The present embodiment provides a phosphogypsum concrete, comprising the following raw materials in parts by weight: 300 parts of modified recycled aggregate, 570 parts of crushed stone, 140 parts of natural rock, 260 parts of pebbles, 400 parts of cement, 550 parts of natural sand, 260 parts of blast furnace slag, 120 parts of silica fume, 50 parts of fly ash, 90 parts of mullite, 350 parts of binder, 170 parts of curing agent, and 580 parts of water.
[0050] The preparation method of modified recycled aggregate is as follows: (1) Crushing and screening the waste concrete to remove impurities, improve the aggregate shape, and remove the hardened cement stone attached to the surface of the aggregate to obtain recycled aggregate; (2) γ-mercaptopropyltrimethoxysilane and water are mixed in a volume ratio of 1:10 to prepare a modified liquid A. The recycled aggregate is completely immersed in the modified liquid A for 3 days, the solid and liquid are separated, and the water is naturally dried to obtain silane-modified recycled aggregate; (3) Hexadecyltrimethylammonium bromide and water were mixed in a volume ratio of 1:15 to prepare a modified liquid B. The recycled aggregate was completely immersed in the modified liquid B for 3 days, the solid and liquid were separated, and the water was naturally dried to obtain a modified recycled aggregate.
[0051] The particle size of the recycled aggregate is 5-20 mm, of which particles with a particle size of less than 10 mm account for 35%, particles with a particle size of ≥10 mm and less than 15 mm account for 20%, and the remainder are particles with a particle size of ≥15 mm.
[0052] The cement is ordinary Portland cement with a strength grade of 42.5MPa.
[0053] The adhesive is a mixture of silicone resin, epoxy resin E-51 and modified epoxy resin in a mass ratio of 1:1.5:0.8.
[0054] The preparation method of the modified epoxy resin is as follows: 18 parts by weight of polyether diol, 5 parts by weight of diphenylmethane diisocyanate, and 0.02 parts by weight of an organic bismuth catalyst are mixed, heated to 75°C, reacted for 5 hours, cooled to room temperature, 3 parts by weight of propylene glycol and 5 parts by weight of trimethylolpropane are added and stirred evenly to obtain a polyurethane prepolymer, and 100 parts by weight of epoxy resin E-44 are continuously added and reacted for 5 hours to obtain a modified epoxy resin.
[0055] The weight average molecular weight of the polyether diol is 1000-3000.
[0056] Organic silicon resin, epoxy value 0.03-0.08. Purchased from Sanmu Group, brand: SMH-30.
[0057] The curing agent is CYDHD-593. Brand: Baling Petrochemical.
[0058] The preparation method of phosphogypsum concrete is as follows: put the raw materials into a mixer and mix them evenly, pour them into a mold, vibrate and press them into shape, demold them after shaping, and send them to a curing kiln for curing. The curing conditions are: temperature is 15°C, relative humidity is 97±1%, and curing time is 28 days.
[0059] Comparative Example 1 The difference between this comparative example and Example 1 is: a phosphogypsum concrete, comprising the following raw materials in parts by weight: 830 parts of crushed stone, 120 parts of natural rock, 240 parts of pebbles, 390 parts of cement, 530 parts of natural sand, 230 parts of blast furnace slag, 100 parts of silica fume, 30 parts of fly ash, 60 parts of mullite, 310 parts of binder, 160 parts of curing agent, and 540 parts of water.
[0060] Comparative Example 2 The difference between this comparative example and Example 1 is: a phosphogypsum concrete, comprising the following raw materials in parts by weight: 470 parts of modified recycled aggregate, 550 parts of crushed stone, 120 parts of natural rock, 240 parts of pebbles, 390 parts of cement, 530 parts of natural sand, 230 parts of blast furnace slag, 310 parts of binder, 160 parts of curing agent, and 540 parts of water.
[0061] Comparative Example 3 The difference between this comparative example and Example 1 is that the preparation method of the modified recycled aggregate is: (1) Crushing and screening the waste concrete to remove impurities, improve the aggregate shape, and remove the hardened cement stone attached to the surface of the aggregate to obtain recycled aggregate; (2) γ-mercaptopropyltrimethoxysilane and water were mixed in a volume ratio of 1:9 to prepare a modified liquid A. The recycled aggregate was completely immersed in the modified liquid A for 5 days, the solid and liquid were separated, and the water was naturally dried to obtain a modified recycled aggregate.
[0062] Comparative Example 4 The difference between this comparative example and Example 1 is that the particle size of the recycled aggregate is 5-20 mm, of which particles with a particle size of <10 mm account for 17%, particles with a particle size of ≥10 mm and less than 15 mm account for 50%, and the remainder are particles with a particle size of ≥15 mm.
[0063] Comparative Example 5 The difference between this comparative example and Example 1 is that the epoxy resin E-51 is replaced by the epoxy resin E-44.
[0064] Comparative Example 6 The difference between this comparative example and Example 1 is that the organic silicon resin is an epoxy-modified organic silicon resin with an epoxy value of 0.06-0.16, purchased from Sanmu Group, brand: SMH-60.
[0065] Comparative Example 7 The difference between this comparative example and Example 1 is that the binder is a mixture of silicone resin, epoxy resin E-51 and modified epoxy resin in a mass ratio of 1:1:1.
[0066] Comparative Example 8 The difference between this comparative example and Example 1 is that the binder is epoxy resin E-51.
[0067] Performance Testing The performance tests were carried out on the phosphogypsum concrete of Examples 1-3 and Comparative Examples 1-8.
[0068] The testing basis for strength grade MU7.5 and water absorption rate is "Ordinary Concrete Small Hollow Block Plus B / T8239-2014" and "Building Structure Load Standardization B50009-2012" respectively. The testing basis for water permeability is "JC / T945-2005". The results are shown in Table 1.
[0069] Table 1 Performance test results
[0070] It can be seen from the above performance test results that the compressive strength, flexural strength, water absorption and water permeability of the phosphogypsum concrete of Examples 1-3 are high, especially the comprehensive performance of Example 1 is the most outstanding, which is mainly due to the synergistic effect of the compounding of multiple raw materials.
[0071] The comparative examples, however, were significantly inferior to the examples in the corresponding performance tests because they did not adopt the necessary technical solutions. In comparative examples 1-2, the raw material ratio was changed, and it can be seen that the water permeability effect decreased, proving that the raw material ratio scheme has an important influence on the water permeability effect. Comparative examples 3-4 did not use the modified recycled aggregate scheme, and the results showed that the water permeability effect decreased and the water absorption rate increased. Comparative examples 5-8 had a change in the binder, and the compressive strength and flexural strength decreased. The above experimental results further prove the importance of the technical solution defined in the present invention for its technical effect.
[0072] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A phosphogypsum concrete, characterized in that: The raw materials include the following parts by weight: 250-300 parts of modified recycled aggregate, 500-570 parts of crushed stone, 100-140 parts of natural rock, 200-260 parts of pebbles, 380-400 parts of cement, 500-550 parts of natural sand, 210-260 parts of blast furnace slag, 60-120 parts of silica fume, 10-50 parts of fly ash, 40-90 parts of mullite, 300-350 parts of binder, 150-170 parts of curing agent and 500-580 parts of water; The preparation method of modified recycled aggregate is: (1) Crushing and screening the waste concrete to remove impurities, improve the aggregate shape, and remove the hardened cement stone attached to the surface of the aggregate to obtain recycled aggregate; (2) The recycled aggregate is completely immersed in the modified liquid A for 2-3 days, the solid and liquid are separated, and the water is naturally dried to obtain the silane-modified recycled aggregate; (3) The recycled aggregate is completely immersed in the modified liquid B for 2-3 days, the solid and liquid are separated, and the water is naturally dried to obtain the modified recycled aggregate.
2. The phosphogypsum concrete according to claim 1, characterized in that: γ-mercaptopropyltrimethoxysilane and water were mixed in a volume ratio of 1:(8-10) to prepare a modified liquid A.
3. The phosphogypsum concrete according to claim 1, characterized in that: The modified liquid B was prepared by mixing hexadecyltrimethylammonium bromide and water in a volume ratio of 1:(12-15).
4. The phosphogypsum concrete according to claim 1, characterized in that: The particle size of the recycled aggregate is 5-20 mm, of which particles with a particle size of less than 10 mm account for 30-35%, particles with a particle size of ≥10 mm and less than 15 mm account for 15-20%, and the remainder are particles with a particle size of ≥15 mm.
5. The phosphogypsum concrete according to claim 1, characterized in that: The cement is ordinary Portland cement with a strength grade of 42.5MPa.
6. The phosphogypsum concrete according to claim 1, characterized in that: The binder is selected from one or more of silicone resin, epoxy resin E-51, and modified epoxy resin; the preparation method of the modified epoxy resin is: 16-18 parts by weight of polyether diol, 5 parts by weight of diphenylmethane diisocyanate, and 0.15-0.02 parts by weight of an organic bismuth catalyst are mixed, heated to 70-75°C, reacted for 3-5 hours, cooled to room temperature, 1-3 parts by weight of propylene glycol and 3-5 parts by weight of trimethylolpropane are added and stirred evenly to obtain a polyurethane prepolymer, and 100 parts by weight of epoxy resin E-44 are continuously added, reacted for 3-5 hours, and the modified epoxy resin is obtained.
7. The phosphogypsum concrete according to claim 6, characterized in that: Silicone resin, epoxy value 0.03-0.
08.
8. The phosphogypsum concrete according to claim 6, characterized in that: The binder is a mixture of silicone resin, epoxy resin E-51 and modified epoxy resin in a mass ratio of 1: (1.2-1.5): (0.6-0.8).
9. A method for preparing phosphogypsum concrete according to any one of claims 1 to 8, characterized in that: The preparation method of phosphogypsum concrete is as follows: put the raw materials into a mixer and mix them evenly, pour them into a mold, vibrate and press them into shape, demould them after shaping, and send them to a curing kiln for curing.
10. Use of the phosphogypsum concrete according to any one of claims 1 to 8.