Grouting material as well as preparation method and application thereof

The grouting material with adjustable setting time and high strength, using specific component ratios, addresses the limitations of traditional grouting materials, ensuring effective water blocking and reinforcement in coal mining.

CN119059779APending Publication Date: 2024-12-03CHINA ENERGY INVESTMENT CORP LTD +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202310648222.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-06-02
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Existing grouting materials face issues with adjustable setting time and high strength requirements, as well as environmental pollution and high costs, limiting their application in coal mining safety.

Method used

A grouting material comprising components A and B, where component A includes cement, fly ash, and additives like a water reducer and retarder, and component B includes an accelerating setting agent, with a controlled mass ratio to adjust setting time and enhance strength.

Benefits of technology

The grouting material achieves adjustable setting times from seconds to minutes, high early and final strength, and improved fluidity, addressing volume ratio changes during grouting and enhancing grouting effectiveness for water blocking and reinforcement.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119059779A_ABST
    Figure CN119059779A_ABST
Patent Text Reader

Abstract

The invention provides a grouting material which comprises a component A and a component B. The component A comprises cement, fly ash, a water reducing agent, a retarder, a moistening agent, a defoaming agent, redispersible latex powder, a thickening agent and water. The component B comprises an accelerator, a moistening agent, a thickening agent, a defoaming agent, a water reducing agent and water; the mass ratio of the component A to the component B is 1: (0.0017-0.067). The setting time of the grouting material is adjusted in real time by adjusting the dosage of the component B, and the grouting material meets the requirements of different grouting conditions in current industrial practice. Meanwhile, the grouting material provided by the invention is high in early strength and final strength after being coagulated, and has a good application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of grouting materials, and in particular to a grouting material and a preparation method and application thereof. Background Art

[0002] my country ranks third in the world in coal reserves and first in production. Coal occupies an important position in my country's energy structure. There are many safety issues in the process of coal resource mining. The first is the water hazard problem. Once a coal mine water hazard accident occurs, rescue is difficult, time-consuming and expensive. The second is the safety of the surrounding rock. The stress of the tunnel surrounding rock causes the tunnel surrounding rock to be broken and loose, and the tunnel is seriously damaged. The third is the goaf formed by the coal mine, which causes ground collapse, ground fissures and other disasters. Grouting technology has been used for the reinforcement of mine and tunnel surrounding rocks since the early 19th century. After long-term practice, it has been proved that it can well solve the safety problems encountered in coal mining.

[0003] Traditional grouting materials are divided into organic grouting materials, inorganic grouting materials and composite grouting materials. Organic grouting materials include: polyurethane, acrylamide, urea-formaldehyde resin, epoxy resin grouting materials, etc.; inorganic grouting materials include: cement slurry, cement clay, cement-water glass two-liquid grouting materials, etc.; composite grouting materials include: acrylate-cement, styrene-butadiene latex-cement composite grouting materials, etc.

[0004] Organic and composite grouting materials have good grouting performance and mechanical properties, but their high prices and environmental pollution risks limit their large-scale application. Traditional inorganic grouting materials have the disadvantages of slow setting speed, difficulty in adjusting according to site needs, large water-cement ratio, large shrinkage, and low strength. Patent application 201911422973.3 discloses an inorganic grouting material that can both stop water and strengthen the structure, including component A and component B. Component A is mainly made of the following raw materials in parts by weight: 3-4 parts of potassium silicate solution, 2-3 parts of sodium silicate solution, 1-1.5 parts of dispersant, 0.1-0.2 parts of defoamer (F04), and 10-13 parts of water; component B is mainly made of the following raw materials in parts by weight: 0.1-0.2 parts of water reducer, 20-25 parts of ultrafine cement, 8-9 parts of mineral powder, 0.5-0.7 parts of silica fume, 2-3 parts of fly ash, 0.5-0.6 parts of flocculant, 0.5-0.6 parts of expansion agent, 0-1 parts of retarder, and 10-13 parts of water. The two components are grouted in equal volumes using a double-liquid grouting machine according to the proportion when they are prepared. In this application, equal volumes of grouting materials were injected into components A and B. During the construction process, the viscosity of the two components was different, which easily caused a change in the volume ratio, resulting in deviations in the grouting results. In addition, a large amount of water was introduced into component A, which ultimately caused the water-cement ratio of the system to be too large, resulting in low final strength, and the final strength was only 5MPa.

[0005] Therefore, in industrial production practice, there is an urgent need for grouting materials with adjustable setting time and high strength after setting. Summary of the invention

[0006] The present invention can adjust the setting time of the grouting material in real time by adjusting the dosage of the B component, which is suitable for the requirements of different grouting conditions in current industrial practice. In addition, the grouting material of the present invention has high final strength after setting and good economic applicability.

[0007] To achieve the above purpose, the present invention adopts the following technical solutions:

[0008] The first aspect of the present invention provides a grouting material, comprising component A and component B, wherein component A comprises 1000-1600 parts by weight of cement, 500-1200 parts by weight of fly ash, 2-10 parts by weight of water reducer, 0.5-5 parts by weight of retarder, 0.5-2 parts by weight of wetting agent, 0.1-5 parts by weight of defoamer, 5-30 parts by weight of redispersible latex powder, 0.5-5 parts by weight of thickener, and 500-800 parts by weight of water;

[0009] The B component includes 400-800 parts by weight of an accelerating setting agent, 0.1-2 parts by weight of a wetting agent, 0.1-2 parts by weight of a thickening agent, 0.1-2 parts by weight of a defoaming agent, 0.1-10 parts by weight of a water reducing agent, and 300-700 parts by weight of water;

[0010] The mass ratio of the component A to the component B is 1:(0.0017-0.067).

[0011] When the mass ratio of component A to component B is greater than 1:0.0017, the setting time is long, the early strength is low, the effect of accelerating setting and early strength is poor, and the requirements of grouting reinforcement cannot be met. When the mass ratio of component A to component B is less than 1:0.067, the setting time is not further shortened, the early strength is not further increased, and the later strength even decreases to a certain extent.

[0012] In some preferred embodiments, the cement is selected from one or more of sulphoaluminate cement, ferroaluminate cement, aluminate cement and fluoroaluminate cement.

[0013] In some preferred embodiments, the pH of the accelerating setting agent is 9-14.

[0014] In some preferred embodiments, the accelerating setting agent includes a calcium-containing compound and a lithium salt or an aluminate; optionally, the accelerating setting agent also includes a sodium-containing compound.

[0015] The pH of the quick-setting agent is 9-14, so that during the hydration process, OH - It can replace A1 in sulphoaluminate cement, ferroaluminate cement, aluminate cement and / or fluoroaluminate cement.3+ The surrounding water molecules promote the dissolution of aluminum and reduce [Al(OH)6] 3- The free energy of octahedral nucleation and the critical size of the nucleus increase the rate of nucleation, which is beneficial to [Al(OH)6] 3- Preferably, when the quick-setting agent comprises a calcium-containing compound and a lithium salt or an aluminate, under alkaline conditions, the calcium-containing compound forms Ca 2+ , adding lithium salt or aluminate to form Li + or Al 3+ The above ions cooperate with each other to further promote [Al(OH)6] 3- The aggregation of octahedrons improves the strength of the grouting material after solidification.

[0016] In some preferred embodiments, the calcium-containing compound is selected from calcium oxide and / or calcium hydroxide; the lithium salt is selected from lithium sulfate and / or lithium carbonate; the aluminate is selected from aluminum sulfate and / or potassium aluminum sulfate dodecahydrate; the sodium-containing compound is selected from sodium hydroxide, sodium silicate, sodium sulfate and / or sodium carbonate.

[0017] In some preferred embodiments, the mass ratio of the lithium salt or aluminate to the calcium-containing compound is 1:(4-6). Optionally, the accelerator further comprises a sodium-containing compound; if a sodium-containing compound is added, the mass ratio of the lithium salt or aluminate to the total mass of the sodium-containing compound and the calcium-containing compound is 1:(4-6).

[0018] In some preferred embodiments, the water reducer is a powder water reducer with a water reducing efficiency greater than 30%, preferably a polycarboxylic acid powder water reducer; the retarder is selected from one or more of tartaric acid, boric acid and citric acid; the wetting agent is selected from one or more of sodium dodecylbenzene sulfonate, sodium dodecyl sulfate and dioctyl sodium succinate sulfonate; the defoamer is a powder defoamer polymerized from polysiloxane, emulsifier and polyether defoamer; the redispersible latex powder is vinyl acetate / ethylene copolymer powder; the thickener is selected from starch ether or cellulose ether.

[0019] In some preferred embodiments, the retarder is tartaric acid; the wetting agent is sodium dodecylbenzene sulfonate; the defoaming agent is BASF F04; the redispersible latex powder is Wacker 4036; and the thickener is methyl hydroxyethyl cellulose ether with a viscosity of less than 100,000.

[0020] In some preferred embodiments, the initial setting time of the grouting material is 30 seconds to 48 minutes, and the final setting time is 35 seconds to 53 minutes; the 1h strength of the grouting material is 2.0-22.9MPa, the 1d strength is 26.3-51.2MPa, and the 28d strength is 48.5-80MPa.

[0021] A second aspect of the present invention provides a method for preparing the grouting material as described above, comprising the following steps:

[0022] Mix cement, water reducing agent, retarder, wetting agent, defoamer, redispersible latex powder, thickener, fly ash and water according to proportion to obtain component A;

[0023] Mix water, wetting agent, thickener, defoamer, water reducing agent and accelerating setting agent according to the proportion to obtain component B;

[0024] The component A and the component B are mixed in a mass ratio of 1:(0.0017-0.067) to obtain the grouting material.

[0025] In some preferred embodiments, when preparing component A, cement, water reducing agent, retarder, wetting agent, defoamer, redispersible latex powder, and thickener are first added in proportion for mixing, and then fly ash is added for mixing. The obtained primary mixture is packaged for standby use. When the grouting material is ready to be used, water is added to the primary mixture and mixed to obtain component A. When preparing component B, water, wetting agent, thickener, defoamer, and water reducing agent are first mixed in proportion, and then an accelerator is added for mixing to obtain component B.

[0026] In some preferred embodiments, the initial fluidity of component A is ≥380 mm, and the fluidity after 30 min is ≥300 mm; the fluidity of component B is ≥380 mm.

[0027] A third aspect of the present invention provides a use of the grouting material as described above or the grouting material prepared by the preparation method as described above in water blocking and / or reinforcement.

[0028] The technical solution provided by the present invention has the following beneficial effects:

[0029] (1) In the grouting material provided by the present invention, by adding a retarder, a defoamer, a water reducer, a wetting agent, a redispersible latex powder and a thickener, these components interact with each other, so that the grouting material has excellent fluidity;

[0030] (2) In the grouting material provided by the present invention, the interaction between cement and accelerating agent enables the grouting material to have ultra-early strength and higher final strength;

[0031] (3) The grouting material provided by the present invention breaks through the limitations of the existing two-component grouting equal proportion and fixed proportion grouting, thereby solving the problem of the volume ratio changing due to the different viscosities of the two components during the grouting process, which ultimately leads to poor grouting effect;

[0032] (4) The grouting material provided by the present invention can adjust the setting time of the grouting material in real time according to the characteristics of the injected body, so as to prevent the setting time from being too long or too short and the grouting diffusion range from being too small. At the same time, the setting time of the grouting material provided by the present invention can be from tens of seconds to tens of minutes, so that it can be used for both water blocking and reinforcement. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 It is a flow chart of the grouting material of the present invention during grouting;

[0034] Figure 2 It is a schematic structural diagram of a grouting device used in one embodiment of the present invention;

[0035] Explanation of the reference numerals: 10 - main pump; 12 - main pump storage bin; 20 - auxiliary pump; 22 - auxiliary pump storage bin; 30 - mixer; 32 - mixing screw; 40 - grouting pipe. DETAILED DESCRIPTION

[0036] The present invention is further described below by means of specific embodiments. The embodiments of the present invention are only used as illustrations of the present invention and do not mean that the scope of the present invention is limited thereto.

[0037] The grouting material provided by the present invention can be prepared and / or used by equipment known in the art, preferably by the following equipment:

[0038] Figure 2 The grouting equipment used for the grouting material used in one embodiment of the present invention is shown, which includes: a main pump 10 with a storage bin 12, an auxiliary pump 20 with a storage bin 22, a mixer 30 and a grouting pipe 40.

[0039] The main pump 10 is used to provide power for the delivery of component A. The main pump 10 can be a screw pump, an extrusion pump, a centrifugal pump, etc., to ensure the smoothness of grouting; the auxiliary pump 20 is used to provide power for the delivery of component B. The auxiliary pump 20 can be a piston pump, a plunger pump, a diaphragm pump, etc., to accurately control the flow rate. In some embodiments, the maximum flow rate of the auxiliary pump 20 is about one tenth of the maximum flow rate of the main pump, and the pressure is ensured to exceed the main pump 10, so as to prevent the grouting material from flowing back into the delivery pipeline of component B and causing blockage. The outlets of the main pump storage bin 12 and the auxiliary pump storage bin 22 are respectively connected to the inlet of the mixer 30, and the mixer 30 is used to mix the component A and the component B evenly. The outlet of the mixer 30 is connected to the grouting body through the grouting pipe 40.

[0040] When grouting is implemented, component A is placed in the storage bin 12 of the main pump 10, and component B is placed in the storage bin 22 of the auxiliary pump 20. The main pump 10 is turned on, and component A enters the mixer 30. After 5-20 seconds, the auxiliary pump 20 is turned on, and component B enters the mixer 30 to be mixed with component A to obtain grouting material. The grouting material enters the grouting body through the grouting pipe 40 for water blocking or reinforcement.

[0041] In some preferred embodiments, the mixer 30 includes a mixing screw 32, which includes left-handed screws and right-handed screws alternately distributed in the axial direction, and each screw appears twice or more. Component A and component B are reversed multiple times by the mixing screw 32, thereby ensuring that the two are fully and evenly mixed.

[0042] In some preferred embodiments, the mixer 30 is communicatively connected with an intelligent control system, so that the intelligent control system can control the feed speed, feed ratio, discharge speed, grouting pressure, temperature, grouting volume record, etc. of the mixer 30, and further realize real-time adjustment of the setting time of the grouting material.

[0043] The grouting material provided by the present invention can be grouted using a mixing device, a grouting device, etc. known in the art, or can be grouted using the grouting device described above. For ease of explanation, the following embodiments all use the above grouting device to mix component A and component B and grout the resulting grouting material.

[0044] Instrument: The instrument for measuring the strength of the grouting material is a multifunctional flexural and compressive press (maximum compressive test force: 300kN, maximum flexural test force: 10kN), the measuring cylinder (1000ml) is used to measure the water seepage rate of the grouting material, and the fullness of the grouting material is measured by a fullness tube (inner diameter 40mm, angle 120 degrees). The specific measurement method refers to the standard: QCR 409-2017 Technical Conditions for Pipe Grouting of Post-Tensioned Prestressed Concrete Beams in Railways.

[0045] Example 1-1

[0046] The preparation method of component A is as follows: add 600g of sulphoaluminate cement and 600g of aluminate cement, add 3.5g of water reducer (Sika 540P), 2.5g of retarder (tartaric acid), 0.5g of wetting agent (sodium dodecylbenzene sulfonate), 1g of defoamer (BASF F04), 8g of redispersible latex powder (Wacker 4036), 0.5g of thickener (Lotte Cellulose B30K) while stirring, then add 1200g of fly ash, continue stirring for 20min, and pack as the primary mixture. When preparing for grouting, add 600g of water to the primary mixture and stir. The initial fluidity of component A is 400mm, and the fluidity after 30min is 370mm.

[0047] The preparation method of component B is as follows: add 500g of water, add 1g of wetting agent (sodium dodecylbenzene sulfonate), 1g of thickener (Lotte Cellulose B30K), 1g of defoamer (BASF F04) and 5g of water reducer (Sika 540P) while stirring, stir evenly, then add 500g of quick-setting agent calcium oxide and 100g of lithium sulfate, the pH of the quick-setting agent is 10, and continue stirring. The fluidity of component B is 390mm.

[0048] Put component A into the storage bin of the main pump and component B into the storage bin of the auxiliary pump, turn on the main pump, component A enters the mixer, and after 15 seconds, turn on the auxiliary pump, component B enters the mixer and is fully mixed with component A (the mass ratio of component A to component B is 1:0.017) to obtain grouting material.

[0049] The initial setting time of the obtained grouting material is 30s, the final setting time is 35s, the 0.5h strength is 14.8MPa, the 1h strength is 22.9MPa, the 24h strength is 51.2MPa, the 28d strength is 80.0MPa, the water seepage rate is 0%, and the filling degree is qualified. The grouting material has short initial setting and final setting times, can reach high strength in a short time, and is suitable for grouting and water blocking.

[0050] Example 1-2

[0051] Example 1-2 is basically the same as Example 1-1, except that: in the preparation method of component A, 800g of sulphoaluminate cement and 400g of aluminate cement are used instead of 600g of sulphoaluminate cement and 600g of aluminate cement. In the preparation method of component B, 100g of lithium carbonate is used instead of 100g of lithium sulfate. The initial fluidity of component A is 390mm, and the fluidity of 30min is 365mm; the fluidity of component B is 400mm. When preparing for grouting, the auxiliary pump is turned on after turning on the main pump for 20s.

[0052] The initial setting time of the obtained grouting material is 40s, the final setting time is 48s, the 0.5h strength is 10.5MPa, the 1h strength is 18.7MPa, the 24h strength is 48.5MPa, the 28d strength is 75.3MPa, the water seepage rate is 0%, and the filling degree is qualified. The grouting material has short initial setting and final setting times, can reach high strength in a short time, and is suitable for grouting and water blocking.

[0053] Examples 1-3

[0054] Example 1-3 is basically the same as Example 1-1, except that: in the preparation method of component A, 1200 g of sulphoaluminate cement is used instead of 600 g of sulphoaluminate cement and 600 g of aluminate cement. The initial fluidity of component A is 395 mm, and the fluidity after 30 min is 370 mm; the fluidity of component B is 385 mm.

[0055] The initial setting time of the obtained grouting material is 315s, the final setting time is 841s, the 1h strength is 17.8MPa, the 24h strength is 39.9MPa, the 28d strength is 65.3MPa, the water seepage rate is 0%, and the filling degree is qualified. The grouting material still has good fluidity after mixing, and the initial setting and final setting time are short, and a high strength can be achieved in a short time. It can be used for both slight grouting water blocking and grouting reinforcement.

[0056] Examples 1-4

[0057] Example 1-4 is basically the same as Example 1-1, except that: in the preparation method of component A, 1200g of sulphoaluminate cement is used instead of 600g of sulphoaluminate cement and 600g of aluminate cement, and 3.7g of water reducer (Sika 540P) and 3g of retarder (tartaric acid) are used instead of 3.5g of water reducer (Sika 540P) and 2.5g of retarder (tartaric acid). In the preparation method of component B, 250g of quick-setting agent calcium oxide, 50g of lithium sulfate and 250g of sodium hydroxide are used instead of 500g of quick-setting agent calcium oxide and 100g of lithium sulfate, and the pH of the quick-setting agent is 14. The initial fluidity of component A is 400mm, and the fluidity of 30min is 375mm; the fluidity of component B is 390mm. When preparing for grouting, turn on the auxiliary pump after turning on the main pump for 20s.

[0058] The initial setting time of the obtained grouting material is 2218s, the final setting time is 2650s, the 1h strength is 5.5MPa, the 24h strength is 38.5MPa, the 28d strength is 62.3MPa, the water seepage rate is 0%, and the filling degree is qualified. The grouting material still has particularly good fluidity after mixing, and the initial setting and final setting times are long, and it is suitable for grouting reinforcement.

[0059] Examples 1-5

[0060] Example 1-5 is basically the same as Example 1-1, except that: in the preparation method of component A, 1200g of aluminate cement is used instead of 600g of sulphoaluminate cement and 600g of aluminate cement, the amount of water reducer is different, 2.5g of water reducer (Sika 540P) is added, 2.5g of retarder (tartaric acid) and 0.5g of (boric acid) are used instead of 2.5g of retarder (tartaric acid). The pH of the quick-setting agent is 12. The initial fluidity of component A is 405mm, and the fluidity after 30min is 380mm; the fluidity of component B is 400mm. When preparing for grouting, turn on the auxiliary pump after turning on the main pump for 20s.

[0061] The initial setting time of the obtained grouting material is 110s, the final setting time is 123s, the 0.5h strength is 8.8MPa, the 1h strength is 15.8MPa, the 24h strength is 36.7MPa, the 28d strength is 60.0MPa, the water seepage rate is 0%, and the filling degree is qualified. The grouting material still has good fluidity after mixing, and the initial setting and final setting time are short, and a high strength can be achieved in a short time. It can be used for both slight grouting water blocking and grouting reinforcement.

[0062] Comparative Example 1-1

[0063] In the preparation method of component A, 1200 g of aluminate cement is added, and while stirring, 2.5 g of water reducer (SIKA 540P), 2.5 g of retarder (tartaric acid) and 0.5 g of (citric acid), 0.5 g of wetting agent (sodium dodecylbenzene sulfonate), 1 g of defoamer (BASF F04), 8 g of redispersible latex powder (Wacker 4036), and 0.5 g of thickener (Lotte Cellulose B30K) are added, and then 1200 g of fly ash is added, and stirring is continued for 20 minutes. The primary mixture is discharged and packaged. When grouting is prepared, 600 g of water is added to the primary mixture and stirred. In the preparation method of component B, add 550g of water, add 1g of wetting agent (sodium dodecylbenzene sulfonate), 1g of thickener (Lotte Cellulose B30K), 1g of defoamer (BASF F04) and 5g of water reducer (Sika 540P) while stirring, stir evenly, then add 550g of quick-setting agent calcium oxide, the pH of the quick-setting agent is 10, and continue stirring. The initial fluidity of component A is 405mm, and the fluidity of 30min is 380mm; the fluidity of component B is 400mm. When preparing for grouting, turn on the auxiliary pump after turning on the main pump for 20s.

[0064] The initial setting time of the obtained grouting material is 210s, the final setting time is 854s, the 1h strength is 0.5MPa, the 24h strength is 22.5MPa, and the 28d strength is 45.5MPa. Comparing Comparative Example 1-1 with Example 1-5, Comparative Example 1-1 does not add lithium carbonate. Compared with Example 1-5, both the initial setting time and the final setting time are greatly delayed. The 1h strength is much smaller than that of Example 1-5, and the 24h strength is also significantly reduced. The above comparison shows that the addition of lithium salts or aluminates promotes the combination reaction of sulfate cement and calcium-containing compounds by changing the hydration environment of cement and the binding state of ions, thereby further promoting the coagulation and early strength of cement.

[0065] Comparative Example 1-2

[0066] In the preparation method of component A, 1200 g of sulphoaluminate cement is added, and while stirring, 3.5 g of water reducer (SIKA 540P), 2.5 g of retarder (tartaric acid), 0.5 g of wetting agent (sodium dodecylbenzene sulfonate), 1 g of defoamer (BASF F04), 8 g of redispersible latex powder (Wacker 4036), and 0.5 g of thickener (Lotte Cellulose B30K) are added, and then 1200 g of fly ash is added, and stirring is continued for 20 minutes. The primary mixture is discharged and packaged. When grouting is prepared, 600 g of water is added to the primary mixture and stirred. In the preparation method of component B, 1000g of water is added, and 1g of wetting agent (sodium dodecylbenzene sulfonate), 1g of thickener (Lotte Cellulose B30K), 1g of defoamer (BASF F04) and 5g of water reducer (Sika 540P) are added while stirring, and after stirring evenly, 100g of accelerator lithium sulfate is added, and the pH of the accelerator is 10, and stirring is continued. The initial fluidity of component A is 395mm, and the fluidity after 30min is 370mm; the fluidity of component B is 385mm.

[0067] The initial setting time of the obtained grouting material is 1800s, the final setting time is 2100s, the 1h strength is 3.2MPa, the 24h strength is 35.8MPa, and the 28d strength is 55.2MPa. Comparing Comparative Example 1-2 with Example 1-3, Comparative Example 1-2 does not add calcium carbonate. Compared with Example 1-3, both the initial setting time and the final setting time are particularly delayed. The 1h strength is much smaller than that of Example 1-3, and the 24h strength is also reduced. The above comparison shows that the calcium-containing compound and lithium salt or aluminate act together, and the calcium-containing compound and lithium salt or aluminate are both necessary. The hydration of lithium salt or aluminate with cement is far from enough, and the technical problem of rapid early strength of cement cannot be solved. It is necessary to add calcium-containing compounds to play a synergistic role.

[0068] Example 2

[0069] Example 2-1

[0070] The compositions of component A and component B are the same as those in Example 1-1. By changing the added mass of component B, the performance of the obtained grouting material was tested. The results are shown in Table 1:

[0071] Table 1

[0072]

[0073] It can be seen from Table 1 that component B has good solidification properties when added in small amounts. As the amount of component B added gradually increases, the setting time of the resulting grouting material can be very short. During grouting, the slurry can quickly solidify and lose fluidity, and will not disperse in water or be washed away by water flow. It is suitable for grouting and water plugging in areas with very serious leakage.

[0074] Example 2-2

[0075] The compositions of component A and component B are the same as those in Example 1-3. By changing the added mass of component B, the performance of the obtained grouting material was tested. The results are shown in Table 2:

[0076] Table 2

[0077]

[0078] It can be seen from Table 2 that a small amount of component B added to the slurry has a certain fluidity, allowing the slurry to diffuse in the rock gap, so it can also be used for grouting reinforcement. With the further addition of component B, the setting time of the grouting material can be shorter. During grouting, the slurry can quickly solidify and lose fluidity, and can be prevented from dispersing in water and being washed away by water flow, which is suitable for grouting water blocking of a slight degree.

[0079] Example 2-3

[0080] The compositions of component A and component B are the same as those in Example 1-4. By changing the added mass of component B, the performance of the obtained grouting material was tested. The results are shown in Table 3:

[0081] Table 3

[0082]

[0083] It can be seen from Table 3 that the setting time of the obtained grouting material is relatively long, and the slurry will not disperse in the water during grouting and is easily washed away by the water flow, which is not suitable for grouting water blocking. However, the slurry also maintains good fluidity, making it easy for the slurry to diffuse in the rock gaps, so it is suitable for grouting reinforcement with more rock gaps.

[0084] Embodiment 2-4

[0085] The compositions of component A and component B are the same as those in Example 1-5. By changing the added mass of component B, the performance of the obtained grouting material was tested. The results are shown in Table 4:

[0086] Table 4

[0087]

[0088]

[0089] It can be seen from Table 4 that component B has good solidification when added in small amounts. As the amount of component B added gradually increases, the setting time of the resulting grouting material can be very short. During grouting, the slurry can quickly solidify and lose fluidity, and will not disperse in water or be washed away by water flow. It is suitable for grouting and water plugging in areas with very serious leakage.

[0090] Embodiment 2-5

[0091] The preparation method of component A is as follows: in a mixing device, add 1600g of sulphoaluminate cement, add 1.6g of water reducer (SIKA 540P), 1.5g of retarder (tartaric acid), 0.5g of wetting agent (sodium dodecylbenzene sulfonate), 1g of defoamer (BASF F04), 8g of redispersible latex powder (Wacker 4036), 0.5g of thickener (Lotte Cellulose B30K) while stirring, then add 1800g of fly ash, continue stirring for 15 minutes, and package the primary mixture as a discharge. When preparing for grouting, add 600g of water to the primary mixture and stir.

[0092] The preparation method of component B is as follows: add 500g of water into a container, add 1g of wetting agent (sodium dodecylbenzene sulfonate), 1g of thickener (Lotte cellulose B30K), 1g of defoamer (powder defoamer F04 polymerized from polysiloxane, special emulsifier and high-activity polyether defoamer) and 5g of water reducer (Sika 540P) while stirring, stir evenly, then add 250g of accelerator calcium oxide, 50g of lithium sulfate and 250g of sodium hydroxide, the pH of the accelerator is 10, and continue stirring.

[0093] By changing the added mass of component B, the performance of the obtained grouting material was tested, and the results are shown in Table 5:

[0094] Table 5

[0095]

[0096] It can be seen from Table 5 that a small amount of component B added to the slurry has a certain fluidity, allowing the slurry to diffuse in the rock gap, so it can also be used for grouting reinforcement. With the further addition of component B, the setting time of the grouting material can be shorter. During grouting, the slurry can quickly solidify and lose fluidity, and can be prevented from dispersing in water and being washed away by water flow, which is suitable for mild grouting water blocking.

[0097] Comparative Example 2-1

[0098] The composition of component A and component B is the same as that of Example 2-2. By changing the added mass of component B, the performance of the obtained grouting material is tested. When the mass ratio of component A to component B is greater than 1:0.0017, the results are shown in Table 6:

[0099] Table 6

[0100]

[0101] It can be seen from the results in Table 6 that when the mass ratio of component A to component B is greater than 1:0.0017, the setting time is long, the early strength is low, the effect of accelerating setting and early strength is poor, and the requirements of grouting reinforcement cannot be met.

[0102] Comparative Example 2-2

[0103] The composition of component A and component B is the same as that of Example 2-4. By changing the added mass of component B, the performance test of the obtained grouting material is carried out. When the mass ratio of component A to component B is less than 1:0.067, the results are shown in Table 7:

[0104] Table 7

[0105]

[0106]

[0107] From the results in Table 7, it can be seen that when the mass ratio of component A to component B is less than 1:0.067, the setting time is not further shortened, the early strength is not further increased, and the later strength even decreases to a certain extent. The reason may be that component B, as a coagulation and early strength accelerator, does not have curing strength itself, so when the dosage is too large, it will dilute the curing strength substance in component A, which will eventually increase the setting time and decrease the early strength and later strength.

[0108] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.

Claims

1. A grouting material, characterized in that: The invention comprises component A and component B, wherein the component A comprises 1000-1600 parts by weight of cement, 500-1200 parts by weight of fly ash, 2-10 parts by weight of water reducer, 0.5-5 parts by weight of retarder, 0.5-2 parts by weight of wetting agent, 0.1-5 parts by weight of defoamer, 5-30 parts by weight of redispersible latex powder, 0.5-5 parts by weight of thickener, and 500-800 parts by weight of water; The B component includes 400-800 parts by weight of an accelerating setting agent, 0.1-2 parts by weight of a wetting agent, 0.1-2 parts by weight of a thickening agent, 0.1-2 parts by weight of a defoaming agent, 0.1-10 parts by weight of a water reducing agent, and 300-700 parts by weight of water; The mass ratio of the component A to the component B is 1:(0.0017-0.067).

2. The grouting material according to claim 1, characterized in that: The cement is selected from one or more of sulphoaluminate cement, ferroaluminate cement, aluminate cement and fluoroaluminate cement.

3. The grouting material according to claim 1, characterized in that: The pH of the quick-setting agent is 9-14.

4. The grouting material according to claim 3, characterized in that: The accelerator comprises a calcium-containing compound and a lithium salt or an aluminate; optionally, the accelerator further comprises a sodium-containing compound; preferably, the calcium-containing compound is selected from calcium oxide and / or calcium hydroxide; the lithium salt is selected from lithium sulfate and / or lithium carbonate; the aluminate is selected from aluminum sulfate and / or potassium aluminum sulfate dodecahydrate; the sodium-containing compound is selected from sodium hydroxide, sodium silicate, sodium sulfate and / or sodium carbonate.

5. The grouting material according to claim 4, characterized in that: The mass ratio of the lithium salt or aluminate to the calcium-containing compound is 1:(4-6).

6. The grouting material according to claim 1, characterized in that: The water reducing agent is a powder water reducing agent with a water reducing efficiency greater than 30%, preferably a polycarboxylic acid powder water reducing agent; The retarder is selected from one or more of tartaric acid, boric acid and citric acid; The wetting agent is selected from one or more of sodium dodecylbenzene sulfonate, sodium dodecyl sulfate and dioctyl sodium sulfosuccinate; The defoamer is a powder defoamer prepared by polymerization of polysiloxane, emulsifier and polyether defoamer, preferably BASF F04; The redispersible latex powder is vinyl acetate / ethylene copolymer rubber powder, preferably Wacker 4036; The thickener is selected from starch ether or cellulose ether, preferably methyl hydroxyethyl cellulose ether with a viscosity less than 100,000.

7. The grouting material according to any one of claims 1 to 6, characterized in that: The initial setting time of the grouting material is 30 seconds to 48 minutes, and the final setting time is 35 seconds to 53 minutes; the 1h strength of the grouting material is 2.0-22.9MPa, the 1d strength is 26.3-51.2MPa, and the 28d strength is 48.5-80MPa.

8. The method for preparing the grouting material according to any one of claims 1 to 7, characterized in that: The steps include: Mix cement, water reducing agent, retarder, wetting agent, defoamer, redispersible latex powder, thickener, fly ash and water according to proportion to obtain component A; Mix water, wetting agent, thickener, defoamer, water reducing agent and accelerating setting agent according to the proportion to obtain component B; The component A and the component B are mixed in a mass ratio of 1:(0.0017-0.067) to obtain the grouting material.

9. The method for preparing the grouting material according to claim 8, characterized in that: The initial fluidity of the A component is ≥380 mm, and the 30-min fluidity is ≥300 mm; the fluidity of the B component is ≥380 mm.

10. Use of the grouting material according to any one of claims 1 to 7 or the grouting material prepared by the preparation method according to claim 8 or 9 in water blocking and / or reinforcement.

Citation Information

Patent Citations

  • Inorganic grouting material capable of stopping open water and reinforcing structure as well as preparation method and application thereof

    CN111072366A

  • Cement grouting material

    CN105272070A

  • Early-strength high-strength double-component grouting material with controllable setting time and preparation method thereof

    CN112441807A