Near-zero thermal expansion ceramic material RE2ZrMo5O20 and preparation method thereof

By preparing RE2ZrMo5O20 near-zero thermal expansion ceramic material, the problems of aging and reduced stability of the material during thermal expansion and contraction are solved, and high-performance applications in medical devices and aerospace fields are achieved.

CN119059816APending Publication Date: 2024-12-03ZHENGZHOU UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411251467.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-07
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

During the thermal expansion and contraction of existing materials, the machine components are aging and the stability is reduced. The difference in thermal expansion coefficients between different materials causes an increase in internal stress, affecting the performance and service life of the instrument, especially in the fields of medical devices and aerospace. .

Method used

Using RE2ZrMo5O20 (RE=Yb or Tm) near-zero thermal expansion ceramic material and its preparation method, the ceramic material with near-zero thermal expansion coefficient is prepared by selecting suitable RE, Zr and Mo sources for mixing and sintering of stoichiometric molar ratios. .

Benefits of technology

The RE2ZrMo5O20 material was successfully prepared, showing the near-zero thermal expansion characteristics, with simple process and low cost, suitable for applications in high-end technical fields, extending the material life and expanding the application range.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119059816A_ABST
    Figure CN119059816A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of thermal expansion materials, and discloses a near-zero thermal expansion ceramic material and a preparation method thereof. The molecular formula of the compound is RE2ZrMo5O20 (RE = Yb or Tm). The preparation method comprises the following steps: selecting an RE source, a Zr source and a Mo source as raw materials, weighing the raw materials according to the stoichiometric molar ratio of RE to Zr to Mo of 2: 1: 5 in the target product RE2ZrMo5O20, grinding and mixing uniformly, directly sintering the obtained mixed powder or sintering the mixed powder after tabletting at the sintering temperature of 700-800 DEG C for 40-50 hours, and cooling to room temperature to obtain the target product RE2ZrMo5O20. The RE2ZrMo5O20 (RE = Yb or Tm) has a thermal expansion coefficient close to zero, has good thermal stability, is simple in preparation process and low in cost, is suitable for industrial production, and is expected to be widely applied to the high-end technical fields of electronic devices, aerospace, precise instruments and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of thermal expansion materials, and specifically relates to a near-zero thermal expansion ceramic material RE2ZrMo5O 20 and a preparation method thereof. Background Art

[0002] Most materials expand and contract when heated and cool, which leads to accelerated aging of machine parts, reduced stability and safety reliability, loss of functional characteristics, and shortened service life. However, very few materials have unique negative thermal expansion characteristics (NTE), which are particularly important in the fields of precision instruments such as medical devices, aerospace, and optical communications. These fields require precise control of the coefficient of thermal expansion (CTE) of the material to ensure stable operation of the instrument in complex environments. The difference in CTE between different materials may cause increased internal stress, change the surface contact state and tribological design, and ultimately lead to functional failure. Therefore, the thermal expansion properties of materials have a profound impact on component performance, system life and application range. Near-zero expansion materials (NZTE) have become the preferred choice for extending material life and expanding application range due to their low sensitivity to temperature changes, high dimensional stability and safety of use. At present, seeking NZTE or controllable expansion materials is an effective way to solve such problems.

[0003] In recent years, molybdate materials have become a shining star in the field of materials science research due to their unique physical and chemical properties, especially their outstanding performance in regulating the thermal expansion coefficient. This type of material not only has adjustable thermal expansion properties, but also exhibits excellent electrical conductivity, opening up new ways to manufacture high-performance ceramics, metals and polymer materials. In high-tech fields such as optical mechanics, aerospace and electronics industries, there is an increasing demand for such materials with specific thermal expansion coefficients. Among the many molybdate materials, dimolybdates such as Ln2Zr3(MoO4)9, Ln2Zr2(MoO4)7 and Ln2Zr(MoO4)5 have attracted much attention due to their complex crystal structures and unique thermal behaviors. These compounds are formed under specific phase equilibrium conditions and exhibit diverse thermal expansion properties, providing rich possibilities for material design. Summary of the invention

[0004] In order to overcome the shortcomings of the prior art, the present invention aims to provide a near-zero thermal expansion ceramic material RE2ZrMo5O 20 and a preparation method thereof.

[0005] To achieve the above purpose, the technical solution adopted by the present invention is as follows: A near-zero thermal expansion ceramic material with the molecular formula RE2ZrMo5O 20 , RE=Yb or Tm.

[0006] A method for preparing a near-zero thermal expansion ceramic material: selecting RE source, Zr source and Mo source as raw materials, and preparing a target product RE2ZrMo5O 20 The stoichiometric molar ratio of RE: Zr: Mo is 2: 1: 5, and the mixture is weighed and ground to mix evenly. The obtained mixed powder is directly sintered or pressed into tablets and sintered at a temperature of 700-800 °C for 40-50 h. The mixture is cooled to room temperature to obtain the target product RE2ZrMo5O 20 ; Wherein, the RE source is RE2O3 or a precursor material that can be heated and decomposed at a temperature not higher than the sintering temperature to obtain RE2O3; RE2O3=Yb2O3 or Tm2O3; The Zr source is ZrO2 or a precursor material such as Zr(OH)4 that can be heated and decomposed to obtain ZrO2 at a temperature not higher than the sintering temperature; The Mo source is MoO3 or a precursor material that can be heated and decomposed at a temperature not higher than the sintering temperature to obtain MoO3.

[0007] Preferably, after weighing the RE source, Zr source and Mo source in proportion and grinding and mixing them evenly, the obtained mixed powder is first pre-sintered directly or pre-sintered after tableting, and then the pre-sintered product is ground and mixed evenly, and then sintered again after tableting; the pre-sintering temperature is 300~400℃ and the time is 5~10h, and the secondary sintering temperature is 700~800℃ and the time is 40~50h.

[0008] Preferably, when the RE source, Zr source and Mo source are weighed in proportion and ground and mixed uniformly, wet grinding is adopted, and ethanol is added during grinding, and the added amount is based on wetting the RE source, Zr source and Mo source.

[0009] Preferably, dry grinding is used when grinding and mixing the pre-sintered product uniformly.

[0010] Preferably, the purity of the RE source, Zr source and Mo source is 99-99.99 wt %.

[0011] Preferably, all sintering processes are carried out at a heating rate of 3-10°C / min to reach the sintering temperature.

[0012] Preferably, all tablets involved are pressed into cylindrical green embryos with a diameter of 8 to 10 mm and a height of 3 to 6 mm.

[0013] Preferably, for all tableting processes involved, the tableting pressure is 4-10 MPa and the holding time is 2-5 min.

[0014] Beneficial effects: (1) The present invention first proposed a molecular formula of RE2ZrMo5O 20The near-zero thermal expansion ceramic material (RE = Yb or Tm) was successfully prepared by characterizing its phase purity and studying its thermal expansion properties. 20 (RE=Yb or Tm) materials exhibit near-zero thermal expansion characteristics within a certain temperature range; (2) RE2ZrMo5O of ​​the present invention 20 (RE=Yb or Tm) The material has a thermal expansion coefficient close to zero, a simple preparation process, low cost, and is suitable for industrial production. It is expected to be widely used in high-end technical fields such as electronic devices, aerospace, and precision instruments. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 :RE2ZrMo5O 20 Room temperature XRD refinement pattern of (RE = Yb, Tm or Y).

[0016] Figure 2 :RE2ZrMo5O 20 (RE=Yb, Tm or Y) structural transition diagram.

[0017] Figure 3 :RE2ZrMo5O 20 Raman spectrum of (RE=Yb, Tm or Y).

[0018] Figure 4 :RE2ZrMo5O 20 (RE=Yb, Tm or Y) relative length curve versus temperature. DETAILED DESCRIPTION

[0019] The following is a clear and complete description of the technical solution of the present invention in conjunction with the specific embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0020] Example 1 Solid-phase method for preparing Yb2ZrMo5O 20 Ceramic powder: Analytical pure Yb2O3, ZrO2 and MoO3 were selected as raw materials, and Yb2O3, ZrO2 and MoO3 were precipitated into the target product Yb2ZrMo5O 20The mixture was weighed and mixed in a stoichiometric molar ratio of Yb:Zr:Mo =2:1:5, put into an agate mortar, and moistened with anhydrous ethanol (the amount of anhydrous ethanol added was based on the amount of Yb2O3, ZrO2 and MoO3 that can be moistened), and ground for 2 hours. The obtained mixed powder was put into a crucible, and heated to 400°C in a muffle furnace at a heating rate of 5°C / min, and pre-sintered for 10 hours at a temperature preservation, and naturally cooled to room temperature in the air. The pre-sintered powder was taken out and dry-ground, and the ground powder was pressed into a cylindrical blank with a diameter of 8 mm and a height of 4 mm at a pressure of 10 MPa for 2 minutes; the cylindrical blank was put into a crucible, and heated to 800°C in a muffle furnace at a heating rate of 5°C / min, and sintered for 50 hours at a temperature preservation, and naturally cooled to room temperature in the air to obtain the target product Yb2ZrMo5O 20 .

[0021] Example 2 Solid-phase method for preparing Tm2ZrMo5O 20 Ceramic powder: Analytical pure Tm2O3, ZrO2 and MoO3 were selected as raw materials, and Tm2O3, ZrO2 and MoO3 were precipitated into the target product Tm2ZrMo5O 20 The mixture was weighed and mixed in a stoichiometric molar ratio of Tm: Zr: Mo = 2: 1: 5, put into an agate mortar, and moistened with anhydrous ethanol (the amount of anhydrous ethanol added was based on the amount of Tm2O3, ZrO2 and MoO3 that can be moistened), and ground for 2 h. The obtained mixed powder was put into a crucible, heated to 400 °C in a muffle furnace at a heating rate of 5 °C / min, and pre-sintered for 10 h at a temperature preservation, and naturally cooled to room temperature in the air. The pre-sintered powder was taken out and dry-ground, and the ground powder was pressed into a cylindrical blank with a diameter of 8 mm and a height of 4 mm at a pressure of 10 MPa for 2 min. The cylindrical blank was put into a crucible, heated to 750 °C in a muffle furnace at a heating rate of 5 °C / min, and sintered for 50 h at a temperature preservation, and naturally cooled to room temperature in the air to obtain the target product Tm2ZrMo5O 20 .

[0022] Comparative Example 1 Solid-state method for preparing Y2ZrMo5O 20 Ceramic powder: Analytical pure Y2O3, ZrO2 and MoO3 were selected as raw materials, and Y2O3, ZrO2 and MoO3 were precipitated into the target product Y2ZrMo5O 20The mixture was weighed and mixed in a stoichiometric molar ratio of Y: Zr: Mo = 2: 1: 5, put into an agate mortar, and wetted with anhydrous ethanol (the amount of anhydrous ethanol added was based on wetting Y2O3, ZrO2 and MoO3), and ground for 2 hours. The obtained mixed powder was put into a crucible, heated to 400°C in a muffle furnace at a heating rate of 5°C / min, and pre-sintered for 10 hours at a temperature preservation, and naturally cooled to room temperature in the air. The pre-sintered powder was taken out and dry-ground, and the ground powder was pressed into a cylindrical blank with a diameter of 8 mm and a height of 4 mm at a pressure of 10 MPa for 2 minutes; the cylindrical blank was put into a crucible, heated to 800°C in a muffle furnace at a heating rate of 5°C / min, and sintered for 50 hours at a temperature preservation, and naturally cooled to room temperature in the air to obtain the target product Y2ZrMo5O 20 .

[0023] Product Characterization and Performance Testing RE2ZrMo5O prepared in Examples 1-2 and Comparative Example 1 20 (RE = Yb, Tm or Y) XRD refinement pattern at room temperature is shown in Figure 1 . Using FullProf software, Yb2ZrMo5O 20 、Tm2ZrMo5O 20 and Y2ZrMo5O 20 The samples were subjected to Rietveld refinement, and the positions and intensities of their diffraction peaks were consistent with those of Ho2ZrMo5O 20 (CSD 2314996) is consistent with the above results, which proves that Yb2ZrMo5O 20 、Tm2ZrMo5O 20 and Y2ZrMo5O 20 The purity is high. In addition, the unit cell parameters of the sample were refined with the help of FullProf software, as shown in Table 1. The results show that: as the atomic radius of the RE atoms increases, their unit cell parameters tend to increase.

[0024]

[0025] RE2ZrMo5O prepared in Examples 1-2 and Comparative Example 1 20 (RE = Yb, Tm or Y) structural transformation diagram see Figure 2 Based on the subsolidus phase equilibrium of RE2O3-ZrO2-MoO3 system, Zr2Mo2O8 and RE2Mo3O 12 The interaction of the double molybdate material RE2ZrMo5O 20 (RE = Yb, Tm or Y), their structures are similar to Ho2ZrMo5O 20 (CSD 2314996) and both belong to the monoclinic P21 space group.20 The structure of (RE = Yb, Tm or Y) is composed of (RE / Zr)O6 hexahedrons, REO8 polyhedrons and slightly deformed MoO4 tetrahedrons connected by vertex oxygen. Its crystal structure along the b axis is as follows Figure 2 As shown in the left figure. As the temperature rises, RE2Zr(MoO4)5 undergoes a phase transition. While keeping the polyhedral connection unchanged, its space group changes to Cmc 21 (orthogonal phase), such as Figure 2 As shown in the picture on the right.

[0026] RE2ZrMo5O prepared in Examples 1-2 and Comparative Example 1 20 (RE = Yb, Tm or Y) Raman spectrum of the sample is shown in Figure 3 Since the three samples have similar structures, their room temperature Raman spectra are similar. Figure 3 Medium, 230cm -1 Up to 400cm -1 The Raman modes in the range correspond to the bending vibrations of MoO4 polyhedron and REO6 (ZrO6) polyhedron; 700 cm -1 Up to 1000cm -1 The Raman modes in this range correspond to the symmetric and antisymmetric stretching vibrations of MoO4 polyhedron.

[0027] RE2ZrMo5O prepared in Examples 1-2 and Comparative Example 1 20 (RE = Yb, Tm or Y) The relative length of the sample (i.e. dL / L0, where dL = the length after expansion - the original length L0, the same below) changes with temperature. Figure 4 .Depend on Figure 4 It can be seen that: Yb2ZrMo5O 20 Between room temperature and 403 K, the relative length increases with increasing temperature, and a phase transition occurs at 403 K. After that, in the temperature range of 403~773 K, the relative length decreases slightly with increasing temperature, and the linear expansion coefficient is -0.75×10 -6 K -1 ;Tm2ZrMo5O 20 Between room temperature and 463 K, the relative length increases with the increase of temperature. A phase transition occurs at 463 K. After that, in the temperature range of 463~773 K, the relative length tends to decrease. The linear expansion coefficient is -1.13×10 -6 K -1 ; Y2ZrMo5O 20 Between room temperature and 458 K, the relative length increases with increasing temperature. At 458 K, a phase transition occurs, and the relative length decreases with increasing temperature. In the temperature range of 458 to 773 K, the linear expansion coefficient is -1.79×10-6 K -1 According to the linear expansion coefficient after the above phase transition, it can be known that: Yb2ZrMo5O 20 and Tm2ZrMo5O 20 After the phase transition, Y2ZrMo5O exhibits near-zero expansion. 20 After the phase transition, it shows negative thermal expansion, that is, as the radius of the RE-site atom increases, RE2ZrMo5O 20 The negative expansion behavior is becoming more and more obvious, so not all RE-site atoms can obtain near-zero expansion materials.

Claims

1. A near-zero thermal expansion ceramic material, characterized in that: Its molecular formula is RE2ZrMo5O 20 , RE=Yb or Tm.

2. A method for preparing the near-zero thermal expansion ceramic material according to claim 1, characterized in that: Select RE source, Zr source and Mo source as raw materials, and according to the target product RE2ZrMo5O 20 The stoichiometric molar ratio of RE: Zr: Mo is 2: 1: 5, and the mixture is weighed and ground to mix evenly. The obtained mixed powder is directly sintered or sintered after tableting. The sintering temperature is 700-800 ° C, the time is 40-50 hours, and the mixture is cooled to room temperature to obtain the target product RE2ZrMo5O 20 ; Wherein, the RE source is RE2O3 or a precursor material that can be heated and decomposed at a temperature not higher than the sintering temperature to obtain RE2O3; RE2O3=Yb2O3 or Tm2O3; The Zr source is ZrO2 or a precursor material that can be heated and decomposed to obtain ZrO2 at a temperature not higher than the sintering temperature; The Mo source is MoO3 or a precursor material that can be heated and decomposed at a temperature not higher than the sintering temperature to obtain MoO3.

3. The method for preparing the near-zero thermal expansion ceramic material according to claim 2, characterized in that: After weighing the RE source, Zr source and Mo source in proportion and grinding and mixing them evenly, the obtained mixed powder is first pre-sintered directly or pre-sintered after tableting, and then the pre-sintered product is ground and mixed evenly, and then secondary sintered after tableting; the pre-sintering temperature is 300~400℃ and the time is 5~10h, and the secondary sintering temperature is 700~800℃ and the time is 40~50h.

4. The method for preparing the near-zero thermal expansion ceramic material according to claim 2 or 3, characterized in that: When the RE source, Zr source and Mo source are weighed in proportion and ground and mixed evenly, wet grinding is adopted, and ethanol is added during grinding, and the added amount is based on wetting the RE source, Zr source and Mo source.

5. The method for preparing the near-zero thermal expansion ceramic material according to claim 3, characterized in that: When the pre-sintered product is ground and mixed uniformly, dry grinding is adopted.

6. The method for preparing the near-zero thermal expansion ceramic material according to claim 2 or 3, characterized in that: The purity of RE source, Zr source and Mo source are all 99~99.99wt%.

7. The method for preparing the near-zero thermal expansion ceramic material according to claim 2 or 3, characterized in that: For all sintering processes involved, the temperature was raised to the sintering temperature at a heating rate of 3 to 10 °C / min.

8. The method for preparing the near-zero thermal expansion ceramic material according to claim 2 or 3, characterized in that: All tablets involved are pressed into cylindrical blanks with a diameter of 8~10mm and a height of 3~6mm.

9. The method for preparing the near-zero thermal expansion ceramic material according to claim 2 or 3, characterized in that: For all tablet pressing processes involved, the tablet pressing pressure is 4~10MPa and the pressure holding time is 2~5min.

Citation Information

Patent Citations

  • Molybdic acid rare earth-based medium / high-entropy ceramic material as well as preparation method and application thereof

    CN115286383A

  • Rare-earth-based molybdate high-entropy negative thermal expansion ceramic material and preparation method thereof

    CN115448717A

  • High-entropy zero thermal expansion material and preparation method thereof

    CN118109735A

  • Low temperature sinterable dielectric ceramic composition and multilayer ceramic chip capacitor using the same

    US20040106510A1

  • Ceramic sintered compact, circuit board using the same, electronic device and thermoelectric conversion module

    WO2011111746A1