Acrylate dielectric elastomer
By copolyacrylonitrile and perfluorodecyl acrylate in butyl acrylate and adding tert-butyl acrylate to prepare acrylate-based dielectric elastomer with high dielectric constant, the existing dielectric elastomer driving performance is solved and the The problem of poor material stability achieves the combination of high dielectric constant and low elastic modulus, improving driving performance and mechanical stability.
Patent Information
- Application Number
- CN202411304104.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-19
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-09-19
AI Technical Summary
In terms of driving performance, existing dielectric elastomers have problems such as high elastic modulus, low dielectric constant, sensitive temperature and humidity, and easy damage after reduced film thickness, resulting in degradation of driving performance and damage to material stability.
By copolying acrylonitrile and/or 1H,1H,2H-perfluorodecyl acrylate in butyl acrylate, high polar groups are introduced and tert-butyl acrylate is added to adjust the viscoelasticity, and the random copolymerization is performed. To prepare acrylate dielectric elastomers with high dielectric constants to avoid the problems of packing agglomeration and modulus reduction.
The high dielectric constant and low elastic modulus of the dielectric elastomer are achieved, which improves driving performance and mechanical stability, extends the service life of the material, and improves the durability of the driving voltage.
Smart Images

Figure CN119060264A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of dielectric elastomers, and specifically discloses an acrylic ester dielectric elastomer with high dielectric constant and low modulus. Background Art
[0002] Some polymers can change their shape and size in response to external stimuli (light, electric field, magnetic field, etc.), and electroactive polymers are one of the most widely studied. As the name suggests, electroactive polymers are polymer materials that can respond to an external electric field, and dielectric elastomers (DE) are a type of electroactive smart material that has attracted much attention. They can convert electrical signal input into mechanical energy output, and mechanical energy input into electrical energy output, and can efficiently achieve force-electricity conversion.
[0003] Dielectric elastomers have large deformation (>100%) and high energy density (>3.4MJ / m 3 ), fast response, similar to the natural muscles of the human body when deformed by force, and is often used as a material for making actuators. In practical applications, dielectric elastomer actuators are involved in the fields of bionics, biomedicine, and aerospace. Dielectric elastomers can be mainly divided into three categories according to the material: acrylates, silicone rubber, and polyurethane. However, acrylates still have some defects, such as slow creep recovery, which affects their drive recovery performance, large viscoelasticity, and high sensitivity to temperature and humidity. Compared with acrylates, silicone rubber dielectric elastomers have a wider operating temperature range and smaller viscoelastic hysteresis, but silicone rubber is a non-polar material with a relatively low dielectric constant (~2.8), which makes it relatively small when used as a dielectric elastomer actuator. At the same time, it also has a very low energy density (0.75J / cm 3 ). Therefore, in order to improve the driving performance of silicone rubber as a flexible actuator, a pre-strain of 50-150% is generally applied, and the pre-strain requires additional stretching devices. Although polyurethane elastomers have a higher dielectric constant (>7), breakdown strength and a certain thickness strain, compared with acrylates and silicone rubber, polyurethane has a higher Young's modulus. This defect will reduce its electric driving performance in flexible actuator applications, and it is more difficult to improve the electric driving strain performance by pre-stretching. Therefore, how to improve the driving performance of dielectric elastomers has always been a hot topic of research.
[0004] The main methods to improve the driving performance of dielectric elastomers are to reduce the elastic modulus and thickness of dielectric elastomers and to increase the dielectric constant and driving voltage of dielectric elastomers. However, when the applied electric field exceeds the maximum voltage that the material can withstand, the dielectric elastomer film will be damaged, resulting in driving failure.
[0005] Improving driving performance by reducing the elastic modulus often leads to changes in other properties of the film, such as viscosity loss, hysteresis, etc. Too low an elastic modulus will lead to a loss of mechanical stability and integrity of the elastomer, impairing the long-term performance and life of the material.
[0006] Reducing the film thickness can cause the material to undergo a larger driving strain at a smaller voltage. The reduction in film thickness is generally achieved through pre-stretching. In addition, pre-stretching can also rearrange the polymer molecular chains perpendicular to the direction of the applied electric field, thereby limiting the flow of charge and improving the dielectric strength. However, the main commercial dielectric elastomer VHB4910 currently requires a reinforced frame to maintain the pre-stretched state after pre-stretching, which will cause stress relaxation and fatigue. Although the interpenetrating polymer network structure can solve the problem of strengthening the frame, the thickness of the film produced on a large scale can only reach 10-20μm at most. If the thickness is further reduced, the unevenness of the film will increase, which will cause the film to be locally subjected to high electric fields and stresses, resulting in premature electrical breakdown.
[0007] Dielectric constant is one of the key parameters that determine the performance of dielectric elastomers, and the dielectric constants of existing polymer elastomer materials (such as natural rubber, silicone rubber, polyurethane elastomers, etc.) are relatively low. A common method to improve the dielectric constant is to add high dielectric constant or conductive fillers to the elastomer matrix in a liquid state. However, solid fillers will have the problem of agglomeration in the liquid elastomer matrix, which will lead to defects such as local stress concentration and a sharp increase in material modulus. Therefore, how to optimize the driving performance of dielectric elastomers is still a problem that needs further in-depth research. Summary of the invention
[0008] In order to overcome the above difficulties, the present invention copolymerizes polyacrylonitrile (AN) and / or 1H,1H,2H,2H-perfluorodecyl acrylate (PFOEA) in butyl acrylate (BA) by copolymerization, thereby introducing a high polar group to generate an acrylate dielectric elastomer with a high dielectric constant. At the same time, tert-butyl acrylate can also be copolymerized to adjust the viscoelasticity of the polymer. The acrylate dielectric elastomer of the present invention has excellent driving performance, low elastic modulus and other characteristics, so that it can be applied to fields such as electroactive drive.
[0009] To achieve the above object, the present invention is implemented through the following technical solutions:
[0010] The invention provides an acrylate dielectric elastomer, which is obtained by curing butyl acrylate, acrylonitrile and / or 1H,1H,2H,2H-perfluorodecyl acrylate as monomers and polyurethane diacrylate as a crosslinking agent under a photoinitiator.
[0011] Preferably, tert-butyl acrylate or a short-chain crosslinking agent is further added to the above-mentioned acrylic dielectric elastomer.
[0012] Furthermore, in the above-mentioned acrylate dielectric elastomer, the short-chain crosslinking agent is selected from hexylene glycol diacrylate (HDDA), neopentyl glycol diacrylate (PNPDA) or polyethylene glycol diacrylate (PEGDA).
[0013] Specifically, in the above-mentioned acrylate dielectric elastomer, the polyurethane diacrylate is selected from CN9021NS, CN9893NS or CN9014NS, preferably CN9021NS.
[0014] Specifically, in the above-mentioned acrylic dielectric elastomer, the photoinitiator is 2,2-dimethoxy-2-phenylacetophenone (DMPA), 2-hydroxy-2-methylpropiophenone, benzophenone (BP), or a combination of benzophenone (BP) and 2,2-dimethoxy-2-phenylacetophenone (DMPA). Preferably, the combination of benzophenone (BP) and 2,2-dimethoxy-2-phenylacetophenone (DMPA) is 1:1 in mass ratio.
[0015] Specifically, in the above-mentioned acrylic ester dielectric elastomer, when the monomer raw materials are butyl acrylate and acrylonitrile or 1H,1H,2H,2H-perfluorodecyl acrylate, in terms of molar percentage, butyl acrylate: acrylonitrile or 1H,1H,2H,2H-perfluorodecyl acrylate = 60-90%: 10-40%. Preferably, it is 85%: 15%, 80%: 20%, 70%: 30% or 60%: 40%. More preferably, it is 80%: 20%.
[0016] Specifically, in the above-mentioned acrylic dielectric elastomer, when the monomer raw materials are butyl acrylate, tert-butyl acrylate, and acrylonitrile, in terms of molar percentage, butyl acrylate: tert-butyl acrylate: acrylonitrile = 30-50%: 30-50%: 20%. Preferably, it is 32%: 48%: 20%, 40%: 40%: 20%, or 48%: 32%: 20%. More preferably, it is 40%: 40%: 20%.
[0017] Specifically, in the above-mentioned acrylic dielectric elastomer, when the monomer raw materials are butyl acrylate, tert-butyl acrylate, and 1H,1H,2H,2H-perfluorodecyl acrylate, in terms of molar percentage, butyl acrylate: tert-butyl acrylate: 1H,1H,2H,2H-perfluorodecyl acrylate = 35-45%: 35-45%: 10-30%. Preferably, it is 45%: 45%: 10%, 40%: 40%: 20%, or 35%: 35%: 30%. More preferably, it is 40%: 40%: 20%.
[0018] Specifically, in the above-mentioned acrylic dielectric elastomer, when the monomer raw materials are butyl acrylate, tert-butyl acrylate, acrylonitrile and 1H,1H,2H,2H-perfluorodecyl acrylate, in terms of molar percentage, butyl acrylate: tert-butyl acrylate: acrylonitrile: 1H,1H,2H,2H-perfluorodecyl acrylate = 40%: 40%: 5-15%: 5-15%. Preferably, it is 40%: 40%: 6%: 14% or 40%: 40%: 8%: 12%. More preferably, it is 40%: 40%: 8%: 12%.
[0019] Preferably, in the above-mentioned acrylic dielectric elastomer, the amount of the photoinitiator added is 0.5-2wt% of the precursor solution, and the precursor solution is the sum of the monomers, the crosslinking agent and the photoinitiator, preferably 1wt%.
[0020] Preferably, in the acrylic dielectric elastomer, the crosslinking agent is added in an amount such that the crosslinking density is 0.26%.
[0021] The present invention adopts butyl acrylate as a raw material, introduces a strong polar group cyano and / or fluorine group into its side chain, and further adds tert-butyl acrylate to adjust the viscoelasticity, thereby preparing a high dielectric constant butyl acrylate dielectric elastomer. The present invention adopts a random copolymerization method for cross-linking, avoids the problem of filler agglomeration caused by blending to improve the dielectric constant, and also avoids the problem of reducing the material modulus or film thickness method to improve the dielectric constant and causing other material properties to decrease. The acrylate dielectric elastomer of the present invention has an elastic modulus of 0.075-0.153MPa, an elongation at break of 1566%-1775%, and a dielectric constant of 7.48-11.8, and can be used as a functional material. The preferred product of the present invention has a better dielectric constant (11.8@1KHZ) and a lower Young's modulus (0.081MPa). BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 Stress-strain curves of Examples 1 and 2 and Comparative Examples 1 and 3;
[0023] Figure 2 Frequency dependence of dielectric constant of samples of Examples 1, 2 and Comparative Examples 1, 3;
[0024] Figure 3 Frequency dependence of dielectric constant of samples of Examples 5 and 6 and Comparative Examples 2 and 3;
[0025] Figure 4 Frequency dependence of dielectric constant of samples of Examples 7 and 8 and Comparative Examples 2 and 3;
[0026] Figure 5 Sample drive test of Examples 1, 2 and Comparative Examples 1, 3;
[0027] Figure 6 Driving performance test of samples of Examples 5 and 6 and Comparative Examples 2 and 3;
[0028] Figure 7 FT-IR analysis spectrum of the sample of Example 1;
[0029] Figure 8 Actual sample pictures, a is the sample in Example 1 placed above the scale and font, b is the landscape picture without the sample, and c is the landscape picture through the sample. DETAILED DESCRIPTION
[0030] The invention provides a novel high dielectric constant acrylic ester dielectric elastomer, which uses butyl acrylate and acrylonitrile and / or 1H,1H,2H,2H-perfluorodecyl acrylate as monomers and polyurethane diacrylate as a crosslinking agent, and is cured under a photoinitiator to obtain the acrylic ester dielectric elastomer.
[0031] In the present invention, tert-butyl acrylate or other short-chain crosslinking agents can also be added as monomers to adjust the viscosity and modulus of the polymer. The short-chain crosslinking agent is selected from hexylene glycol diacrylate (HDDA), neopentyl glycol diacrylate (PNPDA) or polyethylene glycol diacrylate (PEGDA).
[0032] In the present invention, the polyurethane diacrylate is selected from CN9021NS (number average molecular weight is 28000 g / mol), CN9893NS (number average molecular weight is 1600 g / mol) or CN9014NS (number average molecular weight is 6800 g / mol).
[0033] In the present invention, the photoinitiator is selected from 2,2-dimethoxy-2-phenylacetophenone (DMPA), 2-hydroxy-2-methylpropiophenone, benzophenone (BP), or a combination of benzophenone (BP) and 2,2-dimethoxy-2-phenylacetophenone (DMPA). Preferably, benzophenone (BP) and 2,2-dimethoxy-2-phenylacetophenone (DMPA) are used in a mass ratio of 1:1 to ensure that the film is fully cured.
[0034] In the present invention, the structural formula of butyl acrylate is as follows:
[0035]
[0036] In the present invention, the acrylonitrile structural formula is as follows:
[0037]
[0038] In the present invention, the structural formula of the 1H,1H,2H,2H-perfluorodecyl acrylate is as follows:
[0039]
[0040] In the present invention, the structural formula of CN9021NS is as follows:
[0041]
[0042]
[0043] Where: R1 = polyol, R2 = isocyanate. Preferably CN9021NS produced by Sartomer is used.
[0044] In the present invention, when the monomer raw materials are butyl acrylate and acrylonitrile or 1H,1H,2H,2H-perfluorodecyl acrylate, the butyl acrylate is 60-90%, and the acrylonitrile or 1H,1H,2H,2H-perfluorodecyl acrylate is 10-40% by mole percentage. Preferably, butyl acrylate is 85%, and acrylonitrile or 1H,1H,2H,2H-perfluorodecyl acrylate is 15%. Butyl acrylate is 80%, and acrylonitrile or 1H,1H,2H,2H-perfluorodecyl acrylate is 20%. Butyl acrylate is 70%, and acrylonitrile or 1H,1H,2H,2H-perfluorodecyl acrylate is 30%. Butyl acrylate is 60%, and acrylonitrile or 1H,1H,2H,2H-perfluorodecyl acrylate is 40%. More preferably, butyl acrylate is controlled at 80% and acrylonitrile or 1H,1H,2H,2H-perfluorodecyl acrylate is controlled at 20%. The prepared acrylic polymer has a higher dielectric constant and a lower elastic modulus.
[0045] In the present invention, when the monomer raw materials are butyl acrylate, tert-butyl acrylate and acrylonitrile, the molar percentage is 30-50% of butyl acrylate, 30-50% of tert-butyl acrylate and 20% of acrylonitrile. Preferably, 32% of butyl acrylate, 48% of tert-butyl acrylate and 20% of acrylonitrile. 40% of butyl acrylate, 40% of tert-butyl acrylate and 20% of acrylonitrile. 48% of butyl acrylate, 32% of tert-butyl acrylate and 20% of acrylonitrile. More preferably, 40% of butyl acrylate, 40% of tert-butyl acrylate and 20% of acrylonitrile are controlled, and the prepared acrylic polymer has a higher dielectric constant and a lower elastic modulus.
[0046] In the present invention, when the monomer raw materials are butyl acrylate, tert-butyl acrylate, and 1H,1H,2H,2H-perfluorodecyl acrylate, the molar percentage is 35-45% of butyl acrylate, 35-45% of tert-butyl acrylate, and 10-30% of 1H,1H,2H,2H-perfluorodecyl acrylate. Preferably, 45% of butyl acrylate, 45% of tert-butyl acrylate, and 10% of 1H,1H,2H,2H-perfluorodecyl acrylate. 40% of butyl acrylate, 40% of tert-butyl acrylate, and 20% of 1H,1H,2H,2H-perfluorodecyl acrylate. 35% of butyl acrylate, 35% of tert-butyl acrylate, and 30% of 1H,1H,2H,2H-perfluorodecyl acrylate. It is more preferred to control 40% of butyl acrylate, 40% of tert-butyl acrylate, and 20% of 1H,1H,2H,2H-perfluorodecyl acrylate. The prepared acrylic polymer has a higher dielectric constant and a lower elastic modulus.
[0047] In the present invention, when the monomer raw materials are butyl acrylate, tert-butyl acrylate, acrylonitrile and 1H,1H,2H,2H-perfluorodecyl acrylate, the molar percentage is 40% butyl acrylate, 40% tert-butyl acrylate, 5-15% acrylonitrile, and 5-15% 1H,1H,2H,2H-perfluorodecyl acrylate. Preferably, 40% butyl acrylate, 40% tert-butyl acrylate, 6% acrylonitrile, and 14% 1H,1H,2H,2H-perfluorodecyl acrylate. 40% butyl acrylate, 40% tert-butyl acrylate, 8% acrylonitrile, and 12% 1H,1H,2H,2H-perfluorodecyl acrylate. More preferably, 40% butyl acrylate, 40% tert-butyl acrylate, 8% acrylonitrile, and 12% 1H,1H,2H,2H-perfluorodecyl acrylate are controlled, and the prepared acrylic polymer has a higher dielectric constant and a lower elastic modulus.
[0048] In the present invention, the above-mentioned monomer raw materials, photoinitiator and cross-linking agent are added in proportion and then cured by a conventional method in the art to obtain the acrylic dielectric elastomer.
[0049] The specific implementation modes of the present invention are further described below.
[0050] In the examples, CN9021NS was purchased from Sartomer, butyl acrylate, tert-butyl acrylate and benzophenone were purchased from Aladdin, acrylonitrile and 1H,1H,2H,2H-perfluorodecyl acrylate were purchased from MacLean Reagent, and 2,2-dimethoxy-2-phenylacetophenone was purchased from Sigma Aldrich.
[0051] Example 1
[0052] Weigh 3.5g CN9021NS with an analytical balance and calculate the total molar amount of the comonomers with a crosslink density of 0.26% (referring to the ratio of the total number of double bond functional groups of the comonomers to the number of double bond functional groups of the crosslinking agent. The crosslinking agent CN9021NS is difunctional, and the total molar amount of the comonomers is calculated by the ratio of double molar amount of the crosslinking agent to the crosslink density. The amount of crosslinking agent substance: 3.5 / 28000=0.000125mol, CN9021NS is difunctional: 0.000125*2=0.00025mol, the total molar amount of the comonomers: 0.00025 / 0.26%=0.09615mol). Weigh 85% of the total molar amount of butyl acrylate, 15% of the total molar amount of acrylonitrile (PBA 0.85 -AN 0.15 ), and then add 1% of benzophenone and 2,2-dimethoxy-2-phenylacetophenone as photoinitiator. The solution was mixed in a beaker and stirred at 500 rpm for 30 minutes as a precursor solution.
[0053] After the precursor solution was vacuum degassed for 15 minutes, an appropriate amount of the precursor solution was taken on an optical glass sheet, and the thickness of the prepared polymer film was determined by a spacer, and a cover glass was placed on the solution. After that, it was cured for 20 minutes under a UV light source with a power of 250W and a wavelength of 480nm, and the obtained sample was placed in a vacuum oven at 40°C for 24 hours to remove residual monomers. After demolding, a high dielectric constant acrylic dielectric elastomer was obtained.
[0054] Example 2
[0055] Compared with Example 1, the difference is that 80% (70%, 60%) of the total molar amount of butyl acrylate and 20% (30%, 40%) of the total molar amount of acrylonitrile (PBA 0.8 -AN 0.2 ). The curing conditions are the same as those in Example 1.
[0056] Example 3
[0057] Weigh 3.5g CN9021NS with an analytical balance and calculate the total molar amount of the comonomers with a crosslink density of 0.26%. Weigh 32% of the total molar amount of butyl acrylate, 48% of the total molar amount of tert-butyl acrylate, and 20% of the total molar amount of acrylonitrile, and then add 1% of each of benzophenone and 2,2-dimethoxy-2-phenylacetophenone photoinitiator. Mix the solution in a beaker and stir at 500rpm for 30min as a precursor solution. The curing conditions are the same as in Example 1.
[0058] Example 4
[0059] Compared with Example 3, the difference is that 40% (48%) of the total molar amount of butyl acrylate, 40% (32%) of the total molar amount of tert-butyl acrylate, and 20% of the total molar amount of acrylonitrile are weighed. The curing conditions are the same as those of Example 1.
[0060] Example 5
[0061] Weigh 1.765g CN9021NS with an analytical balance, and calculate the total molar amount of the comonomers with a crosslink density of 0.26%. Weigh 45% molar amount of butyl acrylate, 45% molar amount of tert-butyl acrylate, 10% molar amount of 1H,1H,2H,2H-perfluorodecyl acrylate, and add 1% of each of benzophenone and 2,2-dimethoxy-2-phenylacetophenone photoinitiator. Mix the solution in a beaker and stir at 500rpm for 30min as a precursor solution. The curing conditions are the same as in Example 1.
[0062] Example 6
[0063] Compared with Example 5, the difference is that 40% (35%) of the total molar amount of butyl acrylate, 40% (35%) of the total molar amount of tert-butyl acrylate, and 20% (30%) of the total molar amount of 1H,1H,2H,2H-perfluorodecyl acrylate are weighed. The curing conditions are the same as those of Example 1.
[0064] Example 7
[0065] Weigh 1.765g CN9021NS with an analytical balance, and calculate the total molar amount of the comonomers with a crosslink density of 0.26%. Weigh 40% molar amount of butyl acrylate, 40% molar amount of tert-butyl acrylate, 6% molar amount of acrylonitrile, 14% molar amount of 1H,1H,2H,2H-perfluorodecyl acrylate, and add 1% of each of benzophenone and 2,2-dimethoxy-2-phenylacetophenone photoinitiator. Mix the solution in a beaker and stir at 500rpm for 30min as a precursor solution. The curing conditions are the same as in Example 1.
[0066] Example 8
[0067] Compared with Example 7, the difference is that 8 mol% of acrylonitrile and 12 mol% of 1H,1H,2H,2H-perfluorodecyl acrylate are weighed. The curing conditions are the same as those of Example 1.
[0068] Comparative Example 1
[0069] Compared with Example 1, the difference is that the monomer is only butyl acrylate, there is no comonomer, and the crosslinking density is still 0.26%. The curing conditions are the same as in Example 1.
[0070] Comparative Example 2
[0071] Compared with Example 5, the difference is that the monomers are butyl acrylate and tert-butyl acrylate, and the crosslinking density is still 0.26%. The curing conditions are the same as in Example 1.
[0072] Comparative Example 3
[0073] This comparative example is VHB4910 commercial adhesive tape purchased from 3M Company of the United States.
[0074] Dielectric property test: measured using a Keysight E4980AL impedance analyzer, with a sample thickness of 1 mm and an electrode having a diameter of 10 mm.
[0075] Mechanical properties test: The stress-strain curve was tested using a universal testing machine of the company TestStar ETM102B, and the Young's modulus was measured from the stress-strain curve. The samples were made into dumbbell-shaped specimens according to ISO 37-2005 standard.
[0076] from Figure 1 It can be seen that the PBA-AN (Examples 1 and 2) series has relatively excellent elongation at break and relatively satisfactory tensile strength, which can meet the pre-stretching test of the sample.
[0077] The dielectric constant and dielectric loss of each sample in Examples 1 and 2 measured at 50 KHz are shown in Table 1 below.
[0078] Table 1
[0079]
[0080] It can be seen from Table 1 that the dielectric constants in Examples 1 and 2 of the present invention are greatly improved compared with those in the comparative example, thereby proving that the acrylic dielectric elastomer of the present invention has a high dielectric constant.
[0081] from Figure 3 It can be seen that the samples of Examples 5 and 6 of the present invention have a significant improvement in dielectric constant compared to the commercial VHB4910 and the sample in Comparative Example 2. This shows that the present invention improves the problem of low dielectric constant of acrylic dielectric elastomers and is of great help in improving the driving performance of acrylic dielectric elastomers.
[0082] Depend on Figure 4 It can be seen that the samples of Examples 7 and 8 are of great help in improving the dielectric constant of acrylic dielectric elastomers, solving the problem of low dielectric constant of acrylic dielectric elastomers. In addition, compared with the sample in Example 6, the dielectric constant of the sample is greatly improved after the introduction of acrylonitrile.
[0083] from Figure 5It can be seen that under the same electric field strength, the PBA-AN series has better driving ability than VHB4910 and PBA, which proves that the present invention can solve the problem that the dielectric constant of acrylic dielectric elastomers is low and the driving voltage required is high.
[0084] Depend on Figure 6 It can be seen that the addition of tert-butyl acrylate and 1H,1H,2H,2H-perfluorodecyl acrylate appropriately increases the elastic modulus of the sample, thereby greatly improving the breakdown voltage. At the same time, the driving ability of the sample is greatly improved compared with the commercial VHB4910 and comparative example 2. It can be seen that Examples 5 and 6 improve the problems of poor driving performance and high driving voltage of acrylic dielectric elastomers.
[0085] Figure 8 The following are the actual pictures of the samples. a is the sample in Example 1 placed above the scale and font, b is the landscape picture without the sample, and c is the landscape picture through the sample. It can be seen from the above pictures that the PBA-AN series has good transparency.
Claims
1. An acrylic dielectric elastomer, characterized in that: The acrylate dielectric elastomer is obtained by using butyl acrylate, acrylonitrile and / or 1H,1H,2H,2H-perfluorodecyl acrylate as monomers and polyurethane diacrylate as a crosslinking agent and curing under a photoinitiator.
2. The acrylic dielectric elastomer according to claim 1, characterized in that: Tert-butyl acrylate or a short-chain crosslinking agent is also added; further, the short-chain crosslinking agent is selected from hexylene glycol diacrylate, neopentyl glycol diacrylate or polyethylene glycol diacrylate.
3. The acrylic dielectric elastomer according to claim 1 or 2, characterized in that: The polyurethane diacrylate is selected from CN9021NS, CN9893NS or CN9014NS, preferably CN9021NS.
4. The acrylic dielectric elastomer according to any one of claims 1 to 3, characterized in that: The photoinitiator is selected from 2,2-dimethoxy-2-phenylacetophenone, 2-hydroxy-2-methylpropiophenone, benzophenone, or a combination of benzophenone and 2,2-dimethoxy-2-phenylacetophenone; preferably a combination of benzophenone and 2,2-dimethoxy-2-phenylacetophenone.
5. The acrylic dielectric elastomer according to any one of claims 1 to 4, characterized in that: When the raw materials are butyl acrylate and acrylonitrile or 1H,1H,2H,2H-perfluorodecyl acrylate, in molar percentage, butyl acrylate: acrylonitrile or 1H,1H,2H,2H-perfluorodecyl acrylate = 60-90%: 10-40%; preferably 85%: 15%, 80%: 20%, 70%: 30% or 60%: 40%; more preferably 80%: 20%.
6. The acrylic dielectric elastomer according to any one of claims 1 to 4, characterized in that: When the raw materials are butyl acrylate, tert-butyl acrylate and acrylonitrile, in molar percentage, butyl acrylate: tert-butyl acrylate: acrylonitrile = 30-50%: 30-50%: 20%; preferably 32%: 48%: 20%, 40%: 40%: 20% or 48%: 32%: 20%; more preferably 40%: 40%: 20%.
7. The acrylic dielectric elastomer according to any one of claims 1 to 4, characterized in that: When the raw materials are butyl acrylate, tert-butyl acrylate, and 1H,1H,2H,2H-perfluorodecyl acrylate, in molar percentage, butyl acrylate: tert-butyl acrylate: 1H,1H,2H,2H-perfluorodecyl acrylate = 35-45%: 35-45%: 10-30%; preferably 45%: 45%: 10%, 40%: 40%: 20% or 35%: 35%: 30%; more preferably 40%: 40%: 20%.
8. The acrylic dielectric elastomer according to any one of claims 1 to 4, characterized in that: When the raw materials are butyl acrylate, tert-butyl acrylate, acrylonitrile and 1H,1H,2H,2H-perfluorodecyl acrylate, in molar percentage, butyl acrylate:tert-butyl acrylate:acrylonitrile:1H,1H,2H,2H-perfluorodecyl acrylate=40%:40%:5-15%:5-15%; preferably 40%:40%:6%:14% or 40%:40%:8%:12%; more preferably 40%:40%:8%:12%.
9. The acrylic dielectric elastomer according to any one of claims 1 to 8, characterized in that: The amount of the photoinitiator added is 0.5-2 wt % of the precursor solution, and the precursor solution is the sum of the monomers, the crosslinking agent and the photoinitiator; preferably 1 wt %.
10. The acrylic dielectric elastomer according to any one of claims 1 to 9, characterized in that: The crosslinking agent was added in an amount such that the crosslinking density was 0.26%.
Citation Information
Patent Citations
High dielectric constant and low-modulus dielectric elastomer material and preparation method thereof
CN101899177A
Acrylate dielectric elastomer and preparation method thereof
CN112375183A
Dielectric elastomer material and transducer using the same
JP2018059042A
Polymer, elastomer, production method therefor, actuator, and sensor
TW202328238A
Dielectric elastomeric material
US20220135711A1
Cited By
A phase-separated fluorinated polyacrylate dielectric elastomer and preparation method and application