Starch-based degradable composite material and preparation method thereof

By using thermoplastic starch, modified microspheres and hyperbranched macromolecular structural additives, the problem of insufficient mechanical properties and water resistance of starch-based plastics is solved, its flame retardancy and antibacterial properties are improved, and the application scope is expanded.

CN119060417AInactive Publication Date: 2024-12-03TAIZHOU HUANGYAN ZEYU NEW MATERIAL TECH CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411580137.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-11-07
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Starch-based plastics have poor mechanical properties and water resistance, insufficient flame retardancy, and there are degradation in mechanical properties and additive precipitation when used in aqueous environments, which limits its application scope and is difficult to effectively improve its antibacterial properties in the prior art. and weather resistance.

Method used

The starch-based degradable composite materials are prepared by stirring and twin-screw extruder processing, and use hyperbranched macromolecules. The additives of the structure, including quaternary ammonium salts, hindered phenols and sulfide groups, enhance their antibacterial and weathering resistance, and enhance their flame retardancy by introducing DOPO modified microspheres.

Benefits of technology

It significantly improves the mechanical properties, water resistance and flame retardancy of starch-based composite materials, imparts good antibacterial and weather resistance, and expands its use range.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a starch-based degradable composite material and a preparation method thereof, and relates to the technical field of high polymer material preparation, the starch-based degradable composite material comprises the following raw materials by weight: 55-65 parts of thermoplastic starch, 1.1-1.5 parts of modified microspheres, 18-22 parts of glycerin, 25-35 parts of polyhydroxyalkanoate, 3-5 parts of a coupling agent, 15-20 parts of talcum powder, and 1.5-2.0 parts of an auxiliary agent. The synthesized auxiliary agent is a compound with a hyperbranched macromolecular structure and comprises quaternary ammonium salt, hindered phenol and thioether, so that the composite material has stable antibacterial property and weather resistance. The synthesized modified microspheres are obtained by introducing carboxyl and DOPO into the surfaces of polyvinyl alcohol microspheres, so that the starch-based composite material has better mechanical properties, water resistance and flame retardance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of polymer material preparation, and in particular to a starch-based degradable composite material and a preparation method thereof. Background Art

[0002] One of the current development trends is to vigorously develop bio-based and biodegradable plastics and reduce the use of petroleum-based plastics. Starch has the advantages of being widely available, renewable, biodegradable, and inexpensive. Starch-based plastics possess the advantages of both being bio-based and biodegradable, so starch-based composites have been widely researched.

[0003] However, the mechanical properties of starch-based plastics are significantly inferior and cannot meet the requirements of use. Furthermore, starch itself has very strong water absorption, resulting in poor water resistance. Long-term use in environments with high water content can lead to adverse phenomena such as decreased mechanical properties and additive precipitation, which severely limits the scope of use of starch-based plastics. Previous studies have used polyvinyl alcohol microspheres to enhance the mechanical properties and water resistance of starch-based composites. However, polyvinyl alcohol microspheres are not flame retardant, and starch itself has insufficient flame retardant properties. Therefore, the flame retardancy of polyvinyl alcohol microsphere-enhanced starch-based composites cannot meet the requirements of use.

[0004] Furthermore, existing technologies have been used to enhance the weather resistance of starch-based composite materials by directly adding additives such as antioxidants and UV inhibitors. However, the weather resistance of starch-based composite materials still needs to be improved. Starch-based composite materials are widely used in food packaging materials, so the antibacterial properties of starch-based composite materials have been put forward higher requirements.

[0005] Therefore, it is important and necessary to develop a suitable modification method to improve the flame retardancy, weather resistance and antibacterial properties of polyvinyl alcohol microspheres reinforced starch-based composites, so as to obtain starch-based composites with better performance and expand their scope of application. Summary of the Invention

[0006] In order to solve the above technical problems, the present invention provides a starch-based degradable composite material and a preparation method thereof.

[0007] The purpose of the present invention can be achieved through the following technical solutions: A starch-based biodegradable composite material comprises the following raw materials in parts by weight: 55-65 parts of thermoplastic starch, 1.1-1.5 parts of modified microspheres, 18-22 parts of glycerol, 25-35 parts of polyhydroxyalkanoate, 3-5 parts of a coupling agent, 15-20 parts of talc, and 1.5-2.0 parts of an additive; the polyhydroxyalkanoate is polyhydroxybutyrate; and the coupling agent is KH560. The preparation of the starch-based degradable composite material comprises the following steps: Step S1: After stirring and mixing thermoplastic starch, modified microspheres, polyhydroxyalkanoate, coupling agent, and talc for 15-20 minutes, glycerol and auxiliary agents are added, and stirring is carried out at a speed of 100-200 r / min for 4-6 minutes to obtain a mixture; Step S2: adding the obtained mixture into a twin-screw extruder, melting, extruding and granulating at 200-300 r / min and 110-120° C. to obtain pellets, and then injection molding and forming the pellets to obtain a starch-based biodegradable composite material, with an injection molding pressure of 60-65 MPa and an injection molding machine temperature of 125-135° C.

[0008] The preparation of the auxiliary agent comprises the following steps: Step A1: Triallylamine is added to ethanol, and chloroalkane is added with stirring. The mixture is stirred at 50-60°C for 10-12 hours to obtain a quaternary ammonium salt product. The quaternary ammonium salt product is added to dichloromethane, and 3-chloroperoxybenzoic acid is added with stirring. The mixture is stirred at room temperature for 4-5 hours to obtain the epoxy product 1. Furthermore, the dosage ratio of triallylamine, ethanol, and chloroalkane is 0.1-0.15 mol: 50-60 mL: 0.1-0.15 mol, the chloroalkane is selected from one of 1-chlorobutane, 1-chlorohexane, and 1-chlorooctane, and the volume fraction of ethanol is 95%; the dosage ratio of the quaternary ammonium salt product, dichloromethane, and 3-chloroperoxybenzoic acid is 20-30 g: 80-90 mL: 18-20 g; During the reaction of step A1, the tertiary amine of triallylamine reacts with the chlorine atom of the chloroalkane to generate a quaternary ammonium salt product containing a carbon-carbon double bond; the three carbon-carbon double bonds of the quaternary ammonium salt product are all oxidized to epoxy groups to obtain epoxy product 1; Step A2: Under a protective gas atmosphere, add the thioether-containing carboxylic acid to toluene, add pyridine while stirring, and heat to 40-50°C. Then add the epoxy product 1, stir and react for 8-10 hours, then heat to 110-120°C and stir for 1-2 hours to obtain the hydroxyl product; Furthermore, the amount ratio of the thioether-containing carboxylic acid, toluene, pyridine, and epoxidized product 1 is 0.3-0.4 mol: 180-200 mL: 0.03-0.04 mol: 22-28 g, and the thioether-containing carboxylic acid is selected from one of 3-methylthiopropionic acid, 3-(benzylthio)propionic acid, and 3-(butylmercapto)propionic acid; During the reaction of step A2, the carboxyl group of the thioether-containing carboxylic acid reacts with the epoxy group of the epoxy product to form a hydroxyl product containing a thioether group and multiple hydroxyl groups; Step A3: Add a cyano-containing hindered phenol to tetrahydrofuran, add Raney nickel and Pd / C with stirring, introduce hydrogen, and react with stirring at normal pressure for 48-50 hours to obtain an amino product; add epichlorohydrin, the amino product, and tetrabutylammonium bromide to toluene, reflux and stir at 100-110°C for 3-4 hours, cool to room temperature, add sodium hydroxide solution, and stir for 5-6 hours to obtain the epoxy product 2; Furthermore, the amount ratio of the cyano-containing hindered phenol, tetrahydrofuran, Raney nickel, and Pd / C is 0.1-0.15 mol: 60-70 mL: 0.02-0.03 mol: 0.02-0.025 mol, the cyano-containing hindered phenol is selected from one of 3,5-di-tert-butyl-4-hydroxybenzonitrile and 3,5-di-tert-butyl-4-hydroxyphenylacetonitrile; the amount ratio of epichlorohydrin, amino product, tetrabutylammonium bromide, toluene, and sodium hydroxide solution is 22-24 g: 26-28 g: 0.05-0.08 mol: 90-100 mL: 20-25 mL; the mass fraction of the sodium hydroxide solution is 40-50%; During the reaction of step A3, the cyano group of the cyano-containing hindered phenol is reduced to an amino group to obtain an amino product; the amino group of the amino product is ring-opened and then ring-closed with epichlorohydrin to form two epoxy groups to obtain an epoxy product 2 containing a hindered phenol; Step A4: Add the epoxy product 2 and the hydroxyl product to methanol, start stirring, then add trimethylamine, and reflux and stir at 110-120°C for 6-7 hours to obtain the auxiliary agent; Furthermore, the usage ratio of the epoxy product 2, the hydroxyl product, methanol, and trimethylamine is 30-34 g: 24-30 g: 120-130 mL: 0.03-0.05 mol; During the reaction of step A4, the epoxy group of the epoxy product 2 reacts with the hydroxyl group of the hydroxyl product to generate an auxiliary agent having a hyperbranched macromolecular structure containing a quaternary ammonium salt, a hindered phenol and a thioether.

[0009] The preparation of the modified microspheres comprises the following steps: Step B1: Add Span 40 to n-heptane, mix and stir, and heat to 60-65°C. Add polyvinyl alcohol solution and hydrochloric acid dropwise, stir for 1-1.5 hours, add glutaraldehyde, and keep at 60-65°C for 2-2.5 hours. Wash and dry to obtain polyvinyl alcohol microspheres. Furthermore, the usage ratio of Span 40, n-heptane, polyvinyl alcohol solution, hydrochloric acid, and glutaraldehyde is 0.6-0.65 g: 45-50 mL: 25-30 mL: 2-2.5 mL: 5-6 mL, and the polyvinyl alcohol solution is prepared by adding 5-7 g of polyvinyl alcohol to 100-110 mL of deionized water and stirring for 5-10 minutes; During the reaction of step B1, polyvinyl alcohol microspheres are prepared by a reverse suspension cross-linking method; Step B2: Add polyvinyl alcohol microspheres to ethyl acetate, add maleic anhydride and a catalyst while stirring, and react at 80-90°C with constant stirring for 3.5-4.5 hours. After washing and vacuum drying, microspheres containing unsaturated carboxyl groups on the surface are obtained; Furthermore, the usage ratio of polyvinyl alcohol microspheres, ethyl acetate, maleic anhydride and catalyst is 5-7 g:80-90 mL:0.5-1.0 g:0.1-0.15 g, and the catalyst is 4-dimethylaminopyridine; During the reaction of step B2, the hydroxyl groups on the surface of the polyvinyl alcohol microspheres react with maleic anhydride to obtain microspheres containing unsaturated carboxyl groups on the surface; Step B3: In a nitrogen atmosphere, DOPO and microspheres containing unsaturated carboxyl groups on the surface are added to DMF, and the mixture is stirred at 90-110°C for 8-10 hours. After cooling to room temperature, the mixture is recrystallized in an ice-water bath and filtered under reduced pressure to obtain modified microspheres. Furthermore, the usage ratio of DOPO, microspheres containing unsaturated carboxyl groups on the surface, and DMF is 11-13 g: 6-9 g: 80-100 mL; During the reaction of step B3, DOPO adds to the carbon-carbon double bonds of the microspheres containing unsaturated carboxyl groups on the surface to obtain modified microspheres containing DOPO.

[0010] Beneficial effects of the present invention: The present invention discloses a starch-based degradable composite material, comprising the following raw materials: thermoplastic starch, modified microspheres, glycerol, polyhydroxyalkanoate, a coupling agent, talc, and an additive. The additive is a compound with a hyperbranched macromolecular structure, comprising a quaternary ammonium salt, a hindered phenol, and a thioether group; when bacteria come into contact with the starch-based degradable composite material containing a quaternary ammonium salt, the negatively charged bacteria will be attracted by the cations on its surface, resulting in the bacteria's freedom of movement being constrained, inhibiting the bacteria's respiratory function and imparting antibacterial properties to the composite material; the hindered phenol can terminate the chain reaction of peroxyl radicals participating in oxidative degradation, thereby avoiding oxidative degradation of the composite material, while the thioether group can reduce and decompose hydroperoxides, making up for the deficiency of the hindered phenol, and the hindered phenol and thioether group produce intramolecular synergistic effects, significantly improving the weather resistance of the composite material; the hyperbranched macromolecular structure formed by the quaternary ammonium salt, hindered phenol, and thioether group can avoid the migration and failure of small molecule antibacterial agents and antioxidants in the high molecular polymer matrix, and the additive enables the composite material to have stable antibacterial and weather resistance.

[0011] The modified microspheres are obtained by introducing carboxyl groups and DOPO into the surface of polyvinyl alcohol microspheres; the carboxyl groups enhance the bonding strength between the polyvinyl alcohol microspheres and the starch matrix, and the modified microspheres improve the mechanical properties and water resistance of the composite material; when the DOPO burns, the surface of the high molecular polymer is dehydrated and degraded to form a carbon layer, and the phosphorus-containing derivatives produced simultaneously cover the polymer surface, isolating the transfer of combustible gas and heat, and preventing further combustion. The grafting of DOPO onto the surface of the polyvinyl alcohol microspheres not only imparts flame retardancy to the modified microspheres, but also helps to improve the flame retardancy of the starch-based composite material; therefore, the modified microspheres give the starch-based composite material better mechanical properties, water resistance and flame retardancy. DETAILED DESCRIPTION

[0012] The following is a clear and complete description of the technical solutions in the embodiments of the present invention. Obviously, the embodiments described are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making any creative efforts are within the scope of protection of the present invention.

[0013] Example 1 An auxiliary agent, the preparation of which comprises the following steps: Step A1: Triallylamine is added to ethanol, and chloroalkane is added with stirring. The mixture is stirred and reacted at 50°C for 10 hours to obtain a quaternary ammonium salt product. The quaternary ammonium salt product is added to dichloromethane, and 3-chloroperoxybenzoic acid is added with stirring. The mixture is stirred and reacted at room temperature for 4 hours to obtain the epoxy product 1. The amount ratio of triallylamine, ethanol, and chloroalkane is 0.1 mol:50 mL:0.1 mol, the chloroalkane is 1-chlorobutane, and the volume fraction of ethanol is 95%. The amount ratio of the quaternary ammonium salt product, dichloromethane, and 3-chloroperoxybenzoic acid is 20 g:80 mL:18 g. Step A2: Under a nitrogen atmosphere, a thioether-containing carboxylic acid was added to toluene, pyridine was added with stirring, and the temperature was raised to 40°C. The epoxy product 1 was then added and stirred for 8 hours. The temperature was then raised to 110°C and stirred for 1 hour to obtain a hydroxyl product. The amount ratio of the thioether-containing carboxylic acid, toluene, pyridine, and epoxy product 1 was 0.3 mol:180 mL:0.03 mol:22 g. The thioether-containing carboxylic acid was 3-methylthiopropionic acid. Step A3: Add a cyano-containing hindered phenol to tetrahydrofuran, add Raney nickel and Pd / C with stirring, introduce hydrogen, and react with stirring at normal pressure for 48 hours to obtain an amino product; add epichlorohydrin, the amino product, and tetrabutylammonium bromide to toluene, reflux and stir at 100°C for 3 hours, cool to room temperature, add sodium hydroxide solution, and stir for 5 hours to obtain an epoxy product 2; the amount ratio of the cyano-containing hindered phenol, tetrahydrofuran, Raney nickel, and Pd / C is 0.1 mol:60 mL:0.02 mol:0.02 mol, and the cyano-containing hindered phenol is 3,5-di-tert-butyl-4-hydroxybenzonitrile; the amount ratio of epichlorohydrin, the amino product, tetrabutylammonium bromide, toluene, and sodium hydroxide solution is 22 g:26 g:0.05 mol:90 mL:20 mL; the mass fraction of the sodium hydroxide solution is 50%; Step A4: Add the epoxy product 2 and the hydroxyl product to methanol, start stirring, then add trimethylamine, and reflux and stir at 110°C for 6 hours to obtain the auxiliary agent; the amount ratio of the epoxy product 2, the hydroxyl product, methanol, and trimethylamine is 30g:24g:120mL:0.03mol.

[0014] Example 2 An auxiliary agent, the preparation of which comprises the following steps: Step A1: Triallylamine was added to ethanol, and chloroalkane was added with stirring. The mixture was stirred at 55°C for 11 hours to obtain a quaternary ammonium salt product. The quaternary ammonium salt product was added to dichloromethane, and 3-chloroperoxybenzoic acid was added with stirring. The mixture was stirred at room temperature for 4.5 hours to obtain the epoxy product 1. The amount ratio of triallylamine, ethanol, and chloroalkane was 0.13 mol:55 mL:0.13 mol, the chloroalkane was 1-chlorohexane, and the volume fraction of ethanol was 95%. The amount ratio of the quaternary ammonium salt product, dichloromethane, and 3-chloroperoxybenzoic acid was 25 g:85 mL:19 g. Step A2: Under a nitrogen atmosphere, a thioether-containing carboxylic acid was added to toluene, pyridine was added with stirring, and the temperature was raised to 45°C. Then, the epoxy product 1 was added and stirred for 9 hours. The temperature was then raised to 115°C and stirred for 1.5 hours to obtain a hydroxyl product. The amount ratio of the thioether-containing carboxylic acid, toluene, pyridine, and epoxy product 1 was 0.35 mol:190 mL:0.035 mol:25 g. The thioether-containing carboxylic acid was 3-(benzylthio)propionic acid. Step A3: Add a cyano-containing hindered phenol to tetrahydrofuran, add Raney nickel and Pd / C with stirring, introduce hydrogen, and react under stirring at normal pressure for 49 hours to obtain an amino product; add epichlorohydrin, the amino product, and tetrabutylammonium bromide to toluene, reflux and stir at 105°C for 3.5 hours, cool to room temperature, add sodium hydroxide solution, and stir for 5.5 hours to obtain an epoxy product 2; the amount ratio of the cyano-containing hindered phenol, tetrahydrofuran, Raney nickel, and Pd / C is 0.3 mol:65 mL:0.025 mol:0.023 mol, and the cyano-containing hindered phenol is 3,5-di-tert-butyl-4-hydroxybenzonitrile; the amount ratio of epichlorohydrin, the amino product, tetrabutylammonium bromide, toluene, and sodium hydroxide solution is 23 g:27 g:0.06 mol:95 mL:23 mL; the mass fraction of the sodium hydroxide solution is 45%; Step A4: Add the epoxy product 2 and the hydroxyl product to methanol, start stirring, then add trimethylamine, and reflux and stir at 115°C for 6.5 hours to obtain the auxiliary agent; the amount ratio of the epoxy product 2, the hydroxyl product, methanol, and trimethylamine is 32g:27g:125mL:0.04mol.

[0015] Example 3 An auxiliary agent, the preparation of which comprises the following steps: Step A1: Triallylamine is added to ethanol, and chloroalkane is added with stirring. The mixture is stirred and reacted at 60°C for 12 hours to obtain a quaternary ammonium salt product; the quaternary ammonium salt product is added to dichloromethane, and 3-chloroperoxybenzoic acid is added with stirring. The mixture is stirred and reacted at room temperature for 5 hours to obtain the epoxy product 1; the amount ratio of triallylamine, ethanol, and chloroalkane is 0.15 mol:60 mL:0.15 mol, the chloroalkane is 1-chlorooctane, and the volume fraction of ethanol is 95%; the amount ratio of quaternary ammonium salt product, dichloromethane, and 3-chloroperoxybenzoic acid is 30 g:90 mL:20 g; Step A2: Under a nitrogen atmosphere, a thioether-containing carboxylic acid was added to toluene, pyridine was added with stirring, and the temperature was raised to 50°C. Then, the epoxy product 1 was added and stirred for 10 hours. The temperature was then raised to 120°C and stirred for 2 hours to obtain a hydroxyl product. The amount ratio of the thioether-containing carboxylic acid, toluene, pyridine, and epoxy product 1 was 0.4 mol:200 mL:0.04 mol:28 g. The thioether-containing carboxylic acid was 3-(butylmercapto)propionic acid. Step A3: Add a cyano-containing hindered phenol to tetrahydrofuran, add Raney nickel and Pd / C with stirring, introduce hydrogen, and react with stirring at normal pressure for 50 hours to obtain an amino product; add epichlorohydrin, the amino product, and tetrabutylammonium bromide to toluene, reflux and stir at 110°C for 4 hours, cool to room temperature, add sodium hydroxide solution, and stir for 6 hours to obtain an epoxy product 2; the amount ratio of the cyano-containing hindered phenol, tetrahydrofuran, Raney nickel, and Pd / C is 0.15 mol: 70 mL: 0.03 mol: 0.025 mol, and the cyano-containing hindered phenol is 3,5-di-tert-butyl-4-hydroxybenzeneacetonitrile; the amount ratio of epichlorohydrin, the amino product, tetrabutylammonium bromide, toluene, and sodium hydroxide solution is 24 g: 28 g: 0.08 mol: 100 mL: 25 mL; the mass fraction of the sodium hydroxide solution is 40%; Step A4: Add the epoxy product 2 and the hydroxyl product to methanol, start stirring, then add trimethylamine, and reflux and stir at 120°C for 7 hours to obtain the auxiliary agent; the amount ratio of the epoxy product 2, the hydroxyl product, methanol, and trimethylamine is 34g:30g:130mL:0.05mol.

[0016] Example 4 A modified microsphere, the preparation of which comprises the following steps: Step B1: Span 40 was added to n-heptane, mixed with stirring, and heated to 60°C. A polyvinyl alcohol solution and hydrochloric acid were added dropwise, stirred for 1 hour, and then glutaraldehyde was added. The mixture was kept at 60°C for 2 hours. The polyvinyl alcohol microspheres were washed and dried. The amount ratio of Span 40, n-heptane, polyvinyl alcohol solution, hydrochloric acid, and glutaraldehyde was 0.6 g:45 mL:25 mL:2 mL:5 mL. The polyvinyl alcohol solution was prepared by adding 5 g of polyvinyl alcohol to 100 mL of deionized water and stirring for 5 minutes. Step B2: Add polyvinyl alcohol microspheres to ethyl acetate, add maleic anhydride and a catalyst with stirring, and react at 80°C with constant stirring for 3.5 hours. After washing and vacuum drying, microspheres containing unsaturated carboxyl groups on the surface are obtained. The amount ratio of polyvinyl alcohol microspheres, ethyl acetate, maleic anhydride, and catalyst is 5 g:80 mL:0.5 g:0.1 g, and the catalyst is 4-dimethylaminopyridine. Step B3: In a nitrogen atmosphere, DOPO and microspheres containing unsaturated carboxyl groups on the surface were added to DMF, and the reaction was stirred at 90°C for 8 hours. After cooling to room temperature, the modified microspheres were recrystallized in an ice-water bath and filtered under reduced pressure to obtain the modified microspheres; the dosage ratio of DOPO, microspheres containing unsaturated carboxyl groups on the surface, and DMF was 11 g:6 g:80 mL.

[0017] Example 5 A modified microsphere, the preparation of which comprises the following steps: Step B1: Span 40 was added to n-heptane, mixed with stirring, and the temperature was raised to 63°C. A polyvinyl alcohol solution and hydrochloric acid were added dropwise, stirred for 1.3 hours, and then glutaraldehyde was added. The mixture was kept at 63°C for 2.3 hours. The polyvinyl alcohol microspheres were washed and dried. The amount ratio of Span 40, n-heptane, polyvinyl alcohol solution, hydrochloric acid, and glutaraldehyde was 0.63 g:47 mL:27 mL:2.3 mL:5.5 mL. The polyvinyl alcohol solution was prepared by adding 6 g of polyvinyl alcohol to 105 mL of deionized water and stirring for 8 minutes. Step B2: Add polyvinyl alcohol microspheres to ethyl acetate, add maleic anhydride and a catalyst with stirring, and react at 85°C with constant stirring for 4.0 hours. After washing and vacuum drying, microspheres containing unsaturated carboxyl groups on the surface are obtained. The amount ratio of polyvinyl alcohol microspheres, ethyl acetate, maleic anhydride, and catalyst is 6 g:85 mL:0.8 g:0.13 g, and the catalyst is 4-dimethylaminopyridine. Step B3: Under a nitrogen atmosphere, DOPO and microspheres containing unsaturated carboxyl groups on the surface were added to DMF, and the reaction was stirred at 100°C for 9 hours. After cooling to room temperature, the modified microspheres were recrystallized in an ice-water bath and filtered under reduced pressure to obtain the modified microspheres; the dosage ratio of DOPO, microspheres containing unsaturated carboxyl groups on the surface, and DMF was 12 g:7.5 g:90 mL.

[0018] Example 6 A modified microsphere, the preparation of which comprises the following steps: Step B1: Span 40 was added to n-heptane, mixed with stirring, and the temperature was raised to 65°C. A polyvinyl alcohol solution and hydrochloric acid were added dropwise, and the mixture was stirred for 1.5 hours. Glutaraldehyde was then added and the mixture was kept at 65°C for 2.5 hours. The polyvinyl alcohol microspheres were washed and dried. The amount ratio of Span 40, n-heptane, polyvinyl alcohol solution, hydrochloric acid, and glutaraldehyde was 0.65 g:50 mL:30 mL:2.5 mL:6 mL. The polyvinyl alcohol solution was prepared by adding 7 g of polyvinyl alcohol to 110 mL of deionized water and stirring for 10 minutes. Step B2: Add polyvinyl alcohol microspheres to ethyl acetate, add maleic anhydride and a catalyst with stirring, and react at 90°C with constant stirring for 4.5 hours. After washing and vacuum drying, microspheres containing unsaturated carboxyl groups on the surface are obtained; the amount ratio of polyvinyl alcohol microspheres, ethyl acetate, maleic anhydride, and catalyst is 7 g:90 mL:1.0 g:0.15 g, and the catalyst is 4-dimethylaminopyridine; Step B3: In a nitrogen atmosphere, DOPO and microspheres containing unsaturated carboxyl groups on the surface were added to DMF, and the reaction was stirred at 110°C for 10 hours. After cooling to room temperature, the modified microspheres were recrystallized in an ice-water bath and filtered under reduced pressure to obtain the modified microspheres; the dosage ratio of DOPO, microspheres containing unsaturated carboxyl groups on the surface, and DMF was 13 g:9 g:100 mL.

[0019] Example 7 A starch-based biodegradable composite material comprises the following raw materials in parts by weight: 55 parts of thermoplastic starch, 1.1 parts of modified microspheres, 18 parts of glycerol, 25 parts of polyhydroxyalkanoate, 3 parts of a coupling agent, 15 parts of talc, and 1.5 parts of an additive; the polyhydroxyalkanoate is polyhydroxybutyrate; the coupling agent is KH560; The preparation of the starch-based degradable composite material comprises the following steps: Step S1: Thermoplastic starch (supplier: Suzhou Minghua Sugar Alcohol Co., Ltd.), the modified microspheres obtained in Example 4, polyhydroxyalkanoate, a coupling agent, and talc (supplier: Qingdao Lukuang Talc Co., Ltd.) were stirred and mixed for 15 minutes, and then glycerol and the auxiliary agent obtained in Example 1 were added, and the mixture was stirred at a speed of 100 rpm for 4 minutes to obtain a mixture; Step S2: adding the obtained mixture into a twin-screw extruder, melting, extruding and granulating at 200 r / min and 110° C. to obtain pellets, and then injection molding and forming the pellets to obtain a starch-based biodegradable composite material, with an injection molding pressure of 60 MPa and an injection molding machine temperature of 125° C.

[0020] Example 8 A starch-based biodegradable composite material comprises the following raw materials in parts by weight: 60 parts of thermoplastic starch, 1.3 parts of modified microspheres, 20 parts of glycerol, 30 parts of polyhydroxyalkanoate, 4 parts of a coupling agent, 18 parts of talc, and 1.8 parts of an additive; the polyhydroxyalkanoate is polyhydroxybutyrate; the coupling agent is KH560; The preparation of the starch-based degradable composite material comprises the following steps: Step S1: Thermoplastic starch (supplier: Suzhou Minghua Sugar Alcohol Co., Ltd.), the modified microspheres obtained in Example 5, polyhydroxyalkanoate, a coupling agent, and talc (supplier: Qingdao Lukuang Talc Co., Ltd.) were stirred and mixed for 18 minutes, and then glycerol and the auxiliary agent obtained in Example 2 were added, and the mixture was stirred at a speed of 100 r / min for 5 minutes to obtain a mixture; Step S2: adding the obtained mixture into a twin-screw extruder, melting, extruding and granulating at 200 r / min and 115° C. to obtain pellets, and then injection molding and forming the pellets to obtain a starch-based biodegradable composite material, with an injection molding pressure of 60 MPa and an injection molding machine temperature of 130° C.

[0021] Example 9 A starch-based biodegradable composite material comprises the following raw materials in parts by weight: 65 parts of thermoplastic starch, 1.5 parts of modified microspheres, 22 parts of glycerol, 35 parts of polyhydroxyalkanoate, 5 parts of a coupling agent, 20 parts of talc, and 2.0 parts of an additive; the polyhydroxyalkanoate is polyhydroxybutyrate; the coupling agent is KH560; The preparation of the starch-based degradable composite material comprises the following steps: Step S1: Thermoplastic starch (supplier: Suzhou Minghua Sugar Alcohol Co., Ltd.), the modified microspheres obtained in Example 6, polyhydroxyalkanoate, a coupling agent, and talc (supplier: Qingdao Lukuang Talc Co., Ltd.) were stirred and mixed for 20 minutes, and then glycerol and the auxiliary agent obtained in Example 3 were added. The mixture was stirred at a speed of 200 rpm for 6 minutes to obtain a mixture; Step S2: adding the obtained mixture into a twin-screw extruder, melting, extruding and granulating at 300 r / min and 120° C. to obtain pellets, and then injection molding and forming the pellets to obtain a starch-based biodegradable composite material, with an injection molding pressure of 65 MPa and an injection molding machine temperature of 135° C.

[0022] Comparative Example 1 Compared with Example 9, the cyano-containing hindered phenol was replaced with p-toluene nitrile, that is, no hindered phenol was introduced. The rest was exactly the same as Example 9 to obtain a starch-based degradable composite material.

[0023] Comparative Example 2 Compared with Example 9, the thioether-containing carboxylic acid was replaced with 4-methylvaleric acid, that is, no thioether was introduced. The rest was exactly the same as Example 9 to prepare a starch-based degradable composite material.

[0024] Comparative Example 3 Compared with Example 9, the quaternary ammonium salt product was replaced with triallylamine, that is, no quaternary ammonium salt was introduced, and the rest was exactly the same as Example 9 to obtain a starch-based degradable composite material.

[0025] Comparative Example 4 Compared with Example 9, the modified microspheres were replaced with the polyvinyl alcohol microspheres obtained in Step B1 of Example 6, that is, no carboxyl groups and DOPO were introduced. The rest was the same as in Example 9 to obtain a starch-based degradable composite material.

[0026] Comparative Example 5 Compared with Example 9, the modified microspheres were replaced with microspheres containing unsaturated carboxyl groups on the surface obtained in Step B2 of Example 6, that is, DOPO was not introduced. The rest was exactly the same as in Example 9 to obtain a starch-based degradable composite material.

[0027] The starch-based degradable composite material prepared by the present invention is further tested for its effects, and the test results are described below.

[0028] In order to test the starch-based degradable composite material prepared by the present invention, the starch-based degradable composite materials obtained in Examples 7-9 and Comparative Examples 1-5 were subjected to performance tests. The tensile strength and elongation at break were measured using an electronic universal testing machine (E44.304, MTS) according to GB / T1040-2006, with a tensile rate of 20 mm / min. The composite material was placed in an oven at 105°C and dried for 12 h. A weight of about 2 g was taken out and recorded as M0. The composite material was then placed in a sealed container at a humidity of 50% (RH). After 48 h, the weight was taken out and recorded as M0. t , calculate water absorption (%) = (M t -M0) / M0*100; flame retardancy was tested with reference to the UL94V-0 standard; antibacterial rates were determined using Escherichia coli and Staphylococcus aureus as test bacteria, according to GB / T31402-2015 "Test Method for Antibacterial Properties of Plastic Surfaces"; the composite materials were placed in an air oven at 40°C for 24 hours, and the tensile strength and elongation at break after aging were measured; the results are recorded in Table 1.

[0029] According to the data in Table 1, the starch-based biodegradable composite material of the present invention exhibits excellent mechanical properties, water resistance, flame retardancy, antibacterial properties, and antioxidant properties. Comparison of Example 9 with Comparative Example 1 shows that the use of a hyperbranched macromolecular structure additive without the introduction of hindered phenols significantly degrades the mechanical properties and weatherability of the composite material after air oxidative aging. Comparison of Example 9 with Comparative Example 2 shows that the use of a hyperbranched macromolecular structure additive without the introduction of thioethers degrades the mechanical properties and weatherability of the composite material after air oxidative aging. Comparison of Example 9 with Comparative Example 3 shows that the use of a hyperbranched macromolecular structure additive without the introduction of quaternary ammonium salts significantly reduces the antibacterial properties of the composite material. Comparison of Example 9 with Comparative Example 4 shows that the use of polyvinyl alcohol microspheres without the introduction of carboxyl groups and DOPO weakens the binding force between the polyvinyl alcohol microspheres and starch, resulting in reduced mechanical properties, water resistance, and flame retardancy of the composite material. Comparison of Example 9 with Comparative Example 5 shows that the use of polyvinyl alcohol microspheres with carboxyl groups without the introduction of DOPO reduces the flame retardancy of the composite material.

[0030] The above content is merely an example and explanation of the concept of the present invention. Those skilled in the art may make various modifications or additions to the described specific embodiments or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the scope of protection of the present invention.

Claims

1. A starch-based biodegradable composite material, characterized in that: The invention comprises the following raw materials in parts by weight: 55-65 parts of thermoplastic starch, 1.1-1.5 parts of modified microspheres, 18-22 parts of glycerol, 25-35 parts of polyhydroxyalkanoate, 3-5 parts of coupling agent, 15-20 parts of talc, and 1.5-2.0 parts of auxiliary agent; The preparation of the auxiliary agent comprises the following steps: Step A1: adding triallylamine to ethanol, adding chloroalkane under stirring, and stirring to react to obtain a quaternary ammonium salt product; The quaternary ammonium salt product is added to dichloromethane, and 3-chloroperoxybenzoic acid is added under stirring, and the reaction is stirred to obtain the epoxy product 1; Step A2: In a protective gas atmosphere, add a thioether-containing carboxylic acid to toluene, add pyridine under stirring, and then add the epoxy product 1, and stir to react to obtain a hydroxyl product; Step A3: Add a cyano-containing hindered phenol to tetrahydrofuran, add Raney nickel and Pd / C under stirring, introduce hydrogen, and react under normal pressure with stirring to obtain an amino product; add epichlorohydrin, the amino product, and tetrabutylammonium bromide to toluene, reflux and react with stirring, cool to room temperature, add sodium hydroxide solution, and stir to obtain an epoxy product 2; Step A4: Add the epoxy product 2 and the hydroxyl product into methanol, add trimethylamine with stirring, and reflux and stir to react to obtain the auxiliary agent.

2. A starch-based biodegradable composite material according to claim 1, characterized in that: The polyhydroxyalkanoate is polyhydroxybutyrate, and the coupling agent is KH560; in step A1, the dosage ratio of triallylamine, ethanol, and chloroalkane is 0.1-0.15 mol: 50-60 mL: 0.1-0.15 mol, the chloroalkane is selected from one of 1-chlorobutane, 1-chlorohexane, and 1-chlorooctane, and the volume fraction of ethanol is 95%; the dosage ratio of the quaternary ammonium salt product, dichloromethane, and 3-chloroperoxybenzoic acid is 20-30 g: 80-90 mL: 18-20 g.

3. The starch-based biodegradable composite material according to claim 1, characterized in that: In step A2, the amount ratio of the thioether-containing carboxylic acid, toluene, pyridine, and epoxidation product 1 is 0.3-0.4 mol: 180-200 mL: 0.03-0.04 mol: 22-28 g, and the thioether-containing carboxylic acid is selected from one of 3-methylthiopropionic acid, 3-(benzylthio)propionic acid, and 3-(butylmercapto)propionic acid; in step A4, the amount ratio of the epoxidation product 2, the hydroxyl product, methanol, and trimethylamine is 30-34 g: 24-30 g: 120-130 mL: 0.03-0.05 mol.

4. The starch-based degradable composite material according to claim 1, characterized in that: In step A3, the amount ratio of the cyano-containing hindered phenol, tetrahydrofuran, Raney nickel and Pd / C is 0.1-0.15 mol: 60-70 mL: 0.02-0.03 mol: 0.02-0.025 mol, and the cyano-containing hindered phenol is selected from one of 3,5-di-tert-butyl-4-hydroxybenzonitrile and 3,5-di-tert-butyl-4-hydroxybenzeneacetonitrile.

5. The starch-based degradable composite material according to claim 1, characterized in that: In step A3, the dosage ratio of epichlorohydrin, amino product, tetrabutylammonium bromide, toluene and sodium hydroxide solution is 22-24 g: 26-28 g: 0.05-0.08 mol: 90-100 mL: 20-25 mL, and the mass fraction of the sodium hydroxide solution is 40-50%.

6. The starch-based biodegradable composite material according to claim 1, characterized in that: The modified microspheres are prepared by the following steps: Step B1: Add Span 40 to n-heptane, mix and stir, and heat to 60-65°C, dropwise add polyvinyl alcohol solution and hydrochloric acid, stir for 1-1.5 hours, add glutaraldehyde and keep warm at 60-65°C for 2-2.5 hours, wash and dry to obtain polyvinyl alcohol microspheres; Step B2: adding polyvinyl alcohol microspheres to ethyl acetate, adding maleic anhydride and a catalyst under stirring, reacting at 80-90° C. with constant stirring for 3.5-4.5 hours, and obtaining microspheres with unsaturated carboxyl groups on the surface after washing and vacuum drying; Step B3: In a nitrogen atmosphere, DOPO and microspheres containing unsaturated carboxyl groups on the surface are added to DMF, stirred and reacted at 90-110° C. for 8-10 h, cooled to room temperature, recrystallized in an ice-water bath, and filtered under reduced pressure to obtain modified microspheres.

7. The starch-based degradable composite material according to claim 6, characterized in that: In step B1, the usage ratio of Span 40, n-heptane, polyvinyl alcohol solution, hydrochloric acid and glutaraldehyde is 0.6-0.65 g: 45-50 mL: 25-30 mL: 2-2.5 mL: 5-6 mL. The polyvinyl alcohol solution is prepared by adding 5-7 g of polyvinyl alcohol to 100-110 mL of deionized water and stirring for 5-10 min.

8. The starch-based degradable composite material according to claim 6, characterized in that: In step B2, the usage ratio of polyvinyl alcohol microspheres, ethyl acetate, maleic anhydride and catalyst is 5-7 g: 80-90 mL: 0.5-1.0 g: 0.1-0.15 g, and the catalyst is 4-dimethylaminopyridine.

9. The starch-based degradable composite material according to claim 6, characterized in that: In step B3, the usage ratio of DOPO, microspheres containing unsaturated carboxyl groups on the surface, and DMF is 11-13 g: 6-9 g: 80-100 mL.

10. A method for preparing the starch-based degradable composite material according to any one of claims 1 to 9, characterized in that: The steps include: Step S1: After mixing thermoplastic starch, modified microspheres, polyhydroxyalkanoate, coupling agent and talc for 15-20 minutes, glycerol and auxiliary agent are added, and stirred at a speed of 100-200 r / min for 4-6 minutes to obtain a mixture; Step S2: adding the obtained mixture into a twin-screw extruder, melting, extruding and granulating at 200-300 r / min and 110-120° C. to obtain pellets, and then injection molding and forming the pellets to obtain a starch-based biodegradable composite material, with an injection molding pressure of 60-65 MPa and an injection molding machine temperature of 125-135° C.

Citation Information

Patent Citations

  • Non-migration and degradable antimicrobial polyester film and preparation method thereof

    CN104151792A

  • Macromolecular hindered phenol antioxidant containing thioether and carbamate groups and preparation method and application thereof

    CN104292141A

  • Flame-retardant degradable starch-based composition material for injection molding and preparation method thereof

    CN106496645A

  • Flame-retardant degradable plastic and preparation method thereof

    CN112940424A

  • Composite antioxidant and preparation process thereof

    CN113214540A