Ethylene-vinyl acetate rubber foam material as well as preparation method and application thereof
By filling carbon nano-onions in ethylene-vinyl acetate rubber foaming material and adopting intensive refining, refining and foaming processes, the problems of large quality and lack of conductivity of ethylene-vinyl acetate rubber are solved, and light weight and conductive properties are achieved The combination of performance has expanded its application scope.
Patent Information
- Application Number
- CN202411319983.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-23
- Publication Date
- 2024-12-03
AI Technical Summary
Due to its own structural limitations, ethylene-vinyl acetate rubber has a large mass and lacks conductive properties, which limits its application range.
By filling carbon nano-onions in an ethylene-vinyl acetate rubber foam matrix, combined with intensive refining, refining and foaming processes, a lightweight and conductive ethylene-vinyl acetate rubber foaming material is prepared.
It realizes the lightweight and conductive properties of ethylene-vinyl acetate rubber foaming material, can evenly disperse the bending stress of external impact, and broadens its applications in electromagnetic shielding, anti-static, heat dissipation or packaging fields.
Smart Images

Figure CN119060446A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer material foaming, and in particular relates to an ethylene-vinyl acetate rubber foaming material and a preparation method and application thereof. Background Art
[0002] As an important polymer material, rubber foam material has attracted extensive attention from industry and academia. Usually, there are a large number of tiny cells inside its matrix. Compared with bulky polymer materials, rubber foam material has the advantages of low density, good thermal insulation, good sound insulation and good cushioning performance. It has become one of the most widely used polymer materials and occupies a very important position in the polymer industry.
[0003] Ethylene-vinyl acetate rubber (EVM) is a random copolymer of ethylene and vinyl acetate monomers. The main chain of the molecule is a saturated structure, and its chemical activity and processing performance depend on the content of vinyl acetate (VA) in the molecular structure. Since EVM adds vinyl acetate polar groups to ethylene, its processing performance is improved. EVM has good oil resistance and temperature resistance, and its dynamic performance advantages are outstanding, which can meet the requirements of rubber rollers or conveyor belts.
[0004] Although ethylene-vinyl acetate rubber has outstanding advantages, it has certain defects due to its own structural limitations, such as its large weight and lack of electrical conductivity, which limits the application scope of ethylene-vinyl acetate rubber. Summary of the invention
[0005] The object of the present invention is to provide an ethylene-vinyl acetate rubber foam material and a preparation method and application thereof. The ethylene-vinyl acetate rubber foam material provided by the present invention is light in weight and has conductive properties.
[0006] In order to achieve the above object, the present invention provides the following technical solutions:
[0007] The invention provides an ethylene-vinyl acetate rubber foam material, comprising an ethylene-vinyl acetate rubber foam matrix and carbon nano onions filled in the ethylene-vinyl acetate rubber foam matrix.
[0008] Preferably, in the ethylene-vinyl acetate rubber foam matrix, the molar ratio of ethylene units to vinyl acetate units is 0.82-0.90:0.62-0.71.
[0009] Preferably, the porosity of the ethylene-vinyl acetate rubber foam matrix is 31-41%.
[0010] Preferably, the mass ratio of the carbon nano onion to the ethylene-vinyl acetate rubber foaming matrix is 15-20:100.
[0011] Preferably, the density of the ethylene-vinyl acetate rubber foam material is 0.17 to 0.291 g / cm 3 , the conductivity is 1×10 -5 ~3.3×10 -5 S cm -1 .
[0012] The present invention also provides a method for preparing the ethylene-vinyl acetate rubber foam material described in the above scheme, comprising the following steps:
[0013] Ethylene-vinyl acetate rubber, a foaming agent, a carbon nano-onion, a vulcanization accelerator, an activator and a vulcanizing agent are mixed and successively subjected to internal mixing, open mixing and foaming to obtain an ethylene-vinyl acetate rubber foam material.
[0014] Preferably, the mass ratio of the ethylene-vinyl acetate rubber to the foaming agent is 100:5.9-6.2; the mass ratio of the ethylene-vinyl acetate rubber to the carbon nano onion is 100:15-20; the mass ratio of the ethylene-vinyl acetate rubber to the vulcanization accelerator is 100:1.48-1.52; the mass ratio of the ethylene-vinyl acetate rubber to the activator is 100:1.8-2.2; the mass ratio of the ethylene-vinyl acetate rubber to the vulcanizing agent is 100:0.38-0.42.
[0015] Preferably, the banburying temperature is 58-65° C., the banburying time is 7.5-8 min, and the rotor speed of the banburying is 45-50 rpm.
[0016] Preferably, the foaming is as follows: compressing the rubber mix obtained by the open milling and releasing the pressure to expand the rubber mix; the compression molding temperature is 173-176° C. and the pressure is 9.8-10.2 MPa; and the pressure release time is 4.5-5.0 min.
[0017] The present invention also provides the use of the ethylene-vinyl acetate rubber foam material described in the above scheme or the ethylene-vinyl acetate rubber foam material obtained by the preparation method described in the above scheme in the fields of electromagnetic shielding, antistatic, heat dissipation or packaging.
[0018] The present invention provides an ethylene-vinyl acetate rubber foam material. The ethylene-vinyl acetate rubber foam material provided by the present invention uses ethylene-vinyl acetate rubber as a matrix for foaming, uses carbon nano onions (CNOs) as a filler to fill the foam material, and introduces the hollow structure of the carbon nano onions. Compared with traditional fillers such as calcium carbonate with the same filling amount, the ethylene-vinyl acetate rubber foam material provided by the present invention is light in weight and has conductive properties. When subjected to external impact, the bending stress borne by the material can be evenly dispersed, the force is more uniform, and the overall performance is better.
[0019] The present invention also provides a method for preparing the ethylene-vinyl acetate rubber foam material of the above scheme. The present invention uses ethylene-vinyl acetate rubber as a matrix to prepare the ethylene-vinyl acetate rubber foam material. The preparation method provided by the present invention has simple steps, convenient operation and high feasibility.
[0020] The present invention also provides the use of the ethylene-vinyl acetate rubber foam material described in the above scheme or the ethylene-vinyl acetate rubber foam material obtained by the preparation method described in the above scheme in the fields of electromagnetic shielding, antistatic, heat dissipation or packaging. The ethylene-vinyl acetate rubber foam material provided by the present invention is light in weight and has conductive properties. When subjected to external impact, the bending stress borne by the material can be evenly dispersed, and the force is more evenly applied, which broadens the application field of the ethylene-vinyl acetate rubber foam material and is suitable for use in the fields of electromagnetic shielding, antistatic, heat dissipation or packaging, and is particularly suitable for use in the fields of antistatic or packaging. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0022] Figure 1 This is a scanning electron microscope image of carbon nano-onion;
[0023] Figure 2 The figure is a schematic flow chart of the method for preparing the ethylene-vinyl acetate rubber foam material of the present invention;
[0024] Figure symbols: 1 is internal mixing, 2 is open mixing, and 3 is foaming. DETAILED DESCRIPTION
[0025] The invention provides an ethylene-vinyl acetate rubber foam material, comprising an ethylene-vinyl acetate rubber foam matrix and carbon nano onions filled in the ethylene-vinyl acetate rubber foam matrix.
[0026] The ethylene-vinyl acetate rubber foam material provided by the present invention comprises an ethylene-vinyl acetate rubber foam matrix; in the ethylene-vinyl acetate rubber foam matrix, the molar ratio of ethylene units to vinyl acetate units is preferably 0.82-0.90:0.62-0.71, more preferably 0.85-0.88:0.65-0.7, and further preferably 0.85-0.86:0.66-0.68.
[0027] In the present invention, the porosity of the ethylene-vinyl acetate rubber foamed substrate is preferably 31 to 41%, more preferably 35 to 38%, and further preferably 36 to 36.8%.
[0028] The ethylene-vinyl acetate rubber foam material provided by the present invention includes carbon nano-onions; the particle size of the carbon nano-onions is preferably 80 to 160 nm, more preferably 95 to 130 nm, and further preferably 95 to 110 nm.
[0029] In the present invention, the mass ratio of the carbon nano onion to the ethylene-vinyl acetate rubber foaming matrix is preferably 15 to 20:100, more preferably 16 to 19:110, and further preferably 17 to 18:110.
[0030] In the present invention, the density of the ethylene-vinyl acetate rubber foam material is preferably 0.17 to 0.291 g / cm 3 The conductivity is preferably 1×10 -5 ~3.3×10 -5 S cm -1 .
[0031] The present invention also provides a method for preparing the ethylene-vinyl acetate rubber foam material described in the above scheme, comprising the following steps:
[0032] Ethylene-vinyl acetate rubber, a foaming agent, a carbon nano-onion, a vulcanization accelerator, an activator and a vulcanizing agent are mixed and successively subjected to internal mixing, open mixing and foaming to obtain an ethylene-vinyl acetate rubber foam material.
[0033] The present invention mixes ethylene-vinyl acetate rubber, a foaming agent, a carbon nano-onion, a vulcanization accelerator, an activator and a vulcanizing agent (referred to as the first mixing). In the present invention, the foaming agent is preferably azodicarbonamide; the mass ratio of the ethylene-vinyl acetate rubber to the foaming agent is preferably 100:5.9-6.2, more preferably 100:5.9-6.1, and further preferably 100:6. The reaction mechanism of the foaming agent of the present invention is shown in Formula A:
[0034]
[0035] In the present invention, the mass ratio of the ethylene-vinyl acetate rubber to the carbon nano-onion is preferably 100:15-20, more preferably 100:16-19, and further preferably 100:17-18.
[0036] In the present invention, the vulcanization accelerator is preferably stearic acid; the mass ratio of the ethylene-vinyl acetate rubber to the vulcanization accelerator is preferably 100:1.48-1.52, more preferably 100:1.49-1.51, and further preferably 100:1.5.
[0037] In the present invention, the activator is preferably zinc oxide; the mass ratio of the ethylene-vinyl acetate rubber to the activator is preferably 100:1.8-2.2, more preferably 100:1.9-2.1, and further preferably 100:2.
[0038] In the present invention, the vulcanizing agent is preferably dicumyl peroxide; the mass ratio of the ethylene-vinyl acetate rubber to the vulcanizing agent is preferably 100:0.38-0.42, more preferably 100:0.39-0.41, and further preferably 100:0.4.
[0039] In the present invention, the first mixing is preferably: adding carbon nano onion, foaming agent, vulcanization accelerator, activator and vulcanizing agent to ethylene vinyl acetate rubber in sequence.
[0040] After mixing, the present invention sequentially performs banburying, open mixing and foaming to obtain ethylene-vinyl acetate rubber foam material. In the present invention, the banburying temperature is preferably 58-65° C., more preferably 60° C., the banburying time is preferably 7.5-8 min, more preferably 8 min; the banburying equipment is preferably a torque rheometer; the rotor speed of the banburying is preferably 45-50 rpm, more preferably 45 rpm.
[0041] In the present invention, the internal mixing preferably further includes debinding to take out the internal mixing product.
[0042] In the present invention, the temperature of the open mill is preferably 26-32° C., more preferably 30° C.; the equipment for the open mill is preferably a double-roller mill.
[0043] In the present invention, the open refining is preferably: open refining on a double-roller open refining mill, cutting the left and right 3 / 4 5 times each, and thinning through 5 times before exhausting and sheeting.
[0044] In the present invention, after the open refining, the obtained open refining product is preferably allowed to stand; the standing temperature is preferably room temperature, and the standing time is preferably 12 to 24 hours, more preferably 15 to 20 hours, and further preferably 17 hours.
[0045] In the present invention, the foaming is preferably compression foaming; the foaming equipment is preferably a flat-plate compression molding machine; the filling factor of the mold used for the foaming is preferably 109%, and the volume is preferably 78.3 cm 3 .
[0046] In the present invention, the foaming is preferably performed by compression molding the rubber mix obtained by the open milling, and releasing the pressure to cause the rubber mix to expand; the compression molding temperature is preferably 173-176°C, more preferably 175°C, and the pressure is preferably 9.8-10.2MPa, more preferably 10MPa; the pressure release time is preferably 4.5-5.0min, more preferably 5min.
[0047] The preparation method of the ethylene-vinyl acetate rubber foam material provided by the present invention has the following main process flow: Figure 2 The present invention mixes ethylene-vinyl acetate rubber, a foaming agent, a carbon nano-onion, a vulcanization accelerator, an activator and a vulcanizing agent, and sequentially performs internal kneading, open kneading and foaming to obtain an ethylene-vinyl acetate rubber foam material.
[0048] The present invention also provides the use of the ethylene-vinyl acetate rubber foam material described in the above scheme or the ethylene-vinyl acetate rubber foam material obtained by the preparation method described in the above scheme in the fields of electromagnetic shielding, antistatic, heat dissipation or packaging.
[0049] The ethylene-vinyl acetate rubber foam material provided by the present invention is light in weight and has conductive properties. When subjected to external impact, the bending stress borne by the material can be evenly dispersed, and the force is more evenly borne, thereby broadening the application field of the ethylene-vinyl acetate rubber foam material and being suitable for use in electromagnetic shielding, antistatic, heat dissipation or packaging fields, and is particularly suitable for use in antistatic or packaging fields.
[0050] In order to further illustrate the present invention, the scheme of the present invention is described in detail below in conjunction with the accompanying drawings and embodiments, but they should not be understood as limiting the protection scope of the present invention.
[0051] Example 1
[0052] First, 100 parts of EVM rubber were added to the torque rheometer at 60°C and a rotor speed of 45 rpm. When the torque was stable, 15 parts of carbon nano-onions (structured as Figure 1As shown), 6 parts of azodicarbonamide, 2 parts of zinc oxide, 1.5 parts of stearic acid and 0.4 parts of diisopropylbenzene peroxide, after 8 minutes of banburying, the rubber was discharged and taken out; then it was opened on a double-roller open mill at 30°C, and the left and right 3 / 4 were cut 5 times each, and the sheet was vented and removed after 5 thin passes. After standing at room temperature for 12 hours, it was molded and foamed; the mixed rubber was compressed and molded at 175°C and 10MPa pressure for 5 minutes using a flat plate molding machine (the filling factor of the foaming mold is 109%, and the volume is 78.3cm 3 ), during which the pressure is released, the rubber material expands, and bubbles are formed to obtain ethylene-vinyl acetate rubber foam material.
[0053] Example 2
[0054] First, 100 parts of EVM rubber were added to the torque rheometer at 60°C and a rotor speed of 45 rpm. When the torque was stable, 17 parts of carbon nano-onions (structured as Figure 1 As shown), 6 parts of azodicarbonamide, 2 parts of zinc oxide, 1.5 parts of stearic acid and 0.4 parts of diisopropylbenzene peroxide, after mixing for 8 minutes, the rubber was discharged and taken out; then it was mixed on a double-roller mill at 30°C, and the left and right 3 / 4 were cut 5 times each, and the sheet was vented and removed after 5 thin passes. After standing at room temperature for 24 hours, it was molded and foamed; the mixed rubber was compressed and molded at 175°C and 10MPa pressure for 5 minutes using a flat plate molding machine (the filling factor of the foaming mold is 109%, and the volume is 78.3cm 3 ), during which the pressure is released, the rubber material expands, and bubbles are formed to obtain ethylene-vinyl acetate rubber foam material.
[0055] Example 3
[0056] First, 100 parts of EVM rubber were added to the torque rheometer at 60°C and a rotor speed of 45 rpm. When the torque was stable, 19 parts of carbon nano-onions (structured as Figure 1 As shown), 6 parts of azodicarbonamide, 2 parts of zinc oxide, 1.5 parts of stearic acid and 0.4 parts of diisopropylbenzene peroxide, after mixing for 8 minutes, the rubber was discharged and taken out; then it was mixed on a double-roller mill at 30°C, and the left and right 3 / 4 were cut 5 times respectively, and the sheet was vented and removed after 5 thin passes. After standing at room temperature for 18 hours, it was molded and foamed; the mixed rubber was compressed and molded at 175°C and 10MPa pressure for 5 minutes using a flat plate molding machine (the filling factor of the foaming mold is 109%, and the volume is 78.3cm 3 ), during which the pressure is released, the rubber material expands, and bubbles are formed to obtain ethylene-vinyl acetate rubber foam material.
[0057] Example 4
[0058] The preparation method of this embodiment is the same as that of Embodiment 1, except that the number of portions of the carbon nano onion is 16 portions.
[0059] Example 5
[0060] The preparation method of this embodiment is the same as that of Embodiment 1, except that the number of portions of the carbon nano onion is 18 portions.
[0061] Example 6
[0062] The preparation method of this embodiment is the same as that of Embodiment 1, except that the number of portions of the carbon nano onion is 20 portions.
[0063] Test Case
[0064] The ethylene-vinyl acetate rubber foam materials prepared in Examples 4 to 6 were left to stand at room temperature for 24 hours and then tested for characterization. The density (measured by drainage method), tensile strength (measured by universal tensile testing machine) and conductivity (measured by voltammetry, with the rubber foam material without adding carbon nano onions as the control group) of the ethylene-vinyl acetate rubber foam materials were tested. The results are shown in Tables 1 to 3.
[0065] Table 1 Density and weight of rubber foam materials in Examples 4 to 6
[0066] Example <![CDATA[Volume (cm 3 )]]> <![CDATA[Density (g / cm 3 )]]> Weight(g) Example 4 1 0.170 0.170 Example 5 1 0.235 0.235 Example 6 1 0.291 0.291
[0067] It can be seen from Table 1 that as the number of carbon nano onions filled increases, the density of the ethylene-vinyl acetate rubber foam material gradually increases, but the overall density is still small; compared with the ethylene-vinyl acetate rubber foam material filled with the same number of calcium carbonate (20 parts), under the same volume, the density of the rubber foam material provided by the present invention is 0.12-0.17 g / cm 3 , lighter weight.
[0068] Table 2 Tensile strength of rubber foam materials in Examples 4 to 6
[0069] Example Tensile strength(MPa) Example 4 1.42 Example 5 1.56 Example 6 1.31
[0070] According to Table 2, it can be seen that with the increase of the amount of carbon nano onion filling, the tensile strength of ethylene-vinyl acetate rubber foam material shows a trend of first increasing and then decreasing. This may be because the increase of fillers is beneficial to the material reinforcement to a certain extent, but when the fillers increase to a certain extent, the pore structure of the rubber foam material will be destroyed, and stress concentration points will be easily formed, resulting in increased material defects and decreased strength; however, the tensile strength of ethylene-vinyl acetate rubber foam materials with different carbon nano onion filling amounts has a small change trend, indicating that the internal pore structure of each material is relatively uniform and the degree of damage due to force is not much different.
[0071] A voltage of 100 V was applied to the sample for 60 seconds. When the current decreased and stabilized, the current size was recorded and the steady-state current was used as a reference. The product of the voltage applied at both ends of the sample and the current passing through (Q=UI) can be used to calculate the electric power to characterize the heat generation capacity of the material. The results are shown in Table 3.
[0072] Table 3 Steady-state current of rubber foam materials of Examples 4 to 6 at 100V voltage
[0073] Example Control group Example 4 Example 5 Example 6 Initial state current / (mA) 2.0 11.8 15.8 21.6 Steady state current / (mA) 0.0 0.3 0.7 1.0 Electric power / w 0.0 0.03 0.07 0.10
[0074] According to Table 3, it can be seen that the steady-state current of the rubber foam material not filled with carbon nano-onions is 0, indicating that the rubber foam material not filled with carbon nano-onions is not conductive; when the amount of carbon nano-onions increases, the steady-state current gradually increases and the heat generating capacity gradually increases, indicating that the ethylene-vinyl acetate rubber foam material filled with carbon nano-onions has a certain conductivity.
[0075] It can be seen from the above embodiments that the ethylene-vinyl acetate rubber foam material provided by the present invention is light in weight and has conductive properties. When subjected to external impact, the bending stress borne by the material can be evenly dispersed, the force is more uniform, and the overall performance is better.
[0076] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. An ethylene-vinyl acetate rubber foam material, characterized in that: The invention comprises an ethylene-vinyl acetate rubber foaming matrix and carbon nano onions filled in the ethylene-vinyl acetate rubber foaming matrix.
2. The ethylene-vinyl acetate rubber foam material according to claim 1, characterized in that: In the ethylene-vinyl acetate rubber foaming matrix, the molar ratio of ethylene units to vinyl acetate units is 0.82-0.90:0.62-0.
71.
3. The ethylene-vinyl acetate rubber foam material according to claim 1 or 2, characterized in that: The porosity of the ethylene-vinyl acetate rubber foamed matrix is 31-41%.
4. The ethylene-vinyl acetate rubber foam material according to claim 1 or 2, characterized in that: The mass ratio of the carbon nano onion to the ethylene-vinyl acetate rubber foaming matrix is 15-20:
100.
5. The ethylene-vinyl acetate rubber foam material according to claim 1, characterized in that: The density of the ethylene-vinyl acetate rubber foam material is 0.17-0.291 g / cm 3 , the conductivity is 1×10 -5 ~3.3×10 -5 S cm -1 .
6. The method for preparing the ethylene-vinyl acetate rubber foam material according to any one of claims 1 to 5, characterized in that: The following steps are involved: Ethylene-vinyl acetate rubber, a foaming agent, a carbon nano-onion, a vulcanization accelerator, an activator and a vulcanizing agent are mixed and successively subjected to internal mixing, open mixing and foaming to obtain an ethylene-vinyl acetate rubber foam material.
7. The preparation method according to claim 6, characterized in that: The mass ratio of the ethylene-vinyl acetate rubber to the foaming agent is 100:5.9-6.2; The mass ratio of the ethylene-vinyl acetate rubber to the carbon nano onion is 100:15-20; The mass ratio of the ethylene-vinyl acetate rubber to the vulcanization accelerator is 100:1.48-1.52; The mass ratio of the ethylene-vinyl acetate rubber to the activator is 100:1.8-2.2 The mass ratio of the ethylene-vinyl acetate rubber to the vulcanizing agent is 100:0.38-0.
42.
8. The preparation method according to claim 6 or 7, characterized in that: The mixing temperature is 58-65°C and the mixing time is 7.5-8 minutes; The rotor speed of the internal mixing is 45-50 rpm.
9. The preparation method according to claim 6, characterized in that: The foaming step is: compressing the rubber mix obtained by the open milling to form the rubber mix, and releasing the pressure to cause the rubber mix to expand; The compression molding temperature is 173-176°C and the pressure is 9.8-10.2MPa; The pressure release time is 4.5 to 5.0 minutes.
10. Use of the ethylene-vinyl acetate rubber foam material according to any one of claims 1 to 5 or the ethylene-vinyl acetate rubber foam material obtained by the preparation method according to any one of claims 6 to 9 in the fields of electromagnetic shielding, antistatic, heat dissipation or packaging.