Macromolecular brake pad friction material and preparation method thereof
By introducing modified phenolic resin and flame retardant microcapsules into the friction materials of the brake pad, the problem of insufficient water resistance and oxidation resistance of the phenolic resin is solved, and the flame retardant performance and compatibility are significantly improved, achieving better brakes sheet material properties.
Patent Information
- Application Number
- CN202411324185.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-23
- Publication Date
- 2024-12-03
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The phenolic resins of existing brake pad friction materials are insufficient in water resistance, oxidation resistance and ultraviolet resistance, and the compatibility of ammonium polyphosphate with phenolic resin is poor, making it difficult to effectively improve flame retardant performance.
Modified phenolic resin and flame retardant microcapsules are used to enhance the water resistance and oxidation resistance of the phenolic resin by introducing hindered phenol and thiophene structures, and coated with ammonium polyphosphate to improve flame retardant performance.
The flame retardant performance, water resistance and oxidation resistance of the brake pad friction material are significantly improved, compatibility with phenolic resin is improved, and the stable performance and long-term use effect of the material are ensured.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of brake pads, and in particular to a polymer brake pad friction material and a preparation method thereof. Background Art
[0002] Brake pad friction material is a multi-component composite material composed of multiple components, mainly including reinforcing fiber, binder, filler and friction performance modifier, etc. The performance of brake friction material will be affected by the different proportions of each component and raw materials. Among them, the matrix of friction material, i.e. binder, is still mainly phenolic resin.
[0003] There are a large number of aromatic ring rigid structures in phenolic resin, the bond energy between atoms is large, and there is a high cohesive force between molecular chains, so it has good heat resistance and oxidation resistance. Phenolic resin contains many phenolic hydroxyl groups and a certain amount of hydroxymethyl. Phenolic hydroxyl groups are strong polar groups that easily absorb water, which reduces the strength of phenolic resin; phenolic hydroxyl groups are prone to change under the action of heat or ultraviolet rays, generating quinones or other structures, causing the material to change color and the performance of phenolic resin to decrease. Therefore, the water resistance, oxidation resistance and UV resistance of phenolic resin used in friction materials still cannot meet the use requirements.
[0004] In the prior art, the flame retardant properties of brake pad friction materials can be improved by adding flame retardants. Ammonium polyphosphate is non-toxic and odorless, does not produce corrosive gases such as hydrogen halides, has extremely low smoke production, and has high thermal stability. It is a halogen-free flame retardant with very good performance. However, directly adding ammonium polyphosphate will have poor compatibility with the matrix of the friction material, that is, the binder phenolic resin, and cannot effectively improve the flame retardant properties of the brake pad friction material.
[0005] In summary, a suitable modification method is urgently needed to improve the water resistance, oxidation resistance and UV resistance of phenolic resin, and to improve the compatibility of ammonium polyphosphate and phenolic resin, so as to obtain a brake pad friction material with better performance. Summary of the invention
[0006] In order to solve the above technical problems, the present invention provides a polymer brake pad friction material and a preparation method thereof.
[0007] The purpose of the present invention can be achieved by the following technical solutions: A polymer brake pad friction material, comprising the following raw materials in parts by weight: 9-11 parts of modified phenolic resin, 1-3 parts of flame retardant microcapsules, 26-32 parts of composite fibers, 7-9 parts of flake graphite, 6-8 parts of petroleum coke, 5-7 parts of aluminum oxide, 1-3 parts of friction powder, 12-14 parts of calcium carbonate, 4-6 parts of vermiculite powder, 20-22 parts of precipitated barium sulfate, and 1-2 parts of zinc stearate; The mass ratio of coconut fiber, areca palm fiber and basalt fiber in the composite fiber is 2-4:1-2:10-15; The preparation of the polymer brake pad friction material comprises the following steps: Step S1: mixing and stirring the composite fibers to obtain a mixed fiber material; Step S2: further stirring and mixing the modified phenolic resin, flame retardant microcapsules, flake graphite, petroleum coke, aluminum oxide, friction powder, calcium carbonate, vermiculite powder, precipitated barium sulfate, zinc stearate and the mixed fiber material to obtain a mixture; Step S3: adding the mixture into a mold cavity of a hot press to perform hot pressing molding, and then heat treating in a heat treatment drying oven, cutting and flat grinding in a sample cutting and grinding machine to obtain a polymer brake pad friction material; Further, in step S1, the stirring speed is 700-800 rpm and the stirring time is 5-10 min; in step S2, the stirring speed is 1400-1500 rpm and the stirring time is 10-15 min; Further, in step S3, the hot press cavity is preheated to 150-160°C, the hot pressing temperature is 170-180°C, and the hot pressing pressure is 11-13MPa; the total number of holding times is 6 times, the holding time of the 1st and 2nd times is 5-10s, the holding time of the 3rd, 4th and 5th times is 10-15s, and the holding time of the 6th time is 15-20min; the total number of exhausts is 6 times, the exhaust time of the 1st, 2nd, 3rd, 4th and 5th times is 5-10s, and the exhaust time of the 6th time is 30-45s; Furthermore, in step S3, the temperature of the heat treatment drying oven is linearly increased to 140°C within 2 hours, kept warm for 1-1.5 hours, then linearly increased to 160°C within 1 hour, kept warm for 3-3.5 hours, then linearly increased to 180°C within 1 hour, kept warm for 6-7 hours, and then reduced to room temperature.
[0008] The modified phenolic resin is prepared by the following steps: Step A1: Add 2-thiophene methanol to toluene, start stirring, then add sodium hydroxide solution, stir for 5-10 minutes, then dropwise add epichlorohydrin, stir and react at room temperature for 6-7 hours, filter, extract and dry to obtain the epoxy product 1; Furthermore, the dosage ratio of 2-thiophene methanol, toluene, sodium hydroxide solution and epichlorohydrin is 0.1 mol: 85-95 mL: 5-10 mL: 0.1 mol, and the mass fraction of the sodium hydroxide solution is 5-10%; During the reaction of step A1, the hydroxyl group in 2-thiophene methanol reacts with epichlorohydrin to generate an epoxy product 1 containing a thiophene ring; Step A2: In a protective gas atmosphere, add 3,5-di-tert-butyl-4-hydroxyphenylacetic acid to toluene, heat to 45-50° C., add pyridine, start stirring, then add the epoxy product 1, stir and react for 8-10 hours, then heat to 110-120° C., stir for 1-2 hours to obtain an alcohol hydroxyl product; Further, the usage ratio of 3,5-di-tert-butyl-4-hydroxyphenylacetic acid, toluene, pyridine and epoxidation product 1 is 0.1 mol: 140-150 mL: 0.010-0.015 mol: 24-26 g; During the reaction of step A2, the carboxyl group of 3,5-di-tert-butyl-4-hydroxyphenylacetic acid reacts with the epoxy group of the epoxy product 1 to form an alcohol hydroxyl product containing a thiophene ring and a hindered phenol structure; Step A3: Add the alcoholic hydroxyl product to toluene, start stirring, then add sodium hydroxide solution, stir for 5-10 minutes, then dropwise add epichlorohydrin, stir and react at room temperature for 6-7 hours, filter, extract and dry to obtain the epoxy product 2; Further, the usage ratio of alcohol hydroxyl product, toluene, sodium hydroxide solution and epichlorohydrin is 48-50g:85-95mL:5-10mL:0.1mol, and the mass fraction of sodium hydroxide solution is 10-15%; During the reaction of step A3, the hydroxyl group in the alcoholic hydroxyl product reacts with epichlorohydrin to generate an epoxy product 2; Step A4: Add the epoxy product 2 and the phenolic resin into methanol, then add trimethylamine, and stir the mixture at 100-120° C. for 3-4 hours to obtain a modified phenolic resin.
[0009] Further, the usage ratio of the epoxy product 2, the phenolic resin, methanol and trimethylamine is 59-61 g: 14-16 g: 150-160 mL: 0.1-0.2 mol, and the phenolic resin is a water-soluble phenolic resin; During the reaction of step A4, the epoxy group of the epoxy product 2 reacts with the hydroxymethyl group and the phenolic hydroxyl group in the phenolic resin to generate a modified phenolic resin containing hindered phenol and thiophene ring.
[0010] The flame retardant microcapsules are prepared by the following steps: Add ammonium polyphosphate to 1,4-dioxane and stir for 10-15 minutes to obtain dispersion a, then add the wall material to 1,4-dioxane and stir for 30-35 minutes to obtain dispersion b, then add dispersion a to dispersion b, stir and react for 4-5 hours to obtain flame retardant microcapsules; Furthermore, the dosage ratio of ammonium polyphosphate and 1,4-dioxane in dispersion a is 1-1.5 g: 6-8 mL; the dosage ratio of wall material and 1,4-dioxane in dispersion b is 1.5-1.7 g: 15-20 mL; the dosage ratio of dispersion a and dispersion b is 14-18 mL: 32-36 mL; the wall material is the prepared modified phenolic resin; In the preparation process of the flame retardant microcapsule, modified phenolic resin is used as the wall material, ammonium polyphosphate is used as the core material, and the wall material covers the core material to obtain the flame retardant microcapsule.
[0011] Beneficial effects of the invention: The invention discloses a polymer brake pad friction material, which comprises raw materials such as modified phenolic resin, flame retardant microcapsules, composite fibers, flake graphite, petroleum coke, aluminum oxide, friction powder, calcium carbonate, vermiculite powder, precipitated barium sulfate, and zinc stearate.
[0012] The synthesized modified phenolic resin is obtained by introducing hindered phenol and thiophene structures into the phenolic resin through reaction. The epoxy group of the epoxy product 2 containing hindered phenol and thiophene can react with the phenolic hydroxyl group in the phenolic resin. After the phenolic hydroxyl group is consumed, the water resistance of the modified phenolic resin is improved; the hindered phenol structure can quickly terminate the oxidative degradation reaction of the polymer to prevent the oxidation reaction from continuing. When exposed to ultraviolet rays, the thiophene ring can effectively absorb ultraviolet energy and convert it into low-energy heat energy for release. The hindered phenol and the thiophene ring produce intramolecular synergy to prevent the phenolic resin from being subjected to oxidative degradation reactions caused by heat and ultraviolet rays, thereby improving the oxidation resistance of the brake pad friction material.
[0013] The flame retardant microcapsules are microcapsules obtained by using the synthesized modified phenolic resin as the wall material and ammonium polyphosphate as the core material, and the wall material covers the core material. After the ammonium polyphosphate is coated with the modified phenolic resin, its compatibility with the matrix of the brake pad friction material, i.e., the modified phenolic resin, is increased, so that the flame retardant performance of the brake pad friction material is significantly improved, and the low degree of polymerization and high hygroscopicity of the ammonium polyphosphate caused by process defects can be avoided to have adverse effects on the material properties; the hindered phenol and thiophene structures contained in the modified phenolic resin also make the flame retardant microcapsule wall material have strong antioxidant properties, so as to avoid the wall material from oxidative degradation and losing its protective effect on the core material, which is beneficial to the storage and transportation of the flame retardant microcapsules and enables the brake pad friction material to maintain stable flame retardant properties. DETAILED DESCRIPTION
[0014] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0015] Example 1
[0016] A modified phenolic resin, the preparation of which comprises the following steps: Step A1: Add 2-thiophene methanol to toluene, start stirring, then add sodium hydroxide solution, stir for 5 minutes, then drop epichlorohydrin, stir and react at room temperature for 6 hours, filter, extract and dry to obtain epoxy product 1; the dosage ratio of 2-thiophene methanol, toluene, sodium hydroxide solution and epichlorohydrin is 0.1 mol: 85 mL: 5 mL: 0.1 mol, and the mass fraction of sodium hydroxide solution is 5%; Step A2: In a nitrogen atmosphere, 3,5-di-tert-butyl-4-hydroxyphenylacetic acid was added to toluene, the temperature was raised to 45°C, pyridine was added, stirring was started, and then the epoxy product 1 was added, stirring was carried out for 8 hours, and then the temperature was raised to 110°C and stirred for 1 hour to obtain an alcohol hydroxyl product; the amount ratio of 3,5-di-tert-butyl-4-hydroxyphenylacetic acid, toluene, pyridine and epoxy product 1 was 0.1 mol: 140 mL: 0.010 mol: 24 g; Step A3: add the alcoholic hydroxyl product to toluene, start stirring, then add sodium hydroxide solution, stir for 5 minutes, then drop epichlorohydrin, stir and react at room temperature for 6 hours, filter, extract and dry to obtain the epoxy product 2; the amount ratio of the alcoholic hydroxyl product, toluene, sodium hydroxide solution and epichlorohydrin is 48g:85mL:5mL:0.1mol, and the mass fraction of the sodium hydroxide solution is 10%; Step A4: Add the epoxy product 2 and the phenolic resin to methanol, then add trimethylamine, and stir the reaction at 100°C for 3 hours to obtain a modified phenolic resin; the amount ratio of the epoxy product 2, the phenolic resin, the methanol and the trimethylamine is 59g:14g:150mL:0.1mol, and the phenolic resin is a water-soluble phenolic resin.
[0017] Example 2
[0018] A modified phenolic resin, the preparation of which comprises the following steps: Step A1: Add 2-thiophene methanol to toluene, start stirring, then add sodium hydroxide solution, stir for 8 minutes, then drop epichlorohydrin, stir and react at room temperature for 6.5 hours, filter, extract and dry to obtain epoxy product 1; the dosage ratio of 2-thiophene methanol, toluene, sodium hydroxide solution and epichlorohydrin is 0.1 mol: 90 mL: 8 mL: 0.1 mol, and the mass fraction of sodium hydroxide solution is 8%; Step A2: In a nitrogen atmosphere, 3,5-di-tert-butyl-4-hydroxyphenylacetic acid was added to toluene, the temperature was raised to 47°C, pyridine was added, stirring was started, and then the epoxy product 1 was added, stirring was carried out for 9 hours, and then the temperature was raised to 115°C and stirred for 1.5 hours to obtain an alcohol hydroxyl product; the amount ratio of 3,5-di-tert-butyl-4-hydroxyphenylacetic acid, toluene, pyridine and epoxy product 1 was 0.1 mol: 145 mL: 0.013 mol: 25 g; Step A3: add the alcoholic hydroxyl product to toluene, start stirring, then add sodium hydroxide solution, stir for 8 minutes, then drop epichlorohydrin, stir and react at room temperature for 6.5 hours, filter, extract and dry to obtain the epoxy product 2; the amount ratio of the alcoholic hydroxyl product, toluene, sodium hydroxide solution and epichlorohydrin is 49g:90mL:8mL:0.1mol, and the mass fraction of the sodium hydroxide solution is 12%; Step A4: Add the epoxy product 2 and the phenolic resin to methanol, then add trimethylamine, and stir the reaction at 110°C for 3.5 hours to obtain a modified phenolic resin; the amount ratio of the epoxy product 2, the phenolic resin, the methanol and the trimethylamine is 60:15g:155mL:0.15mol, and the phenolic resin is a water-soluble phenolic resin.
[0019] Example 3
[0020] A modified phenolic resin, the preparation of which comprises the following steps: Step A1: Add 2-thiophene methanol and toluene into a flask, start stirring, then add sodium hydroxide solution, stir for 10 minutes, then drop epichlorohydrin into the flask, stir and react at room temperature for 7 hours, filter, extract and dry to obtain epoxy product 1; the dosage ratio of 2-thiophene methanol, toluene, sodium hydroxide solution and epichlorohydrin is 0.1 mol: 95 mL: 10 mL: 0.1 mol, and the mass fraction of sodium hydroxide solution is 10%; Step A2: In a nitrogen atmosphere, 3,5-di-tert-butyl-4-hydroxyphenylacetic acid was added to toluene, the temperature was raised to 50°C, pyridine was added, stirring was started, and then the epoxy product 1 was added, stirring was carried out for 10 hours, and then the temperature was raised to 120°C and stirred for 2 hours to obtain an alcohol hydroxyl product; the amount ratio of 3,5-di-tert-butyl-4-hydroxyphenylacetic acid, toluene, pyridine and epoxy product 1 was 0.1 mol: 150 mL: 0.015 mol: 26 g; Step A3: Add the alcoholic hydroxyl product to toluene, start stirring, then add sodium hydroxide solution, stir for 10 minutes, then drop epichlorohydrin, stir and react at room temperature for 7 hours, filter, extract and dry to obtain the epoxy product 2; the amount ratio of the alcoholic hydroxyl product, toluene, sodium hydroxide solution and epichlorohydrin is 50g:95mL:10mL:0.1mol, and the mass fraction of the sodium hydroxide solution is 15%; Step A4: Add the epoxy product 2 and the phenolic resin to methanol, then add trimethylamine, and stir the reaction at 120°C for 4 hours to obtain a modified phenolic resin; the amount ratio of the epoxy product 2, the phenolic resin, the methanol and the trimethylamine is 61g:16g:160mL:0.2mol, and the phenolic resin is a water-soluble phenolic resin.
[0021] Example 4
[0022] A flame retardant microcapsule, the preparation of which comprises the following steps: Add ammonium polyphosphate to 1,4-dioxane and stir for 10 minutes to obtain dispersion a, then add the wall material to 1,4-dioxane and stir for 30 minutes to obtain dispersion b, then add dispersion a to dispersion b, stir and react for 4 hours to obtain flame retardant microcapsules; the amount ratio of ammonium polyphosphate to 1,4-dioxane in dispersion a is 1g:6mL; the amount ratio of wall material to 1,4-dioxane in dispersion b is 1.5g:15mL; the amount ratio of dispersion a to dispersion b is 14mL:32mL; the wall material uses the modified phenolic resin prepared in Example 1.
[0023] Example 5
[0024] A flame retardant microcapsule, the preparation of which comprises the following steps: Add ammonium polyphosphate to 1,4-dioxane and stir for 13 minutes to obtain dispersion a, then add the wall material to 1,4-dioxane and stir for 33 minutes to obtain dispersion b, then add dispersion a to dispersion b, stir and react for 4.5 hours to obtain flame retardant microcapsules; the amount ratio of ammonium polyphosphate to 1,4-dioxane in dispersion a is 1.3g:7mL; the amount ratio of wall material to 1,4-dioxane in dispersion b is 1.6g:18mL; the amount ratio of dispersion a to dispersion b is 16mL:34mL; the wall material uses the modified phenolic resin prepared in Example 2.
[0025] Example 6
[0026] A flame retardant microcapsule, the preparation of which comprises the following steps: Add ammonium polyphosphate to 1,4-dioxane and stir for 15 minutes to obtain dispersion a, then add the wall material to 1,4-dioxane and stir for 35 minutes to obtain dispersion b, then add dispersion a to dispersion b, stir and react for 5 hours to obtain flame retardant microcapsules; the amount ratio of ammonium polyphosphate to 1,4-dioxane in dispersion a is 1.5g:8mL; the amount ratio of wall material to 1,4-dioxane in dispersion b is 1.7g:20mL; the amount ratio of dispersion a to dispersion b is 18mL:36mL; the wall material uses the modified phenolic resin prepared in Example 3.
[0027] Example 7
[0028] A polymer brake pad friction material, comprising the following raw materials in parts by weight: 9 parts of modified phenolic resin, 1 part of flame retardant microcapsules, 26 parts of composite fibers, 7 parts of flake graphite, 6 parts of petroleum coke, 5 parts of aluminum oxide, 1 part of friction powder, 12 parts of calcium carbonate, 4 parts of vermiculite powder, 20 parts of precipitated barium sulfate, and 1 part of zinc stearate; The mass ratio of coconut fiber, areca palm fiber and basalt fiber in the composite fiber is 2:1:10; The preparation of the polymer brake pad friction material comprises the following steps: Step S1: mixing and stirring the composite fibers at a stirring speed of 700 rpm for 5 minutes to obtain a mixed fiber material; Step S2: further stirring and mixing the modified phenolic resin obtained in Example 1, the flame retardant microcapsules obtained in Example 4, flake graphite, petroleum coke, aluminum oxide, friction powder, calcium carbonate, vermiculite powder, precipitated barium sulfate, zinc stearate and the mixed fiber material at a stirring speed of 1400 rpm to obtain a mixture; Step S3: adding the mixture into the mold cavity of the hot press for hot pressing molding treatment, and then subjecting the mixture to heat treatment in a heat treatment drying oven, cutting and flat grinding on a sample cutting and grinding machine to obtain a polymer brake pad friction material; the hot press mold cavity is first preheated to 150°C, the hot pressing temperature is 170°C, and the hot pressing pressure is 11MPa; the total number of holding pressures is 6 times, the holding time for the 1st and 2nd times is 5s, the holding time for the 3rd, 4th and 5th times is 10s, and the holding time for the 6th time is 15min; the total number of exhausts is 6 times, the exhaust time for the 1st, 2nd, 3rd, 4th and 5th times is 5s, and the exhaust time for the 6th time is 30s; the temperature of the heat treatment drying oven is linearly increased to 140°C within 2h, kept warm for 1h, then linearly increased to 160°C within 1h, kept warm for 3h, then linearly increased to 180°C within 1h, kept warm for 6h, and then cooled to room temperature.
[0029] Example 8
[0030] A polymer brake pad friction material, comprising the following raw materials in parts by weight: 10 parts of modified phenolic resin, 2 parts of flame retardant microcapsules, 29 parts of composite fibers, 8 parts of flake graphite, 7 parts of petroleum coke, 6 parts of aluminum oxide, 2 parts of friction powder, 13 parts of calcium carbonate, 5 parts of vermiculite powder, 21 parts of precipitated barium sulfate, and 1.5 parts of zinc stearate; The mass ratio of coconut fiber, areca palm fiber and basalt fiber in the composite fiber is 3:1.5:13; The preparation of the polymer brake pad friction material comprises the following steps: Step S1: mixing and stirring the composite fibers at a stirring speed of 700 rpm for 8 minutes to obtain a mixed fiber material; Step S2: further stirring and mixing the modified phenolic resin obtained in Example 2, the flame retardant microcapsules obtained in Example 5, flake graphite, petroleum coke, aluminum oxide, friction powder, calcium carbonate, vermiculite powder, precipitated barium sulfate, zinc stearate and the mixed fiber material at a stirring speed of 1450 rpm to obtain a mixture; Step S3: adding the mixture into the mold cavity of the hot press for hot pressing molding, and then subjecting the mixture to heat treatment in a heat treatment drying oven, cutting and flat grinding on a sample cutting and grinding machine to obtain a polymer brake pad friction material; the hot press mold cavity is first preheated to 155°C, the hot pressing temperature is 175°C, and the hot pressing pressure is 12MPa; the total number of holding pressures is 6 times, the holding time for the 1st and 2nd times is 8s, the holding time for the 3rd, 4th and 5th times is 13s, and the holding time for the 6th time is 18min; the total number of exhausts is 6 times, the exhaust time for the 1st, 2nd, 3rd, 4th and 5th times is 8s, and the exhaust time for the 6th time is 37s; the temperature of the heat treatment drying oven is linearly increased to 140°C within 2h, kept warm for 1.3h, then linearly increased to 160°C within 1h, kept warm for 3.3h, then linearly increased to 180°C within 1h, kept warm for 6.5h, and then cooled to room temperature.
[0031] Example 9
[0032] A polymer brake pad friction material, comprising the following raw materials in parts by weight: 11 parts of modified phenolic resin, 3 parts of flame retardant microcapsules, 32 parts of composite fibers, 9 parts of flake graphite, 8 parts of petroleum coke, 7 parts of aluminum oxide, 3 parts of friction powder, 14 parts of calcium carbonate, 6 parts of vermiculite powder, 22 parts of precipitated barium sulfate, and 2 parts of zinc stearate; The mass ratio of coconut fiber, areca palm fiber and basalt fiber in the composite fiber is 4:2:15; The preparation of the polymer brake pad friction material comprises the following steps: Step S1: mixing and stirring the composite fibers at a stirring speed of 800 rpm for 10 min to obtain a mixed fiber material; Step S2: further stirring and mixing the modified phenolic resin obtained in Example 3, the flame retardant microcapsules obtained in Example 6, flake graphite, petroleum coke, aluminum oxide, friction powder, calcium carbonate, vermiculite powder, precipitated barium sulfate, zinc stearate and the mixed fiber material at a stirring speed of 1500 rpm to obtain a mixture; Step S3: adding the mixture into the mold cavity of the hot press for hot pressing molding, and then subjecting the mixture to heat treatment in a heat treatment drying oven, cutting and flat grinding on a sample cutting and grinding machine to obtain a polymer brake pad friction material; the hot press mold cavity is first preheated to 160°C, the hot pressing temperature is 180°C, and the hot pressing pressure is 13MPa; the total number of holding pressures is 6 times, the holding time for the 1st and 2nd times is 10s, the holding time for the 3rd, 4th and 5th times is 15s, and the holding time for the 6th time is 20min; the total number of exhausts is 6 times, the exhaust time for the 1st, 2nd, 3rd, 4th and 5th times is 10s, and the exhaust time for the 6th time is 45s; the temperature of the heat treatment drying oven is linearly increased to 140°C within 2h, kept warm for 1.5h, then linearly increased to 160°C within 1h, kept warm for 3.5h, then linearly increased to 180°C within 1h, kept warm for 7h, and then cooled to room temperature.
[0033] Comparative Example 1 Compared with Example 9, the modified phenolic resin used was replaced with an unmodified water-soluble phenolic resin, that is, no hindered phenol and thiophene ring were introduced into the phenolic resin. The rest was exactly the same as Example 9 to prepare a polymer brake pad friction material.
[0034] Comparative Example 2 Compared with Example 9, the epoxy product 2 in step A4 during the preparation of the modified phenolic resin is replaced with the epoxy product 1 in step A1, that is, only the thiophene ring is introduced into the phenolic resin without introducing the hindered phenol, and the rest is exactly the same as in Example 9 to obtain a polymer brake pad friction material.
[0035] Comparative Example 3 Compared with Example 9, the flame retardant microcapsules were replaced with ammonium polyphosphate, and the rest was exactly the same as Example 9 to obtain a polymer brake pad friction material.
[0036] Comparative Example 4 Compared with Example 9, the wall material of the flame retardant microcapsule was replaced with unmodified water-soluble phenolic resin, and the rest was exactly the same as Example 9 to obtain a polymer brake pad friction material.
[0037] The effect of the polymer brake pad friction material prepared by the present invention is further tested below, and the test results are as follows.
[0038] In order to test the polymer brake pad friction material prepared by the present invention, the oxygen index was tested with reference to GB / T2406.1-2008 "Determination of Combustion Behavior of Plastics by Oxygen Index Method" standard; the brake pad material was immersed in distilled water at room temperature for 3 days with reference to GB / T34007-2017 standard, and the friction coefficient before and after immersion was measured; the brake pad friction material was placed in a strength of 1000W / m 2 After irradiation with ultraviolet light for 200 hours, the friction coefficient and oxygen index were measured, and the results are recorded in Table 1; Table 1: Test results Example 7 Example 8 Example 9 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Oxygen index (%) 61.5 61.8 62.3 62.2 62.1 56.8 62.2 Oxygen index after UV aging (%) 61.0 61.3 61.9 58.3 59.6 56.4 57.2 Friction coefficient before immersion 0.48 0.52 0.53 0.50 0.52 0.53 0.52 Friction coefficient after immersion 0.47 0.51 0.52 0.30 0.51 0.52 0.52 Friction coefficient after UV aging 0.48 0.52 0.52 0.32 0.44 0.51 0.51 According to the data in Table 1, the polymer brake pad friction material of the present invention has excellent flame retardant properties, water resistance, oxidation resistance and flame retardant properties. Comparison between Example 9 and Comparative Example 1 shows that the water resistance of the brake pad friction material is very poor because the hindered phenol and thiophene ring are not introduced into the phenolic resin, and the phenolic hydroxyl group is not consumed, resulting in poor water resistance, and the friction coefficient cannot be maintained stably after being soaked in water, and the friction performance is poor, so that the modified phenolic resin has poor oxidation resistance, and the flame retardant property of the modified phenolic resin matrix decreases due to oxidation degradation, which is not conducive to the stable maintenance of the friction coefficient of the friction material after ultraviolet aging, and the oxygen index of the friction material decreases; Comparison between Example 9 and Comparative Example 2 shows that the phenolic resin is modified by using the epoxy product 1 containing only thiophene rings, and only the thiophene rings play an antioxidant role, and the friction coefficient of the friction material cannot be stably maintained after ultraviolet aging, and the flame retardant property of the modified phenolic resin matrix decreases due to the decrease in antioxidant effect, and the oxygen index decreases; Comparison between Example 9 and Comparative Example 3 shows that the direct addition of ammonium polyphosphate has poor compatibility with the modified phenolic resin, and the oxygen index of the friction material decreases more. Comparison of Example 9 with Comparative Example 4 shows that by using ordinary unmodified phenolic resin as the wall material of flame retardant microcapsules without introducing hindered phenol and thiophene rings, the antioxidant property of the flame retardant microcapsule wall material decreases, and after ultraviolet oxidation, the oxygen index decreases, and the flame retardant performance of the brake pad friction material decreases.
[0039] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.
Claims
1. A polymer brake pad friction material, characterized by: The invention comprises the following raw materials in parts by weight: 9-11 parts of modified phenolic resin, 1-3 parts of flame retardant microcapsules, 26-32 parts of composite fibers, 7-9 parts of flake graphite, 6-8 parts of petroleum coke, 5-7 parts of aluminum oxide, 1-3 parts of friction powder, 12-14 parts of calcium carbonate, 4-6 parts of vermiculite powder, 20-22 parts of precipitated barium sulfate, and 1-2 parts of zinc stearate; The modified phenolic resin is prepared by the following steps: Step A1: Add 2-thiophene methanol to toluene, start stirring, then add sodium hydroxide solution, stir for 5-10 minutes, then dropwise add epichlorohydrin, stir and react at room temperature for 6-7 hours, filter, extract and dry to obtain the epoxy product 1; Step A2: In a protective gas atmosphere, add 3,5-di-tert-butyl-4-hydroxyphenylacetic acid to toluene, heat to 45-50° C., add pyridine, start stirring, then add the epoxy product 1, stir and react for 8-10 hours, then heat to 110-120° C., stir for 1-2 hours to obtain an alcohol hydroxyl product; Step A3: Add the alcoholic hydroxyl product to toluene, start stirring, then add sodium hydroxide solution, stir for 5-10 minutes, then dropwise add epichlorohydrin, stir and react at room temperature for 6-7 hours, filter, extract and dry to obtain the epoxy product 2; Step A4: Add the epoxy product 2 and the phenolic resin into methanol, then add trimethylamine, and stir the mixture at 100-120° C. for 3-4 hours to obtain a modified phenolic resin.
2. The polymer brake pad friction material according to claim 1, characterized in that: In step A1, the amount ratio of 2-thiophene methanol, toluene, sodium hydroxide solution and epichlorohydrin is 0.1 mol: 85-95 mL: 5-10 mL: 0.1 mol, and the mass fraction of the sodium hydroxide solution is 5-10%; in step A2, the amount ratio of 3,5-di-tert-butyl-4-hydroxyphenylacetic acid, toluene, pyridine and epoxidation product 1 is 0.1 mol: 140-150 mL: 0.010-0.015 mol: 24-26 g.
3. The polymer brake pad friction material according to claim 1, characterized in that: In step A3, the amount ratio of the alcohol hydroxyl product, toluene, sodium hydroxide solution and epichlorohydrin is 48-50g:85-95mL:5-10mL:0.1mol, and the mass fraction of the sodium hydroxide solution is 10-15%; in step A4, the amount ratio of the epoxy product 2, phenolic resin, methanol and trimethylamine is 59-61g:14-16g:150-160mL:0.1-0.2mol, and the phenolic resin is a water-soluble phenolic resin.
4. The polymer brake pad friction material according to claim 1, characterized in that: The flame retardant microcapsules are prepared by the following steps: Add ammonium polyphosphate to 1,4-dioxane and stir for 10-15 minutes to obtain dispersion a, then add the wall material to 1,4-dioxane and stir for 30-35 minutes to obtain dispersion b, then add dispersion a to dispersion b, stir and react for 4-5 hours to obtain flame retardant microcapsules.
5. The polymer brake pad friction material according to claim 4, characterized in that: In the preparation of the flame retardant microcapsules, the usage ratio of ammonium polyphosphate and 1,4-dioxane in dispersion a is 1-1.5 g: 6-8 mL; the usage ratio of wall material and 1,4-dioxane in dispersion b is 1.5-1.7 g: 15-20 mL; the usage ratio of dispersion a and dispersion b is 14-18 mL: 32-36 mL; the wall material is the prepared modified phenolic resin.
6. A polymer brake pad friction material according to claim 1, wherein the mass ratio of coconut fiber, areca palm fiber and basalt fiber in the composite fiber is 2-4:1-2:10-15.
7. A method for preparing the polymer brake pad friction material according to any one of claims 1 to 6, characterized in that: The steps include: Step S1: mixing and stirring the composite fibers to obtain a mixed fiber material; Step S2: further stirring and mixing the modified phenolic resin, flame retardant microcapsules, flake graphite, petroleum coke, aluminum oxide, friction powder, calcium carbonate, vermiculite powder, precipitated barium sulfate, zinc stearate and the mixed fiber material to obtain a mixture; Step S3: adding the mixture into a mold cavity of a hot press to perform hot pressing molding, and then heat treating it in a heat treatment drying oven, and then cutting and flat grinding to obtain a polymer brake pad friction material.
8. The method for preparing a polymer brake pad friction material according to claim 7, characterized in that: In step S1, the stirring speed is 700-800 rpm and the stirring time is 5-10 min; in step S2, the stirring speed is 1400-1500 rpm and the stirring time is 10-15 min.
9. The method for preparing a polymer brake pad friction material according to claim 7, characterized in that: In step S3, the hot press cavity is first preheated to 150-160°C, the hot pressing temperature is 170-180°C, and the hot pressing pressure is 11-13MPa; the total number of holding times is 6 times, the holding time for the 1st and 2nd times is 5-10s, the holding time for the 3rd, 4th and 5th times is 10-15s, and the holding time for the 6th time is 15-20min; a total of 6 exhaust times are performed, the exhaust time for the 1st, 2nd, 3rd, 4th and 5th times is 5-10s, and the exhaust time for the 6th time is 30-45s.
10. The method for preparing a polymer brake pad friction material according to claim 7, characterized in that: In step S3, the temperature of the heat treatment drying oven is linearly increased to 140°C within 2 hours, kept warm for 1-1.5 hours, then linearly increased to 160°C within 1 hour, kept warm for 3-3.5 hours, then linearly increased to 180°C within 1 hour, kept warm for 6-7 hours, and then dropped to room temperature.
Citation Information
Patent Citations
Waterproof plastic material and preparation method thereof
CN116063835A
Production process of modified phenolic resin brake pad