Poly (phthalazinone) polyarylether resin-based composite material pipe product and preparation method thereof

By using pipe products prepared by heteronaphthalene biphenyl polyarylether resin-based composite materials, the problem of aging of metal pipes in complex environments is solved, and excellent high-temperature mechanical properties, corrosion resistance and resistance are achieved 磨的效果,提供了替代金属材料的解决方案。

CN119060523APending Publication Date: 2024-12-03DALIAN UNIV OF TECH +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411396105.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-08
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Metal material pipes have short service life, heavy self-weight, serious corrosion, and high processing and forming costs in complex environments. Ordinary plastics age under high temperature environments and have poor temperature resistance.

Method used

Tube products made of heteronaphthalene biphenyl polyarylether resin-based composite materials are prepared by drying, premixing, melt blending, granulation and extrusion molding or injection molding processes to prepare density below 1.6g/cm3. The glass transition temperature is 250℃-370℃ and the pipes and connecting parts can be adjusted, with excellent high-temperature mechanical properties, corrosion resistance, radiation resistance and wear resistance.

Benefits of technology

It realizes lightweight, high-strength, corrosion-resistant, radiation-resistant and wear-resistant pipes and connecting parts in high temperature environments, which can replace metal materials, extend the use cycle, reduce processing costs, and be used in petrochemicals, vehicles, ships, aerospace, etc. There are good application prospects in the field.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119060523A_ABST
    Figure CN119060523A_ABST
Patent Text Reader

Abstract

The invention provides a pipe product made of a phthalazinone polyarylether resin-based composite material and a preparation method of the pipe product, and belongs to the technical field of advanced resin-based composite materials. According to the invention, one or more phthalazinone polyarylether resin, a fluidity improving auxiliary agent, a reinforcing body and a functional filler are subjected to melt blending, a composite material pipe is stably and continuously formed by using a single screw extruder under the conditions that the temperature range is 340-400 DEG C and the melt pressure is 10-40MPa, and a connecting part is prepared through an injection molding process; finally, the phthalazinone polyarylether resin-based composite material pipe and the connecting part which have the advantages of light weight, high strength, high temperature resistance, corrosion resistance, wear resistance, radiation resistance and the like are obtained, so that the phthalazinone polyarylether resin-based composite material pipe and the connecting part replace metal pipes to serve in complex environments, and the phthalazinone polyarylether resin-based composite material pipe and the connecting part have wide application prospects and outstanding practical values in the fields of petrochemical engineering, vehicles, ships, aerospace and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of advanced resin-based composite materials, and in particular to a pipe product of a poly(phthalazine biphenyl) polyarylether resin-based composite material and a preparation method thereof. Background Art

[0002] With the development of the times, the requirements for the use of pipes in different environments are becoming more and more complex, and the disadvantages of using metal pipes and connecting parts in the fields of shipbuilding, aerospace, energy, vehicles, etc. are becoming increasingly prominent, such as weak corrosion resistance in acidic and saline-alkali environments, heavy weight due to high density, high energy consumption in the molding process, difficult installation and processing, and high maintenance costs due to frequent replacement. It is urgent to develop new material pipes to adapt to the development trend.

[0003] Compared with metals, plastics have a series of advantages such as light weight, easy processing and molding, and corrosion resistance. Under such a background, "replacing steel with plastics" has become a new research and development trend. Plastic pipes at room temperature have been used in all aspects of life, such as water supply and drainage pipes, wear-resistant pipes, fiber-wound pipes, etc., and have good use effects. However, the use of ordinary plastics in high temperature environments is still limited due to poor temperature resistance and other reasons. They are usually used in the form of plastic coated on the metal surface, which solves the problem of metal corrosion to a certain extent, but fails to completely solve the problem of the weight of metal materials. At the same time, ordinary plastics are prone to aging in high temperature environments, and their use time is greatly reduced.

[0004] Dalian University of Technology and Dalian Baolimo New Materials Co., Ltd. have applied for patents for a series of high-performance engineering plastics and composite materials of poly(arylether) of phthalated biphenyls (CN03111540.3, CN93109179.9, CN03111540.3, CN201410201589.1). The glass transition temperature of this series of high-performance engineering plastics can be adjusted in the range of 250℃-370℃, and the use temperature is higher than 200℃. It has the advantages of both melting and solution processing, and still maintains good mechanical properties in high-temperature use environments, making it a suitable material for pipe processing. However, the high viscosity and high processing temperature of poly(arylether) of phthalated biphenyls resins themselves make their pipe processing and molding technology different from conventional polymers. In order to make the molded pipes have light weight and high strength, use temperature greater than 200℃, excellent high-temperature mechanical properties, corrosion resistance and other properties, give full play to the advantages of poly(arylether) of phthalated biphenyls high-performance engineering resins and composite materials, and replace metal pipes in various complex environments, the present invention is specially proposed. Summary of the invention

[0005] The object of the present invention is to provide a pipe product of a poly(arylene ether) resin-based composite material and a preparation method thereof. The pipe product fully utilizes the advantages of the poly(arylene ether) resin and its composite material, has the characteristics of light weight and high strength, operating temperature greater than 200°C, corrosion resistance, radiation resistance, good wear resistance, good sealing, safety and reliability, etc., can replace metal pipes in various environments, and solve the problems of short service life, heavy weight, severe corrosion and high processing and molding cost of metal pipes and their connectors in complex environments.

[0006] In order to achieve the above object, the present invention provides the following technical solutions:

[0007] In a first aspect, a pipe product of a poly(arylene ether) resin-based composite material, wherein the pipe product is a pipe and / or a connecting component for a pipe, wherein the pipe and the connecting component are both made of the poly(arylene ether) resin-based composite material, and the raw materials of the poly(arylene ether) resin-based composite material include the following components in parts by weight:

[0008] Phthalate polyarylether resin matrix: 100 parts;

[0009] Flowability improving agent: 10-30 parts;

[0010] Reinforcement: 15-30 parts;

[0011] Functional filler: 0-10 parts;

[0012] The poly(arylene ether) phthalazine resin matrix comprises at least one of the following resins: PPESK, PPES, PPEK, PPENS, PPENK, PPEKK and PPENSK, and PPBESK, PPBES, PPBEK and PPBESKK containing biphenyl structures;

[0013] The general structural formula of the PPESK, PPES, PPEK, PPENS, PPENK, PPENSK, PPBESK, PPBES, PPBEK, PPEKK and PPBESKK is:

[0014]

[0015] Wherein, when the resin structure does not contain a biphenyl structure, Ar is:

[0016] When the resin structure contains a biphenyl structure, Ar is The sum of the two proportions is 100%; R1, R2, R3 and R4 are each independently selected from hydrogen, a halogen substituent, a phenyl group, a phenoxy group, an alkyl group or an alkoxy group, the alkyl group or the alkoxy group contains at least one carbon atom, and the structures of R1, R2, R3 and R4 are the same or different;

[0017] Where: PPESK: a≥3, b≥3, c=0, d=0;

[0018] PPES: a≥3, b=0, c=0, d=0;

[0019] PPEK: a=0, b≥3, c=0, d=0;

[0020] PPENS: a≥3, b=0, c=0, d≥3;

[0021] PPENK: a=0, b≥3, c=0, d≥3;

[0022] PPENSK: a≥3, b≥3, c=0, d≥3;

[0023] PPBESK: a≥3, b≥3, c=0, d=0;

[0024] PPBES: a≥3, b=0, c=0, d=0;

[0025] PPBEK: a=0, b≥3, c=0, d=0;

[0026] PPEKK: a=0, b=0, c≥3, d=0;

[0027] PPBESKK: a≥3, b=0, c≥3, d=0.

[0028] Further, the fluidity improving agent includes at least one of polyamide, polysulfone, polyethersulfone, polyetheretherketone, polyetherketoneketone, polyetherimide, and polyphenylene sulfide;

[0029] And / or, the reinforcement comprises fibers having a length between 2 μm and 5 mm, wherein the fibers comprise at least one of carbon fibers, glass fibers, basalt fibers, and quartz fibers;

[0030] And / or, the functional filler includes at least one of graphite powder, nano-silicon dioxide, nano-silicon carbide, nano-silicon nitride, nano-calcium carbonate, nano-metal powder, and porous carbon.

[0031] Furthermore, the number average molecular weight of the poly(arylene ether) phthalazine resin matrix is ​​10,000-40,000 g / mol; and / or the melt index of the fluidity improving agent is 20-70 g / 10 minutes.

[0032] Furthermore, the preparation method of the pipe comprises: drying, premixing, melt blending and granulating the raw materials in sequence to obtain blend particles; drying and extruding the blend particles to obtain the pipe;

[0033] And / or, the axial tensile strength of the pipe is 90-180 MPa, the circumferential bursting stress is 40-90 MPa, and the density is less than 1.6 g / cm 3 .

[0034] Furthermore, the preparation method of the connecting component comprises: drying, premixing, melt blending, and granulating the raw materials in sequence to obtain blend particles; drying and injection molding the blend particles to obtain the connecting component;

[0035] And / or, the density of the connecting component is lower than 1.6 g / cm 3 .

[0036] Furthermore, in the method for preparing the pipe and / or the connecting component, the drying temperature is 120-180°C; and / or the melt blending temperature is 330-400°C; and / or the length of the blend particles is less than 8 mm.

[0037] Furthermore, in the method for preparing the pipe, the extrusion molding temperature is 340-400°C, the melt pressure is 10-40MPa, and the screw speed is 1-20rpm;

[0038] And / or, in the preparation method of the connecting component, the injection molding temperature is 340-400° C., the injection pressure is 30-130 MPa, the connecting component molding mold temperature is 80-200° C., and the cooling time is 10-90 s.

[0039] In a second aspect, a method for preparing a tube product of the poly(phenylene ether) resin-based composite material of the first aspect comprises drying, premixing, melt blending, and granulating the raw materials in sequence to obtain blend particles;

[0040] The method for preparing the pipe comprises: drying and extruding the blend particles to obtain the pipe;

[0041] The preparation method of the connecting component comprises: drying and injection molding the blend particles to obtain the connecting component.

[0042] Furthermore, in the method for preparing the pipe and / or the connecting component, the drying temperature is 120-180° C.; and / or the melt blending temperature is 330-400° C.; and / or the length of the blend particles is less than 8 mm.

[0043] Furthermore, in the method for preparing the pipe, the extrusion molding temperature is 340-400°C, the melt pressure is 10-40MPa, and the screw speed is 1-20rpm;

[0044] And / or, in the preparation method of the connecting component, the injection molding temperature is 340-400° C., the injection pressure is 30-130 MPa, the connecting component molding mold temperature is 80-200° C., and the cooling time is 10-90 s.

[0045] The present invention provides a pipe product (pipe and connecting component) of a poly(phenylene ether) resin-based composite material and a preparation method thereof, which has the following beneficial effects:

[0046] 1. The pipe and connecting parts of the poly(phenylene ether) resin-based composite material of the present invention have a density lower than 1.6 g / cm 3 The glass transition temperature is adjustable between 250℃ and 370℃, the use temperature is higher than 200℃, the corrosion resistance is excellent, and it has the properties of wear resistance, impact resistance, and radiation resistance. It can be used in various complex environments to replace metal pipes, and has good application prospects in various industries such as petrochemical, vehicles and ships, and aerospace.

[0047] 2. The pipe of the poly(phenylene)phthalate resin-based composite material of the present invention has a tensile strength range of 90-180 MPa and a circumferential bursting stress range of 40-90 MPa according to the raw material ratio.

[0048] 3. The preparation method of the pipe and connecting parts of the poly(phenylene ether) resin-based composite material of the present invention can be obtained by using existing technical equipment, which is easy to operate, and the process conditions are simple and easy to achieve. The formed pipe has a uniform diameter and a glossy appearance, and the connecting parts have a complex shape and are precise, and both have excellent performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0049] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0050] Figure 1 A schematic structural diagram of a connecting component with a complex thread structure provided in an embodiment of the present invention. DETAILED DESCRIPTION

[0051] In order to make the purpose, technical scheme and advantages of the present invention clearer, the technical scheme in the embodiment of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention. The process parameters of the following embodiments that do not specify specific conditions are usually based on conventional conditions.

[0052] The endpoints and any values ​​of the ranges disclosed in the present invention are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be regarded as specifically disclosed in the present invention.

[0053] According to a first aspect of the present invention, there is provided a pipe product of a poly(arylene ether) resin-based composite material, wherein the pipe product is a pipe and / or a connecting component for the pipe, wherein the pipe and the connecting component are both made of the poly(arylene ether) resin-based composite material, and the raw materials of the poly(arylene ether) resin-based composite material include the following components in parts by weight:

[0054] Phthalate polyarylether resin matrix: 100 parts;

[0055] Flowability improving agent: 10-30 parts;

[0056] Reinforcement: 15-30 parts;

[0057] Functional filler: 0-10 parts;

[0058] The polyarylether phthalate resin matrix comprises at least one of the following resins: polyarylether sulfoneketone (PPESK), polyarylether sulfone (PPES), polyarylether ketone (PPEK), polyarylether nitrile sulfone (PPENS), polyarylether nitrile ketone (PPENK), polyarylether nitrile sulfone ketone (PPENSK), polyarylether ketone ketone (PPEKK), polyarylether sulfone ketone containing biphenyl structure (PPBESK), polyarylether sulfone containing biphenyl structure (PPBES), polyarylether ketone containing biphenyl structure (PPBEK), polyarylether sulfone ketone ketone (PPBESKK) containing biphenyl structure.

[0059] The general structural formula of the PPESK, PPES, PPEK, PPENS, PPENK, PPENSK, PPBESK, PPBES, PPBEK, PPEKK and PPBESKK is:

[0060]

[0061] When the resin structure does not contain a biphenyl structure, Ar is: When the resin structure contains a biphenyl structure, Ar is The sum of the two proportions is 100%. R1, R2, R3 and R4 are independently selected from hydrogen, halogen substituents, phenyl, phenoxy, alkyl or alkoxy, and the alkyl or alkoxy group contains at least 1 carbon atom, and the structures of R1, R2, R3 and R4 are the same or different.

[0062] Where: PPESK: a≥3, b≥3, c=0, d=0;

[0063] PPES: a≥3, b=0, c=0, d=0;

[0064] PPEK: a=0, b≥3, c=0, d=0;

[0065] PPENS: a≥3, b=0, c=0, d≥3;

[0066] PPENK: a=0, b≥3, c=0, d≥3;

[0067] PPENSK: a≥3, b≥3, c=0, d≥3;

[0068] PPBESK: a≥3, b≥3, c=0, d=0;

[0069] PPBES: a≥3, b=0, c=0, d=0;

[0070] PPBEK: a=0, b≥3, c=0, d=0;

[0071] PPEKK: a=0, b=0, c≥3, d=0;

[0072] PPBESKK: a≥3, b=0, c≥3, d=0.

[0073] The pipe of the present invention is regulated according to the raw material ratio, and the tensile strength of the pipe is in the range of 90-180MPa; the circumferential bursting stress is in the range of 40-90MPa, and the density is lower than 1.6g / cm 3, the glass transition temperature is adjustable at 250-370°C, the operating temperature is higher than 200°C, it has excellent corrosion resistance, and has the properties of wear resistance, impact resistance, and radiation resistance; it can be used in various complex environments to replace metal pipes, and has good application prospects in various industries. In the raw materials for the pipe products of the present invention, the polyphenylene ether resin matrix (resin matrix) of polyphenylene ether can be selected from polyphenylene ether high-performance engineering resins. Specifically, the polyphenylene ether resin matrix of the present invention is divided into two categories, one of which contains a biphenyl structure, and Ar can be optionally selected from and These two groups are not connected to each other, and their specific proportions can be adjusted, and the sum of their proportions is 100%.

[0074] When configuring the raw materials of the pipe and its connecting parts of the present invention, in order to give full play to the advantages of the high-performance engineering resin and its composite materials of phthalated biphenyl polyarylether, the molded pipe and connecting parts have the properties of light weight and high strength, use temperature greater than 200°C, excellent high-temperature mechanical properties, corrosion resistance, etc., after a lot of research, it is found that by adding 10-30 parts of a polymer with good fluidity and close to the processing window of the resin matrix as a fluidity improvement agent in the raw materials, the processing viscosity of the resin matrix itself can be reduced, the processing performance can be improved, and the existing pipe preparation equipment such as a single screw extruder and a plastic injection molding machine can be used to achieve preparation, and obtain pipe products that can replace metal materials. However, if the content of the fluidity improvement agent is too high or too low, it will cause adverse effects. For example, a high content will cause the mechanical properties of the product to be poor, and a low content will increase the difficulty of composite material processing and cannot be formed.

[0075] Functional fillers can be added selectively. After addition, the function of the functional fillers is to bring wear resistance, reinforcement and toughness enhancement to the pipe and its connecting parts.

[0076] Therefore, when the raw materials of the present invention are configured, the fluidity improving agent can be typically but not limited to 11 parts, 12 parts, 13 parts, 14 parts, 15 parts, 16 parts, 17 parts, 18 parts, 19 parts, 20 parts, 21 parts, 22 parts, 23 parts, 24 parts, 25 parts, 26 parts, 27 parts, 28 parts, 29 parts; the reinforcement can be typically but not limited to 16 parts, 17 parts, 18 parts, 19 parts, 20 parts, 21 parts, 22 parts, 23 parts, 24 parts, 25 parts, 26 parts, 27 parts, 28 parts, 29 parts; the functional filler can be typically but not limited to 0 parts, 1 parts, 2 parts, 3 parts, 4 parts, 5 parts, 6 parts, 7 parts, 8 parts, 9 parts.

[0077] As an optional form of the poly(phenylene biphenyl) ether resin-based composite material pipe product of the present invention, the fluidity improving agent is 18-30 parts; and / or the reinforcing body is 20-30 parts.

[0078] As an optional form of the poly(phenylene ether) resin-based composite material pipe product of the present invention, the melt index of the fluidity improving agent is 20-70 g / 10 minutes, typically but not limitedly 21 g / 10 minutes, 25 g / 10 minutes, 30 g / 10 minutes, 35 g / 10 minutes, 40 g / 10 minutes, 45 g / 10 minutes, 50 g / 10 minutes, 55 g / 10 minutes, 60 g / 10 minutes, 65 g / 10 minutes, 68 g / 10 minutes, etc. The melt index of the fluidity improving agent needs to be adapted to the main material poly(phenylene ether) resin matrix. If the melt index is too high, the viscosity of the two materials differs too much and the fluidity cannot be improved. If it is too small, the fluidity cannot be improved either.

[0079] As an optional form of the poly(phthalazine biphenyl) ether resin-based composite material pipe product of the present invention, the fluidity improving agent includes at least one of polyamide, polysulfone, polyethersulfone, polyetheretherketone, polyetherketoneketone, polyetherimide, and polyphenylene sulfide having a melt index of 20-70 g / 10 minutes;

[0080] And / or, the reinforcement comprises fibers having a length between 2 μm and 5 mm, wherein the fibers comprise at least one of carbon fibers, glass fibers, basalt fibers, and quartz fibers;

[0081] And / or, the functional filler includes at least one of graphite powder, nano-silicon dioxide, nano-silicon carbide, nano-silicon nitride, nano-calcium carbonate, nano-metal powder, and porous carbon.

[0082] In the above technical solution, as a fluidity improving agent, polyamide with a melt index of 20-70g / 10 minutes has high fluidity, and the processing window has a certain overlap with other raw materials, which is more convenient for processing parameter control. Fibers can be reinforced, but if they are less than 2μm, the mechanical properties brought by the fiber length will be lost. Therefore, the fiber length can be typically but not limitedly selected to be 3μm, 5μm, 10μm, 100μm, 1mm, 2mm, 3mm, 4mm. Functional fillers are all nano- and / or micron-sized powders. The fluidity improving agents, reinforcements and functional fillers listed above can all be purchased directly from the market.

[0083] As an optional form of the poly(arylene ether) resin-based composite material pipe product of the present invention, the number average molecular weight of the poly(arylene ether) resin matrix is ​​10,000-40,000 g / mol. The poly(arylene ether) resin of this molecular weight has good mechanical properties. Therefore, the number average molecular weight of the poly(arylene ether) resin matrix can be typically but not limitatively selected to be 15,000 g / mol, 20,000 g / mol, 25,000 g / mol, 30,000 g / mol, or 35,000 g / mol.

[0084] The method for preparing a tubular product of a poly(arylene ether) resin-based composite material of the first aspect, i.e., the second aspect of the present invention, provides a method for preparing a tubular product (a tubular product and / or a connecting component) of a poly(arylene ether) resin-based composite material, which is specifically as follows:

[0085] A method for preparing a pipe product of a phthalazine polyarylether resin-based composite material, comprising sequentially drying, premixing, melt blending, and granulating the raw materials to obtain blend particles;

[0086] The method for preparing the pipe comprises: drying and extruding the blend particles to obtain the pipe;

[0087] The preparation method of the connecting component comprises: drying and injection molding the blend particles to obtain the connecting component.

[0088] That is, in the present invention: the preparation method of the pipe comprises: sequentially drying, premixing, melt blending and granulating the raw materials to obtain blend particles; drying and extruding the blend particles to obtain the pipe.

[0089] The preparation method of the connecting component comprises: sequentially drying, premixing, melt blending and granulating the raw materials to obtain blend particles; and drying and injection molding the blend particles to obtain the connecting component.

[0090] As an optional embodiment of the preparation method of the poly(phenylene phthalate) resin-based composite material pipe product of the present invention, in the preparation method of the pipe and / or the connecting component, the drying temperature is 120-180°C (such as 125°C, 130°C, 135°C, 140°C, 145°C, 150°C, 155°C, 160°C, 165°C, 170°C, 175°C), and a good drying effect is achieved at this temperature; the melt blending temperature is 330-400°C (such as 335°C, The temperature is preferably 340°C, 345°C, 350°C, 355°C, 360°C, 365°C, 370°C, 375°C, 380°C, 385°C, 390°C, 395°C). If the temperature is too low, the composite material will solidify, and if the temperature is too high, the material will decompose. The length of the blend particles is less than 8 mm (such as 7.5 mm, 7 mm, 6.5 mm, 6 mm, 5.5 mm, 5 mm, 4.5 mm, 4 mm, 3.5 mm, 3 mm, 2.5 mm, 2 mm, 1.5 mm, 1 mm).

[0091] As an optional embodiment of the preparation method of the poly(phenylene phthalate) resin-based composite material pipe product of the present invention, in the preparation method of the pipe, the extrusion molding temperature is 340-400°C (such as 345°C, 350°C, 355°C, 360°C, 365°C, 370°C, 375°C, 380°C, 385°C, 390°C, 395°C), and the melt pressure is 10-40MPa (such as 12MPa, 15MPa, 17MPa, 20MPa). , 22MPa, 25MPa, 27MPa, 30MPa, 32MPa, 35MPa, 37MPa, 39MPa), and the screw speed is 1-20rpm (such as 2rpm, 3rpm, 4rpm, 5rpm, 6rpm, 7rpm, 8rpm, 9rpm, 10rpm, 11rpm, 12rpm, 13rpm, 14rpm, 15rpm, 16rpm, 17rpm, 18rpm, 19rpm).

[0092] As an optional embodiment of the preparation method of the poly(phenylene phthalate) resin-based composite material pipe product of the present invention, in the preparation method of the connecting component, the injection molding temperature is 340-400°C (such as 345°C, 350°C, 355°C, 360°C, 365°C, 370°C, 375°C, 380°C, 385°C, 390°C, 395°C), and the injection pressure is 30-130MPa (such as 35MPa, 40MPa, 45MPa, 50MPa, 55MPa, 60MPa, 65MPa, 70MPa, 75MPa, 80MPa, 85MPa, 90MPa, 95MPa, 100MPa, 105MPa, 110MPa). The temperature of the connecting component molding mold is 80-200℃ (such as 85℃, 90℃, 95℃, 100℃, 105℃, 110℃, 115℃, 120℃, 125℃, 130℃, 135℃, 140℃, 145℃, 150℃, 155℃, 160℃, 165℃, 170℃, 175℃, 180℃, 185℃, 190℃, 195℃), and the cooling time is 10-90s (such as 11s, 15s, 20s, 25s, 30s, 35s, 40s, 45s, 50s, 55s, 60s, 65s, 70s, 75s, 80s, 85s, 89s).

[0093] During the molding process of the above-mentioned pipes and / or connecting parts, each interval is the only processing window, and molding cannot be performed above or below each processing interval. In particular, the molding process requires overall dynamic regulation. If the raw materials cannot be melted well due to insufficient heating of the heating element, the melt pressure will increase, and the screw speed must be reduced accordingly. Therefore, when related preparation equipment such as single-screw extruders and twin-screw extruders are used, dynamic regulation is required, but the regulation range should not exceed the above-mentioned interval range.

[0094] In the present invention, no special requirements are made on the equipment used in the preparation process, and any equipment in the prior art that can achieve the relevant purpose can be used. For example, drying requires 120-180°C, which can be carried out in a heating device that can reach this temperature, such as an existing hot blast oven, etc.; premixing requires that raw materials of different forms be well dispersed, which can be carried out in a mixer that can disperse well, such as an existing high-speed mixer, etc.; melt blending requires that raw materials of various forms can be prepared into uniform, well-dispersed granular composite materials, which can be carried out in equipment that can melt blend and granulate, such as an existing twin-screw extruder, granulator, etc.; extrusion molding requires that the blend particles can be heated to a higher processing temperature (340-400°C) and extruded into pipes, which can be carried out in equipment that can heat at high temperature and extrude into pipes, such as a single-screw extruder generally used for polymer pipe molding at this stage, etc.; injection molding requires that the blend particles can be heated and pressurized to certain parameters, which can be carried out in injection molding equipment that meets the conditions, such as an existing plastic injection molding machine, etc.; and so on.

[0095] According to the high viscosity, high processing temperature and multi-morphology of the raw materials, the inventors found that the specific molding of pipes and connecting parts of polyphenylene ether resin-based composite materials can be achieved through the following preparation method, and the molded pipes and connecting parts have light weight and high strength, a service temperature greater than 200°C, excellent high-temperature mechanical properties, corrosion resistance and other properties, giving full play to the advantages of polyphenylene ether high-performance engineering resins and their composite materials, and can replace metal pipes in various complex environments, and can solve the problems of short service life, heavy weight, severe corrosion and high processing and molding costs of metal pipes and their connecting parts in complex environments. The specific preparation is as follows:

[0096] The resin matrix, fluidity improving agent, reinforcement and functional filler are dried in a hot air oven at 120-180°C (such as 125°C, 130°C, 135°C, 140°C, 145°C, 150°C, 155°C, 160°C, 165°C, 170°C, 175°C), and then placed in a high-speed mixer for premixing according to a certain proportion to obtain a premixed material; the premixed material is extruded using a twin-screw extruder at 330-400°C (such as 335°C, 340°C, 345°C, 350°C, 355°C, 360°C, 365°C, 370°C, 375°C, 380°C, 385°C, 390°C, 395°C) The blending is carried out, and the screw speed is controlled to be 60-150rpm (such as 65rpm, 70rpm, 75rpm, 80rpm, 85rpm, 90rpm, 95rpm, 100rpm, 105rpm, 110rpm, 115rpm, 120rpm, 125rpm, 130rpm, 135rpm, 140rpm, 145rpm) to obtain polymer filaments with uniform diameter and smooth appearance; the polymer filaments are cooled and cut by a granulator to obtain blend particles (composite particles) with a length of less than 8mm (such as 2mm, 3mm, 4mm, 5mm, 6mm, 7mm, 8mm).

[0097] In the above raw material compounding process, the premixing process is mainly carried out according to the parameters of the high-speed mixer, and the specific parameters are not limited, as long as the premixing is uniform. During the blending process, the temperature and screw speed within the process parameter range are dynamically coordinated and controlled, so that the material has a good molding effect.

[0098] The forming method of the pipe of the poly(phenylene ether) resin-based composite material is as follows:

[0099] After the blend particles are dried in a hot blast oven at 120-180°C, a single screw extruder and a tube forming die are used to form the tube. The processing conditions are 340-400°C (such as 345°C, 350°C, 355°C, 360°C, 365°C, 370°C, 375°C, 380°C, 385°C, 390°C, 395°C), and the melt pressure is 10-40MPa (such as 12MPa, 15MPa, 17MPa, 20MPa, 22MPa, 25MPa, 27MPa, 30MPa, 32MPa, 35MPa, 37 MPa, 39MPa), the screw speed is 1-20rpm (such as 2rpm, 3rpm, 4rpm, 5rpm, 6rpm, 7rpm, 8rpm, 9rpm, 10rpm, 11rpm, 12rpm, 13rpm, 14rpm, 15rpm, 16rpm, 17rpm, 18rpm, 19rpm), and each parameter is adjusted to ensure that the pipe is continuously and stably formed, the pipe diameter is uniform and the appearance is shiny; after sizing and cooling, it is towed by a traction machine and cutter segmented into dimensionally stable poly(phenylene ether) resin-based composite pipe.

[0100] In the above-mentioned pipe forming process, the pipe diameter is determined by the pipe forming die. The pipe forming die is connected to the front end of the single screw extruder and is a device specially used for composite pipe forming. In a broad sense, it is a component of the single screw extruder and can be selected according to pipe requirements such as pipe diameter. In the present invention, the pipe forming die can be an existing conventional one or a customized one.

[0101] The method for forming the connection parts of the poly(phenylene ether) resin-based composite material is as follows:

[0102] The blend particles are dried in a hot air oven at 120-180°C (such as 125°C, 130°C, 135°C, 140°C, 145°C, 150°C, 155°C, 160°C, 165°C, 170°C, 175°C), and then molded using a plastic injection molding machine and a connecting component molding mold (hereinafter referred to as the mold). The injection molding process conditions are 340-400°C (such as 345°C, 350°C, 355°C). , 360℃, 365℃, 370℃, 375℃, 380℃, 385℃, 390℃, 395℃), the injection pressure is 30-130MPa (such as 35MPa, 40MPa, 45MPa, 50MPa, 55MPa, 60MPa, 65MPa, 70MPa, 75MPa, 80MPa, 85MPa, 90MPa, 95MPa, 100 MPa, 105MPa, 110MPa, 115MPa, 120MPa, 125MPa), the connection component molding mold temperature is 80-200℃ (such as 85℃, 90℃, 95℃, 100℃, 105℃, 110℃, 115℃, 120℃, 125℃, 130℃, 135℃, 140℃, 145℃, 150℃, 155℃, 160℃, 16 The cooling time is 10-90s (such as 11s, 15s, 20s, 25s, 30s, 35s, 40s, 45s, 50s, 55s, 60s, 65s, 70s, 75s, 80s, 85s, 89s) to obtain the poly(phenylene ether) resin-based composite material pipe connecting parts.

[0103] In the above-mentioned specific preparation, the inventors found through a large number of experiments that the raw materials of the composite material include powders (resin matrix, functional fillers), granules (fluidity improving additives), filamentary fibers and other forms, which can have good dispersion after premixing by a high-speed mixer. The use of a twin-screw extruder for processing can prepare the multi-form raw materials into a uniform, well-dispersed granular composite material, which lays the foundation for the next step of processing; regulating the extrusion molding process parameters of the pipe and the injection molding process parameters of the connecting parts to determine the processing window of the composite material can ensure accurate and stable molding.

[0104] In particular, the composite material of the present invention has certain particularities. The processing parameters given in the present invention cover the total temperature range of each heating section of the twin-screw extruder and the single-screw extruder. In the process involving melt processing (blending and pipe and / or connecting component molding), the control of process parameters such as screw speed, heating temperature of each section, and pulling speed are all dynamically adjusted according to the plasticization and cooling process of the composite material melt during the processing.

[0105] The present invention will be further described in detail below with reference to specific embodiments and comparative examples.

[0106] Embodiment 1:

[0107] A pipe product of a polyarylether resin-based composite material, comprising a pipe and a connecting component for the pipe, wherein the pipe and the connecting component are both made of the polyarylether resin-based composite material, and the raw materials of the polyarylether resin-based composite material include the following components by weight:

[0108] Poly(arylene ether) phthalate resin matrix: 100 parts, of which 80 parts are PPESK and 20 parts are PPBESK;

[0109] Flowability improving agent: 20 parts of polyetheretherketone with a melt index of 20-25g / 10 minutes;

[0110] Reinforcement: 30 parts of 1mm chopped carbon fiber;

[0111] Functional filler: 5 parts of nano-grade graphite powder;

[0112] The number average molecular weight of PPESK is 27000, and its general structural formula is:

[0113]

[0114] The number average molecular weight of PPBESK is 20,000, and its general structural formula is:

[0115]

[0116] The preparation method of the pipe and the connecting parts for the pipe is as follows:

[0117] After the raw materials were dried in a hot air oven at 150°C for 6 hours, 100 parts of PPESK and PPBESK resins (PPESK accounted for 80% of the total mass ratio of the two), 20 parts of polyetheretherketone, 30 parts of 1mm short-cut carbon fibers, and 5 parts of nano-graphite powder were placed in a high-speed mixer and stirred at a high speed of 1000rpm for 5 minutes to obtain a premixed material; the premixed material was placed in the feeding port of a twin-screw extruder, and the screw speed was controlled at 330°C-370°C at 60rpm-120rpm to obtain a polymer filament with uniform diameter and smooth surface, which was then cut into composite material particles with a length of 5mm by a granulator after cooling.

[0118] Take some of the composite material particles that have been secondary dried in a hot air oven at 150°C for 6 hours and put them into the feeding port of a single-screw extruder for pipe preparation. The pipe forming conditions using a single-screw extruder (equipped with a conventional pipe forming head) are as follows: the forming temperature is 340°C-400°C, the melt pressure is 10MPa-40MPa, and the screw speed is 1rpm-10rpm. Adjust each parameter until the pipe is continuously and stably formed, and the pipe diameter is uniform and the appearance is glossy.

[0119] The pipe connection parts are made of composite material particles that have been secondary dried in a hot air oven at 150°C for 6 hours and then injected into a plastic injection molding machine. The injection molding process conditions are 340°C-400°C, injection pressure 30MPa-130MPa, connection part molding mold temperature 120°C-150°C, and cooling time 30s. Finally, a complex-shaped precision poly(phenylene ether) resin-based composite pipe connection part is obtained, and its structure is as follows: Figure 1 As shown, it can be seen that the pipe connection component has a complex thread structure inside and a concave structure outside.

[0120] Embodiment 2:

[0121] A pipe product of a polyarylether resin-based composite material, comprising a pipe and a connecting component for the pipe, wherein the pipe and the connecting component are both made of the polyarylether resin-based composite material, and the raw materials of the polyarylether resin-based composite material include the following components by weight:

[0122] Poly(arylene ether) phthalate resin matrix: 100 parts, including PPESK, PPES and PPBESK resins, and the mass ratio of the three resins is 1:1:1;

[0123] Flowability improving agent: 20 parts of polyethersulfone with a melt index of 40 g / 10 minutes;

[0124] Reinforcement: 20 parts of 5mm chopped carbon fiber;

[0125] Functional filler: 5 parts of nano calcium carbonate, 5 parts of nano silicon nitride;

[0126] The number average molecular weight of PPESK is 25,000, and its general structural formula is:

[0127]

[0128] The number average molecular weight of PPES is 25,000, and its general structural formula is:

[0129]

[0130] The number average molecular weight of PPBESK is 20,000, and its general structural formula is:

[0131]

[0132] The preparation method of the pipe and the connecting parts for the pipe is as follows:

[0133] The raw materials were dried in a hot air oven at 120°C for 8 hours, and then 100 parts of PPESK, PPES and PPBESK resins (the mass ratio of the three resins was 1:1:1), 20 parts of polyethersulfone, 20 parts of 5mm short-cut carbon fibers, 5 parts of nano-calcium carbonate and 5 parts of nano-silicon nitride were placed in a high-speed mixer and stirred at a high speed of 1000 rpm for 5 minutes to obtain a premixed material; the premixed material was placed in a feeding port of a twin-screw extruder, and the screw speed was controlled at 340°C-380°C at 60rpm-100rpm to obtain a polymer filament with uniform diameter and smooth surface, which was then cut into composite material particles with a length of 5mm by a granulator after cooling.

[0134] Take some of the composite material particles that have been secondary dried in a hot air oven at 120°C for 8 hours and put them into the feeding port of a single-screw extruder for pipe preparation. The pipe is formed using a single-screw extruder (equipped with a conventional pipe forming head) under the following conditions: forming temperature of 340°C-400°C, melt pressure of 10MPa-40MPa, screw speed of 1rpm-8rpm, and each parameter is adjusted until the pipe is continuously and stably formed, and the pipe diameter is uniform and has a glossy appearance.

[0135] The pipe connection parts are made of composite material particles that have been secondary dried in a hot air oven at 120°C for 8 hours and then injected into a plastic injection molding machine. The injection molding process conditions are 340°C-360°C, injection pressure 30MPa-110MPa, connection part molding mold temperature 120°C-140°C, and cooling time 30s. Finally, a complex-shaped precision poly(phenylene ether) resin-based composite material connection part is obtained, and its structure is as follows: Figure 1 As shown, it can be seen that the pipe connection component has a complex thread structure inside and a concave structure outside.

[0136] Embodiment 3:

[0137] A pipe product of a polyarylether resin-based composite material, comprising a pipe and a connecting component for the pipe, wherein the pipe and the connecting component are both made of the polyarylether resin-based composite material, and the raw materials of the polyarylether resin-based composite material include the following components by weight:

[0138] Phthalate polyarylether resin matrix: PPENSK 100 parts;

[0139] Flowability improving agent: 10 parts of polyamide with a melt index of 50 g / 10 minutes;

[0140] Reinforcement: 15 parts of 3mm basalt fiber, 5 parts of 3mm glass fiber;

[0141] Functional filler: 0 parts;

[0142] The number average molecular weight of PPENSK is 23000, and its general structural formula is:

[0143]

[0144] The preparation method of the pipe and the connecting parts for the pipe is as follows:

[0145] The raw materials were dried in a hot air oven at 150°C for 6 hours, and then 100 parts of PPENSK, 10 parts of polyamide, 15 parts of 3mm basalt fiber, and 5 parts of 3mm glass fiber were placed in a high-speed mixer and stirred at 1000 rpm for 5 minutes to obtain a premixed material. The obtained premixed material was put into the feed port of a twin-screw extruder, and the screw speed was controlled at 330°C-360°C at 60rpm-100rpm to obtain polymer filaments with uniform diameter and smooth appearance. After cooling, the filaments were cut into composite material particles with a length of 5mm using a granulator.

[0146] Take some of the composite material particles that have been secondary dried in a hot air oven at 150°C for 6 hours and put them into the feeding port of a single-screw extruder for pipe preparation. The pipe is formed using a single-screw extruder (equipped with a conventional pipe forming head) under the following conditions: forming temperature of 340°C-370°C, melt pressure of 10MPa-40MPa, screw speed of 1rpm-10rpm, and each parameter is adjusted until the pipe is continuously and stably formed, and the pipe diameter is uniform and has a glossy appearance.

[0147] The pipe connection parts are made of composite material particles that have been secondary dried in a hot air oven at 150°C for 6 hours and then injected into a plastic injection molding machine. The injection molding process conditions are 340°C-365°C, injection pressure 30MPa-100MPa, connection part molding mold temperature 110°C-160°C, and cooling time 20s. Finally, a complex-shaped precision poly(phenylene ether) resin-based composite material connection part is obtained, and its structure is as follows: Figure 1 As shown, it can be seen that the pipe connection component has a complex thread structure inside and a concave structure outside.

[0148] Embodiment 4:

[0149] A pipe product of a polyarylether resin-based composite material, comprising a pipe and a connecting component for the pipe, wherein the pipe and the connecting component are both made of the polyarylether resin-based composite material, and the raw materials of the polyarylether resin-based composite material include the following components by weight:

[0150] Poly(arylene ether) phthalate resin matrix: 100 parts, of which 50 parts are PPEKK and 50 parts are PPBESK;

[0151] Flowability improving agent: 30 parts of polyetherketoneketone with a melt index of 20g / 10min;

[0152] Reinforcement: 30 parts of 3mm chopped carbon fiber;

[0153] Functional filler: 5 parts of nano-grade graphite powder;

[0154] The number average molecular weight of PPEKK is 25000, and its general structural formula is:

[0155]

[0156] The number average molecular weight of PPBESK is 20,000, and its general structural formula is:

[0157]

[0158] The preparation method of the pipe and the connecting parts for the pipe is as follows:

[0159] The raw materials were dried in a hot air oven at 150°C for 6 hours, and then 100 parts of PPEKK and PPBESK resins (PPESKK accounted for 50% of the total mass ratio of the two), 30 parts of polyetherketoneketone, 30 parts of 3mm short-cut carbon fibers, and 5 parts of nano-graphite powder were placed in a high-speed mixer and stirred at 1000 rpm for 5 minutes to obtain a premixed material; the obtained premixed material was put into the feeding port of a twin-screw extruder, and the screw speed was controlled at 330°C-360°C at 60rpm-150rpm to obtain polymer filaments with uniform diameter and smooth appearance, which were then cut into composite material particles with a length of 5mm by a granulator after cooling.

[0160] Take some of the composite material particles that have been secondary dried in a hot air oven at 150°C for 6 hours and put them into the feeding port of a single-screw extruder for pipe preparation. The pipe is formed using a single-screw extruder (equipped with a conventional pipe forming head) under the following conditions: forming temperature of 340°C-390°C, melt pressure of 10MPa-30MPa, screw speed of 3rpm-10rpm, and each parameter is adjusted until the pipe is continuously and stably formed, the pipe diameter is uniform and the appearance is glossy.

[0161] The pipe connection parts are made of composite material particles that have been secondary dried in a hot air oven at 150°C for 6 hours and then injected into a plastic injection molding machine. The injection molding process conditions are 340°C-390°C, injection pressure 30MPa-120MPa, connection part molding mold temperature 120°C-140°C, and cooling time 50s. Finally, a complex-shaped precision poly(phenylene ether) resin-based composite material connection part is obtained, and its structure is as follows: Figure 1 As shown, it can be seen that the pipe connection component has a complex thread structure inside and a concave structure outside.

[0162] Performance Testing and Results

[0163] The axial tensile strength test of the pipe is carried out with reference to the national standard GB / T 1040.1 plastic tensile performance test.

[0164] The pipe pressure test method is: according to the size of the inner diameter of the pipe, use a self-locking pipe pressure bursting fixture to seal both ends, control the internal pressure of the pipe through the hydraulic cylinder, record the pressure value (burst pressure) when the pipe is damaged, and calculate the annular bursting stress of the pipe through the pipe wall thickness. The reference formula is as follows:

[0165]

[0166] Where:

[0167] σ θ ——Annular bursting stress (MPa);

[0168] p——burst pressure (MPa);

[0169] D0——outer diameter of the pipe, mm;

[0170] δ——minimum wall thickness, mm; since the tube walls of the tubes in the above embodiments are uniform, it is also the average wall thickness, i.e. the tube wall thickness.

[0171] The test results of the pipe performance prepared in the embodiment are shown in Table 1:

[0172] Table 1

[0173]

[0174] Through the test of the embodiment, it can be seen that the pipe of the present invention is prepared according to the raw material ratio, and the tensile strength of the obtained pipe is in the range of 90MPa-180MPa, and the circumferential bursting stress is in the range of 40MPa-90MPa. In addition, the density is less than 1.6g / cm 3 It can replace metal pipes and be used in various complex environments. It has good application prospects in various industries.

[0175] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A pipe product of a poly(phenylene ether) resin-based composite material, characterized in that: The pipe products are pipes and / or connecting parts for pipes, and the pipes and connecting parts are both made of the polyarylether phthalate resin-based composite material. The raw materials of the polyarylether phthalate resin-based composite material include the following components in parts by weight: Phthalate polyarylether resin matrix: 100 parts; Flowability improving agent: 10-30 parts; Reinforcement: 15-30 parts; Functional filler: 0-10 parts; The poly(arylene ether) phthalazine resin matrix comprises at least one of the following resins: PPESK, PPES, PPEK, PPENS, PPENK, PPEKK and PPENSK, and PPBESK, PPBES, PPBEK and PPBESKK containing biphenyl structures; The general structural formula of the PPESK, PPES, PPEK, PPENS, PPENK, PPENSK, PPBESK, PPBES, PPBEK, PPEKK and PPBESKK is: Wherein, when the resin structure does not contain a biphenyl structure, Ar is: When the resin structure contains a biphenyl structure, Ar is and The sum of the two proportions is 100%; R1, R2, R3 and R4 are each independently selected from hydrogen, a halogen substituent, a phenyl group, a phenoxy group, an alkyl group or an alkoxy group, the alkyl group or the alkoxy group contains at least one carbon atom, and the structures of R1, R2, R3 and R4 are the same or different; Where: PPESK: a≥3, b≥3, c=0, d=0; PPES: a≥3, b=0, c=0, d=0; PPEK: a=0, b≥3, c=0, d=0; PPENS: a≥3, b=0, c=0, d≥3; PPENK: a=0, b≥3, c=0, d≥3; PPENSK: a≥3, b≥3, c=0, d≥3; PPBESK: a≥3, b≥3, c=0, d=0; PPBES: a≥3, b=0, c=0, d=0; PPBEK: a=0, b≥3, c=0, d=0; PPEKK: a=0, b=0, c≥3, d=0; PPBESKK: a≥3, b=0, c≥3, d=0.

2. The tube product of the poly(phenylene ether) resin-based composite material according to claim 1, characterized in that: The fluidity improving agent comprises at least one of polyamide, polysulfone, polyethersulfone, polyetheretherketone, polyetherketoneketone, polyetherimide and polyphenylene sulfide; And / or, the reinforcement comprises fibers having a length between 2 μm and 5 mm, wherein the fibers comprise at least one of carbon fibers, glass fibers, basalt fibers, and quartz fibers; And / or, the functional filler includes at least one of graphite powder, nano-silicon dioxide, nano-silicon carbide, nano-silicon nitride, nano-calcium carbonate, nano-metal powder, and porous carbon.

3. The tube product of the poly(phenylene ether) resin-based composite material according to claim 1, characterized in that: The number average molecular weight of the poly(arylene ether) phthalazine resin matrix is ​​10,000-40,000 g / mol; and / or the melt index of the fluidity improving agent is 20-70 g / 10 minutes.

4. The tube product of the poly(phenylene ether) resin-based composite material according to claim 1, characterized in that: The preparation method of the pipe comprises: drying, premixing, melt blending and granulating the raw materials in sequence to obtain blend particles; drying and extruding the blend particles to obtain the pipe; And / or, the axial tensile strength of the pipe is 90-180 MPa, the circumferential bursting stress is 40-90 MPa, and the density is less than 1.6 g / cm 3 .

5. The tube product of the poly(phenylene ether) resin-based composite material according to claim 1, characterized in that: The preparation method of the connecting component comprises: drying, premixing, melt blending and granulating the raw materials in sequence to obtain blend particles; drying and injection molding the blend particles to obtain the connecting component; And / or, the density of the connecting component is lower than 1.6 g / cm 3 .

6. The tube product of the poly(phthalazine biphenyl) ether resin-based composite material according to claim 4 or 5, characterized in that: In the method for preparing the pipe and / or the connecting component, the drying temperature is 120-180° C.; and / or the melt blending temperature is 330-400° C.; and / or the length of the blend particles is less than 8 mm.

7. The tube product of the poly(phthalazine biphenyl) ether resin-based composite material according to claim 4 or 5, characterized in that: In the method for preparing the pipe, the extrusion molding temperature is 340-400°C, the melt pressure is 10-40MPa, and the screw speed is 1-20rpm; And / or, in the preparation method of the connecting component, the injection molding temperature is 340-400° C., the injection pressure is 30-130 MPa, the connecting component molding mold temperature is 80-200° C., and the cooling time is 10-90 s.

8. A method for preparing a tube product of the poly(phenylene ether) resin-based composite material according to any one of claims 1 to 7, characterized in that: The raw materials are sequentially dried, premixed, melt-blended, and granulated to obtain blend particles; The method for preparing the pipe comprises: drying and extruding the blend particles to obtain the pipe; The preparation method of the connecting component comprises: drying and injection molding the blend particles to obtain the connecting component.

9. The preparation method according to claim 8, characterized in that: In the method for preparing the pipe and / or the connecting component, the drying temperature is 120-180° C.; and / or the melt blending temperature is 330-400° C.; and / or the length of the blend particles is less than 8 mm.

10. The preparation method according to claim 8, characterized in that: In the method for preparing the pipe, the extrusion molding temperature is 340-400°C, the melt pressure is 10-40MPa, and the screw speed is 1-20rpm; And / or, in the preparation method of the connecting component, the injection molding temperature is 340-400° C., the injection pressure is 30-130 MPa, the connecting component molding mold temperature is 80-200° C., and the cooling time is 10-90 s.

Citation Information

Cited By

  • Automobile nylon tube and preparation method thereof

    CN121086519A