Scratch-resistant and stain-resistant coating for bathroom door plate and surface treatment process of scratch-resistant and stain-resistant coating
By using modified fillers and polytetrafluoroethylene emulsion on the bathroom door panel, the scratch resistance and toxicity problems of traditional paints are solved, and scratch resistance and wear resistance and antibacterial effects are achieved, which improves the durability of the door panel and Health and safety.
Patent Information
- Application Number
- CN202411395183.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-08
- Publication Date
- 2024-12-03
AI Technical Summary
Traditional bathroom door panel coatings are insufficient in scratch resistance and durability during long-term use and high-strength friction, and some paints have toxic risks, affecting the health and safety of users.
Using a scratch-resistant and stain-resistant coating formulation, including aqueous resins, modified fillers, polydimethylsiloxanes, silane coupling agents, palm waxes and antioxidants, silica and mussel shell powder are refined by ball milling. , combined with polytetrafluoroethylene emulsion and carboxymethyl chitosan, form a durable coating, enhancing the scratch resistance and antibacterial ability of the coating.
Significantly improves the hardness and wear resistance of the coating, enhances scratch resistance and antibacterial ability, reduces bacterial adhesion and reproduction, improves the self-cleaning ability of the door panel, extends the service life of the coating, and reduces the risk of toxicity .
Smart Images

Figure BDA0005073570110000051 
Figure BDA0005073570110000061
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of surface treatment, and relates to a scratch-resistant and stain-resistant coating for a bathroom door panel and a surface treatment process thereof. Background Art
[0002] Bathrooms are frequently used spaces in daily life, and their door panels are often subject to corrosion from water vapor, detergents and other chemicals, as well as physical wear caused by frequent opening and closing. Although traditional bathroom door panel materials meet basic decoration and usage requirements to a certain extent, they are obviously insufficient in terms of scratch resistance, anti-fouling self-cleaning and long-term stability. Therefore, it is particularly important to develop a bathroom door panel coating and its surface treatment process with excellent scratch resistance and stain resistance.
[0003] At present, there are many waterproof and antifouling coatings on the market for bathroom door panels, but the scratch resistance and durability of most products are greatly reduced when facing long-term use and high-intensity friction. In addition, some coatings have toxic risks due to chemical composition problems, affecting the health and safety of users. Therefore, it is necessary to develop a new type of bathroom door panel coating that is environmentally friendly, efficient, scratch-resistant and stain-resistant and its supporting surface treatment process. Summary of the invention
[0004] The purpose of the present invention is to provide a scratch-resistant and stain-resistant paint for bathroom door panels and a surface treatment process thereof, which has the characteristics of scratch-resistant, wear-resistant, stain-resistant and antibacterial.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] A scratch-resistant and stain-resistant coating for bathroom door panels, wherein the formula of the scratch-resistant and stain-resistant coating is as follows: by weight, 80 to 90 parts of water-based resin, 20 to 30 parts of modified filler, 5 to 8 parts of polydimethylsiloxane, 3 to 5 parts of silane coupling agent, 2 to 5 parts of thickener, 1 to 3 parts of palm wax, 0.5 to 1 part of antioxidant, and 65 to 75 parts of deionized water.
[0007] Wherein, the preparation method of the modified filler is as follows:
[0008] S1-1: 40 to 50 parts by weight of filler are placed in a ball mill for ball milling at a speed of 400 r / min for 45 to 60 min, and passed through a 200-mesh sieve to obtain a mixture A;
[0009] S1-2: Mix the mixture A with 40-50 parts by weight of deionized water, stir at 550-650 r / min for 30 min, add 1-2 parts by weight of an anti-settling agent, adjust the pH to 8-9 with a 2M sodium bicarbonate solution, and stir ultrasonically for 30 min to obtain a mixed solution B;
[0010] S1-3: 3 to 5 parts by weight of polytetrafluoroethylene emulsion is added to the mixed solution B, ultrasonicated at 50° C. for 30 minutes, 1 to 3 parts by weight of carboxymethyl chitosan solution is added, and then dispersed in a high-speed disperser for 1 hour to obtain the modified filler.
[0011] Furthermore, the filler in the S1-1 is a mixture of silicon dioxide and mussel shell powder in a mass ratio of 2:1.
[0012] Furthermore, the anti-settling agent in S1-2 is a polyamide wax anti-settling agent, wherein the mass fraction of the polyamide wax is 50%.
[0013] Furthermore, the silane coupling agent is one of KH550, KH560 and KH570.
[0014] Furthermore, the water-based resin is one or both of water-based polyurethane resin and water-based acrylic resin.
[0015] Furthermore, the thickener is one of carboxymethyl cellulose, hydroxyethyl cellulose and hydroxypropyl methyl cellulose.
[0016] Furthermore, the antioxidant is one of antioxidant 1010 and antioxidant 1076.
[0017] A method for preparing a scratch-resistant and stain-resistant coating for a bathroom door panel comprises the following preparation steps:
[0018] S8-1: Mix the modified filler and the water-based resin according to the formula, and stir at a speed of 500-600 r / min for 30 min to obtain a mixture C;
[0019] S8-2: polydimethylsiloxane, silane coupling agent, palm wax and antioxidant are added to mixture C in sequence, and stirred at a speed of 850-950 r / min for 30 min to obtain mixture D;
[0020] S8-3: Deionized water and a thickener are sequentially added to the mixture D, and stirred at a speed of 650 to 750 r / min for 10 min to obtain the scratch-resistant and stain-resistant coating.
[0021] A scratch-resistant and stain-resistant surface treatment process for bathroom door panels includes the following process flows:
[0022] S9-1: The surface of the bathroom door panel was cleaned with 75% ethanol by mass, then washed three times with deionized water, dried at room temperature for 12 hours, and polished with 300-400 mesh water-abrasive sandpaper to remove minor defects and increase surface roughness, thereby obtaining a door panel to be treated;
[0023] S9-2: Mix the anti-scratch and stain-resistant coating with deionized water to a viscosity of 55-60KU, use an air compression spray gun to evenly spray the anti-scratch and stain-resistant coating on the surface of the door panel to be treated, place it in an 80°C oven for pre-curing for 10-20 minutes, then place it in a UV curing machine for curing for 1-2 minutes, and finally polish it to obtain a scratch-resistant and stain-resistant surface.
[0024] Furthermore, the energy of the UV curing machine is 1100-1200 MJ / cm 2 , the distance of UV light source is 0.5m.
[0025] Silica and mussel shell powder are selected as fillers. Silica has excellent hardness and wear resistance, which can significantly improve the hardness and wear resistance of the coating, making the coating more durable and not easy to be scratched or worn; the porous structure and good adhesion of mussel shell powder help to form a strong coating. Its main component calcium carbonate also has high hardness and wear resistance. Combined with silica, it can enhance the scratch resistance of the coating. In addition, the natural texture and lustrous color of mussel shell powder can add beauty to bathroom door panels; mussel shell powder and silica are refined and mixed evenly by ball milling. The collision and friction between particles during the ball milling process gradually break large particles into small particles, while increasing the contact area between particles, which is conducive to subsequent processing. The refined filler can be more evenly distributed in the coating, improving the density and hardness of the coating, thereby enhancing its scratch resistance.
[0026] Polytetrafluoroethylene emulsion is a polymer emulsion, which contains a large number of fluorine atoms in its molecules, making polytetrafluoroethylene have extremely low surface energy and excellent lubricity. The low surface energy of polytetrafluoroethylene makes it difficult for liquids such as water, oil, and stains to form a stable wetting layer on the coating surface, thereby reducing the contact area and adhesion between the liquid and the coating surface; in addition, polytetrafluoroethylene has excellent stability to a variety of chemical substances and can resist corrosion by corrosive substances such as acids, alkalis, and salts, thereby protecting the coating from chemical pollution. At the same time, its excellent lubricity also helps to reduce friction and wear on the coating surface, thereby enhancing the coating's anti-scratch performance; in addition, polytetrafluoroethylene can also form a good bonding interface with the resin matrix, improving the overall strength and durability of the coating.
[0027] Carboxymethyl chitosan is a natural polymer material with good film-forming properties and biocompatibility. The carboxyl and amino groups on its molecular chain can interact with fillers and polytetrafluoroethylene, which not only promotes the uniform dispersion of fillers and reduces particle agglomeration, but also significantly enhances the interfacial bonding force between fillers and substrates, further improving the scratch resistance and stain resistance of the coating. In addition, carboxymethyl chitosan has a broad-spectrum antibacterial ability. Through the interaction of its molecular chain with bacterial cell walls or membrane structures, it interferes with the normal physiological functions of bacteria, thereby inhibiting or even killing a variety of bacteria. Therefore, the addition of an appropriate amount of carboxymethyl chitosan can effectively reduce the adhesion and reproduction of bacteria on the coating surface, improve the self-cleaning ability of door panels, and create a more hygienic and healthy bathroom environment.
[0028] Polydimethylsiloxane has a low surface tension, which can reduce the viscosity of the paint, improve its fluidity and smoothness of construction, making it easier to evenly distribute the paint on the surface of the bathroom door panel; after the paint dries, polydimethylsiloxane can form a flexible protective layer on the coating surface, enhancing the wear and scratch resistance of the coating. Silane coupling agents can form stable chemical bonds with the surface materials of bathroom door panels, improve the adhesion between the paint and the door panels, and prevent the coating from falling off; at the same time, they can also improve the interfacial bonding between the filler and the resin matrix, and improve the overall performance of the coating. Antioxidants can capture free radicals in the paint, interrupt the free radical chain reaction, prevent the coating from being degraded due to oxidation during storage and use, and extend the service life of the coating.
[0029] The introduction of palm wax can form a protective layer in the coating, effectively preventing water penetration and improving the water resistance of the coating; improving the anti-emulsification properties of the coating, preventing water from emulsifying in the coating, and maintaining the stability and quality of the coating; reducing the friction coefficient of the coating surface, making the coating smoother, reducing the occurrence of scratches, and improving the convenience of cleaning; in addition, palm wax has a high hardness, which can enhance the wear resistance of the coating, making the door panel less likely to be damaged during long-term use, and its smooth surface is also stain-resistant, which can prevent stains from adhering and keep the door panel clean.
[0030] Beneficial effects of the present invention:
[0031] (1) By using silica and mussel shell powder as fillers and refining and mixing them by ball milling, the hardness and wear resistance of the coating were significantly improved. The introduction of polytetrafluoroethylene emulsion, with its extremely low surface energy and excellent lubricity, improved the stain resistance of the coating. At the same time, the stability of polytetrafluoroethylene to a variety of chemicals also protected the coating from corrosion by corrosive substances. The addition of carboxymethyl chitosan not only promoted the uniform dispersion of the filler and enhanced the scratch resistance and stain resistance of the coating, but also effectively reduced the adhesion and reproduction of bacteria on the coating surface through its broad-spectrum antibacterial ability, thereby improving the self-cleaning ability of the door panel.
[0032] (2) The modified filler, water-based resin, polydimethylsiloxane, palm wax and silane coupling agent are used together to prepare a scratch-resistant and wear-resistant coating, which further improves the construction performance of the coating and the adhesion between the coating and the door panel, and further enhances the scratch-resistant and wear-resistant properties of the coating. The addition of palm wax further improves the water resistance and stability of the coating, and the addition of antioxidants further extends the service life of the coating. DETAILED DESCRIPTION
[0033] In order to further illustrate the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods, structures, features and effects of the present invention are described in detail below in combination with the embodiments.
[0034]
[0035]
[0036] Example 1
[0037] The formula 1 of the scratch-resistant and stain-resistant coating is as follows: by weight, 85 parts of waterborne polyurethane resin, 30 parts of modified filler, 6 parts of polydimethylsiloxane, 4 parts of silane coupling agent KH550, 3 parts of carboxymethyl cellulose, 2 parts of palm wax, 10101 parts of antioxidant, 70 parts of deionized water,
[0038] Wherein, the preparation method of the modified filler is as follows:
[0039] S1-1: 30 parts by weight of silicon dioxide and 15 parts by weight of mussel shell powder were placed in a ball mill for ball milling at a ball milling speed of 400 r / min for 45 min, and passed through a 200-mesh sieve to obtain a mixture A;
[0040] S1-2: Mix the mixture A with 40 parts by weight of deionized water, stir at a speed of 550 r / min for 30 min, add 1 part by weight of a polyamide wax anti-settling agent, wherein the mass fraction of the polyamide wax in the anti-settling agent is 50%, adjust the pH to 8 with a 2M sodium bicarbonate solution, and stir ultrasonically for 30 min to obtain a mixed solution B;
[0041] S1-3: 4 parts by weight of polytetrafluoroethylene emulsion is added to the mixed solution B, ultrasonicated at 50°C for 30 minutes, 2 parts by weight of carboxymethyl chitosan solution is added, wherein the mass fraction of carboxymethyl chitosan in the carboxymethyl chitosan solution is 35%, and then dispersed in a high-speed disperser for 1 hour to obtain the modified filler.
[0042] A method for preparing a scratch-resistant and stain-resistant coating for a bathroom door panel comprises the following preparation steps:
[0043] S8-1: Mix the modified filler and the waterborne polyurethane resin according to formula 1, and stir at a speed of 500 r / min for 30 min to obtain a mixture C;
[0044] S8-2: polydimethylsiloxane, silane coupling agent KH550, palm wax and antioxidant 1010 were added to mixture C in sequence, and stirred at a speed of 850 r / min for 30 min to obtain mixture D;
[0045] S8-3: Deionized water and carboxymethyl cellulose were added to the mixture D in sequence, and the mixture was stirred at a speed of 650 r / min for 10 min to obtain the scratch-resistant and stain-resistant coating.
[0046] A scratch-resistant and stain-resistant surface treatment process for bathroom door panels includes the following process flows:
[0047] S9-1: The surface of the bathroom door panel was cleaned with 75% ethanol by mass, then washed three times with deionized water, dried at room temperature for 12 hours, and the surface of the door panel was polished with 300-mesh water-abrasive sandpaper to remove minor defects and increase surface roughness, thereby obtaining a door panel to be treated;
[0048] S9-2: Mix the anti-scratch and anti-fouling paint with deionized water to a viscosity of 55KU, use an air compression spray gun to evenly spray the anti-scratch and anti-fouling paint on the surface of the door panel to be treated, place it in an 80℃ oven for pre-curing for 20 minutes, and then place it in a UV curing machine for curing for 1 minute. The energy of the UV curing machine is 1200MJ / cm 2 , the distance of UV light source is 0.5m, and finally polishing treatment is performed to obtain a scratch-resistant and stain-resistant surface with a coating thickness of 20μm.
[0049] Example 2
[0050] The scratch-resistant and stain-resistant coating formula 2 is as follows: by weight, 80 parts of water-based acrylic resin, 20 parts of modified filler, 5 parts of polydimethylsiloxane, 4 parts of silane coupling agent KH560, 3 parts of hydroxyethyl cellulose, 2 parts of palm wax, 10760.5 parts of antioxidant, and 75 parts of deionized water.
[0051] Wherein, the preparation method of the modified filler is as follows:
[0052] S1-1: 30 parts by weight of silicon dioxide and 15 parts by weight of mussel shell powder were placed in a ball mill for ball milling at a ball milling speed of 400 r / min for 55 min, and passed through a 200-mesh sieve to obtain a mixture A;
[0053] S1-2: Mixture A and 45 parts by weight of deionized water were mixed, stirred at a speed of 600 r / min for 30 min, 1.5 parts by weight of a polyamide wax anti-settling agent was added, the mass fraction of the polyamide wax in the anti-settling agent was 50%, the pH was adjusted to 8 with a 2M sodium bicarbonate solution, and ultrasonic stirring was performed for 30 min to obtain a mixed solution B;
[0054] S1-3: 4 parts by weight of polytetrafluoroethylene emulsion is added to the mixed solution B, ultrasonicated at 50°C for 30 minutes, 2 parts by weight of carboxymethyl chitosan solution is added, wherein the mass fraction of carboxymethyl chitosan in the carboxymethyl chitosan solution is 35%, and then dispersed in a high-speed disperser for 1 hour to obtain the modified filler.
[0055] A method for preparing a scratch-resistant and stain-resistant coating for a bathroom door panel comprises the following preparation steps:
[0056] S8-1: The modified filler and the water-based acrylic resin were mixed according to formula 2, and stirred at a speed of 550 r / min for 30 min to obtain a mixture C;
[0057] S8-2: polydimethylsiloxane, silane coupling agent KH560, palm wax and antioxidant 1076 were added to mixture C in sequence, and stirred at a speed of 900 r / min for 30 min to obtain mixture D;
[0058] S8-3: Deionized water and hydroxyethyl cellulose were added to the mixture D in sequence, and the mixture was stirred at a speed of 700 r / min for 10 min to obtain the scratch-resistant and stain-resistant coating.
[0059] A scratch-resistant and stain-resistant surface treatment process for bathroom door panels includes the following process flows:
[0060] S9-1: The surface of the bathroom door panel was cleaned with 75% ethanol by mass, then washed three times with deionized water, dried at room temperature for 12 hours, and the surface of the door panel was polished with 300-mesh water-abrasive sandpaper to remove minor defects and increase surface roughness, thereby obtaining a door panel to be treated;
[0061] S9-2: Mix the anti-scratch and anti-fouling paint with deionized water until the viscosity is 60KU, use an air compression spray gun to evenly spray the anti-scratch and anti-fouling paint on the surface of the door panel to be treated, place it in an 80℃ oven for pre-curing for 15 minutes, and then place it in a UV curing machine for curing for 1.5 minutes. The energy of the UV curing machine is 1150MJ / cm 2 , the distance of UV light source is 0.5m, and finally polishing treatment is performed to obtain a scratch-resistant and stain-resistant surface with a coating thickness of 20μm.
[0062] Example 3
[0063] The formula 3 of the scratch-resistant and stain-resistant coating is as follows: by weight, 85 parts of waterborne polyurethane resin, 25 parts of modified filler, 5 parts of polydimethylsiloxane, 4 parts of silane coupling agent KH570, 3 parts of hydroxypropyl methylcellulose, 2 parts of palm wax, 10760.5 parts of antioxidant, and 75 parts of deionized water.
[0064] Wherein, the preparation method of the modified filler is as follows:
[0065] S1-1: 30 parts by weight of silicon dioxide and 15 parts by weight of mussel shell powder were placed in a ball mill for ball milling at a ball milling speed of 400 r / min for 60 min, and passed through a 200-mesh sieve to obtain a mixture A;
[0066] S1-2: Mix the mixture A with 50 parts by weight of deionized water, stir at a speed of 650 r / min for 30 min, add 2 parts by weight of a polyamide wax anti-settling agent, wherein the mass fraction of the polyamide wax in the anti-settling agent is 50%, adjust the pH to 9 with a 2M sodium bicarbonate solution, and stir ultrasonically for 30 min to obtain a mixed solution B;
[0067] S1-3: 4 parts by weight of polytetrafluoroethylene emulsion is added to the mixed solution B, ultrasonicated at 50°C for 30 minutes, 2 parts by weight of carboxymethyl chitosan solution is added, wherein the mass fraction of carboxymethyl chitosan in the carboxymethyl chitosan solution is 35%, and then dispersed in a high-speed disperser for 1 hour to obtain the modified filler.
[0068] A method for preparing a scratch-resistant and stain-resistant coating for a bathroom door panel comprises the following preparation steps:
[0069] S8-1: Mix the modified filler and the waterborne polyurethane resin according to formula 3, and stir at a speed of 600 r / min for 30 min to obtain a mixture C;
[0070] S8-2: polydimethylsiloxane, silane coupling agent KH570, palm wax and antioxidant 1076 were added to mixture C in sequence, and stirred at a speed of 950 r / min for 30 min to obtain mixture D;
[0071] S8-3: Deionized water and hydroxypropyl methylcellulose were added to the mixture D in sequence, and stirred at a speed of 750 r / min for 10 min to obtain the scratch-resistant and stain-resistant coating.
[0072] A scratch-resistant and stain-resistant surface treatment process for bathroom door panels includes the following process flows:
[0073] S9-1: The surface of the bathroom door panel was cleaned with 75% ethanol by mass, then washed three times with deionized water, dried at room temperature for 12 hours, and the surface of the door panel was polished with 300-mesh water-abrasive sandpaper to remove minor defects and increase surface roughness, thereby obtaining a door panel to be treated;
[0074] S9-2: Mix the anti-scratch and anti-fouling paint with deionized water to a viscosity of 55KU, use an air compression spray gun to evenly spray the anti-scratch and anti-fouling paint on the surface of the door panel to be treated, place it in an 80℃ oven for pre-curing for 10 minutes, and then place it in a UV curing machine for curing for 2 minutes. The energy of the UV curing machine is 1100MJ / cm 2 , the distance of UV light source is 0.5m, and finally polishing treatment is performed to obtain a scratch-resistant and stain-resistant surface with a coating thickness of 20μm.
[0075] Comparative Example 1
[0076] During the preparation of the modified filler, no polytetrafluoroethylene emulsion was added, and the remaining steps were consistent with those in Example 1.
[0077] Comparative Example 2
[0078] Polydimethylsiloxane was not added during the preparation of the coating, and the remaining steps were consistent with those in Example 1.
[0079] Comparative Example 3
[0080] No palm wax was added during the preparation of the coating, and the remaining steps were the same as those in Example 1.
[0081] The wear resistance of the embodiment and the comparative example was tested using a UMT-2MT friction and wear tester. The test conditions were water lubrication, a friction steel ball of grade G10 and a diameter of 6 mm, a load of 20 N, a frequency of 3 Hz, and a time of 30 min.
[0082] The stain resistance test was performed on the examples and comparative examples. 2 mL of liquid foundation was dripped onto the surface of the examples and comparative examples, and the surfaces were left to stand at room temperature for 24 hours. The liquid foundation was wiped off, and the color change of the surfaces of the examples and comparative examples was observed. The liquid foundation used in the test was Maybelline Customized Watery Liquid Foundation Soft Mist Sunscreen Edition 110.
[0083] The experimental results are summarized in the following table:
[0084] <![CDATA[Wear rate (mm 3 / N·m)]]> Stain resistance Example 1 <![CDATA[1.75×10 -4 ]]> No color change Example 2 <![CDATA[1.81×10 -4 ]]> No color change Example 3 <![CDATA[1.79×10 -4 ]]> No color change Comparative Example 1 <![CDATA[2.52×10 -4 ]]> Some degree of staining Comparative Example 2 <![CDATA[2.31×10 -4 ]]> No color change Comparative Example 3 <![CDATA[2.28×10 -4 ]]> Some degree of staining
[0085] It can be seen from the data of the embodiments and comparative examples that the use of silicon dioxide and mussel shell powder as wear-resistant fillers and the introduction of polytetrafluoroethylene emulsion can further increase the stain resistance and wear resistance of the coating. The addition of polydimethylsiloxane in the formula can also improve the wear resistance of the coating. The addition of palm wax can further improve the wear resistance and stain resistance of the coating.
[0086] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solution of the present invention still fall within the scope of the technical solution of the present invention.
Claims
1. A scratch-resistant and stain-resistant coating for bathroom door panels, characterized in that: The formula of the scratch-resistant and stain-resistant coating is as follows: by weight, 80-90 parts of water-based resin, 20-30 parts of modified filler, 5-8 parts of polydimethylsiloxane, 3-5 parts of silane coupling agent, 2-5 parts of thickener, 1-3 parts of palm wax, 0.5-1 part of antioxidant, and 65-75 parts of deionized water. in, The preparation method of the modified filler is as follows: S1-1: 40 to 50 parts by weight of filler are placed in a ball mill for ball milling at a speed of 400 r / min for 45 to 60 min, and passed through a 200-mesh sieve to obtain a mixture A; S1-2: Mix the mixture A with 40-50 parts by weight of deionized water, stir at 550-650 r / min for 30 min, add 1-2 parts by weight of an anti-settling agent, adjust the pH to 8-9 with a 2M sodium bicarbonate solution, and stir ultrasonically for 30 min to obtain a mixed solution B; S1-3: 3 to 5 parts by weight of polytetrafluoroethylene emulsion is added to the mixed solution B, ultrasonicated at 50° C. for 30 minutes, 1 to 3 parts by weight of carboxymethyl chitosan solution is added, and then dispersed in a high-speed disperser for 1 hour to obtain the modified filler.
2. The scratch-resistant and stain-resistant paint for bathroom door panels according to claim 1, characterized in that: The filler in S1-1 is a mixture of silicon dioxide and mussel shell powder in a mass ratio of 2:
1.
3. The scratch-resistant and stain-resistant paint for bathroom door panels according to claim 1, characterized in that: The anti-settling agent in S1-2 is a polyamide wax anti-settling agent, wherein the mass fraction of the polyamide wax is 50%.
4. The scratch-resistant and stain-resistant paint for bathroom door panels according to claim 1, characterized in that: The silane coupling agent is one of KH550, KH560 and KH570.
5. The scratch-resistant and stain-resistant paint for bathroom door panels according to claim 1, characterized in that: The water-based resin is one or both of water-based polyurethane resin and water-based acrylic resin.
6. The scratch-resistant and stain-resistant paint for bathroom door panels according to claim 1, characterized in that: The thickener is one of carboxymethyl cellulose, hydroxyethyl cellulose and hydroxypropyl methyl cellulose.
7. The scratch-resistant and stain-resistant paint for bathroom door panels according to claim 1, characterized in that: The antioxidant is one of antioxidant 1010 and antioxidant 1076.
8. A method for preparing the scratch-resistant and stain-resistant coating for bathroom door panels according to any one of claims 1 to 7, characterized in that: The method comprises the following preparation steps: S8-1: Mix the modified filler and the water-based resin according to the formula, and stir at a speed of 500-600 r / min for 30 min to obtain a mixture C; S8-2: polydimethylsiloxane, silane coupling agent, palm wax and antioxidant are added to mixture C in sequence, and stirred at a speed of 850-950 r / min for 30 min to obtain mixture D; S8-3: Add deionized water and thickener to mixed material D in sequence, and stir at a speed of 650-750 r / min for 10 min to obtain the scratch-resistant and stain-resistant coating.
9. A process for treating a bathroom door panel with a scratch-resistant and stain-resistant surface using the coating according to any one of claims 1 to 7, characterized in that: Including the following process: S9-1: The surface of the bathroom door panel was cleaned with 75% ethanol by mass, then washed three times with deionized water, dried at room temperature for 12 hours, and polished with 300-400 mesh water-abrasive sandpaper to remove minor defects and increase surface roughness, thereby obtaining a door panel to be treated; S9-2: Mix the anti-scratch and stain-resistant coating with deionized water to a viscosity of 55-60KU, use an air compression spray gun to evenly spray the anti-scratch and stain-resistant coating on the surface of the door panel to be treated, place it in an 80°C oven for pre-curing for 10-20 minutes, then place it in a UV curing machine for curing for 1-2 minutes, and finally polish it to obtain a scratch-resistant and stain-resistant surface.
10. The use of a scratch-resistant and stain-resistant coating for bathroom door panels according to claim 9, characterized in that: The UV curing energy is 1100-1200 MJ / cm 2 , the distance of UV light source is 0.5m.
Citation Information
Patent Citations
Fabrication method of wear-resistant automobile door panel
CN107955484A
Water-based wear-resistant coating and preparation method thereof
CN112409867A