Variable-temperature curing insulating solid crystal adhesive and preparation method thereof
Variable temperature curable insulated crystal glue prepared by using thermosetting resins, acrylic resins and inorganic fillers, the problems of low bond strength and fixed curing temperature of solid crystal glue are solved, and high bond strength and good anti-humidity and heat aging performance are achieved , suitable for advanced packaging technology.
Patent Information
- Application Number
- CN202411250806.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-12-03
AI Technical Summary
The existing solid crystal glue has low bond strength and fixed curing reaction temperature, making it difficult to meet different bonding and fixing requirements.
Adhesives composed of thermosetting resin, acrylic resin, inorganic filler and thermal cation initiator are used, and the curing reaction temperature can be adjusted between 85-150°C, and can be prepared by mixing uniformly and applying it to the surface of the protective base film to dry it. Variable temperature curing insulated crystal solid glue.
It realizes insulated solid crystal glue with high bonding strength, good anti-humidity and heat aging and hot and cold impact performance after curing. It is suitable for chip packaging. The curing reaction temperature can be adjusted according to process requirements to meet different packaging process requirements.
Smart Images

Figure BDA0005032194180000021 
Figure BDA0005032194180000023 
Figure BDA0005032194180000061
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electronic packaging materials, and in particular relates to a variable temperature curing insulating die-bonding adhesive and a preparation method thereof. Background Art
[0002] With the rapid development of 5G / 6G communications, big data, artificial intelligence and other technological fields, the electronic components used in the above fields are developing towards high integration, miniaturization and low cost. At present, the chip process has evolved to 3 nanometers and below. Moore's Law is facing extreme challenges. Advanced packaging technology has become one of the key paths to expand Moore's Law and promote the development of semiconductors. Advanced packaging has put forward higher requirements on die bonding methods and materials.
[0003] At present, the traditional die bonding method is to apply die attach adhesive (DAA) to the die bonding area of the bracket through a dispensing device, then attach the chip to the adhesive surface, and then bake and solidify. This method of die bonding has the following technical problems: (1) The diffusion area of the die adhesive applied to the die bonding area must be larger than the area of the chip to ensure that the chip is completely bonded and fixed, which is not conducive to reducing the package size; (2) Since the liquid die adhesive has surface tension and capillary action, it often forms a certain degree of glue creeping abnormality on the chip, resulting in short circuits or chip contamination. The chip needs to have sufficient thickness to prevent short circuits or chip surface contamination; (3) In the process of applying the die adhesive to the die bonding area, the dispensing process has very high requirements, such as the dispensing amount, dispensing position, and chip picking accuracy, which also puts higher requirements on the dispensing equipment.
[0004] To solve the above problems, in recent years, the industry has developed technologies such as wafer backside coating (WBC) and die attach film (DAF). Compared with the traditional dispensing die attach method, sheet-shaped die attach adhesive can provide more controllable thickness and fluidity, will not cause the problem of glue overflow, and has uniform glue creeping. It can maintain the stability of the glue layer before and after curing, and can inhibit chip cracking, adhesive inflow, chip tilting and other conditions. It has the advantage of flattening, and the die attach preparation process is simple, and has a lower coefficient of thermal expansion (CTE) after die attach. However, the common die attach adhesive currently has problems such as low bonding strength, fixed curing reaction temperature, and difficulty in meeting different bonding and fixing requirements.
[0005] In view of this, it is necessary to further improve the die-bonding adhesive in the prior art. Summary of the invention
[0006] To this end, the technical problem to be solved by the present invention is that the existing solid crystal adhesive has low bonding strength, a fixed curing reaction temperature, and is difficult to meet different bonding and fixing requirements. Therefore, a variable temperature curing insulating solid crystal adhesive is proposed, which has high bonding strength and a curing reaction temperature that can be adjusted between 85-150°C to meet a variety of bonding and fixing requirements.
[0007] In order to solve the above technical problems, the technical solution of the present invention is:
[0008] The first aspect of the present invention provides a variable temperature curable insulating die-bonding adhesive, which includes an adhesive, which is prepared from the following raw materials in parts by weight: 5-10 parts of thermosetting resin, 7-15 parts of acrylic resin, 5-10 parts of inorganic filler, and 1-3 parts of thermal cationic initiator.
[0009] Preferably, the acrylic resin has a structure shown in general formula (I):
[0010]
[0011] In the general formula (I), R1, R2, R3, and R4 are all selected from the following substituents: -COOCH3, -CN, -COOC4H9, And the general formula (I) contains at least two of the above substituents.
[0012] Preferably, the thermal cationic initiator has a structure shown in general formula (II):
[0013]
[0014] In the general formula (II), R 1 Select from the following substituents: HO- R 2 Select from the following substituents: H;
[0015] When R 1 for When R 2 for
[0016] R 1 When HO-, R 2 for Any of;
[0017] R 1 for When R 2 For H.
[0018] Preferably, the thermosetting resin is an alicyclic epoxy resin, and the alicyclic epoxy resin is 3,4-epoxycyclohexylmethyl 3,4-epoxycyclohexylcarboxylate.
[0019] Preferably, the filler is silicon dioxide, and the particle size of the silicon dioxide is 5-10 μm.
[0020] Preferably, the acrylic resin is a copolymer of two or more of methyl methacrylate, glycidyl methacrylate, butyl methacrylate and methacrylonitrile, the weight average molecular weight of the acrylic resin is 750000-1000000 g / mol, and the glass transition temperature of the acrylic resin is 3-7°C.
[0021] Preferably, the thermal cationic initiator is at least one of (4-acetoxyphenyl)(dimethyl)sulfonium hexafluoroantimonate and (4-hydroxyphenyl)(methyl)(benzyl)sulfonium hexafluoroantimonate. When the thermal cationic initiator is a mixture of (4-acetoxyphenyl)(dimethyl)sulfonium hexafluoroantimonate and (4-hydroxyphenyl)(methyl)(benzyl)sulfonium hexafluoroantimonate, the mass ratio of the two is 1:3-3:1.
[0022] Preferably, the variable temperature curable insulating die-bonding adhesive further comprises a protective base film layer, and the adhesive is coated and cured on the protective base film layer.
[0023] The second aspect of the present invention provides a method for preparing the variable temperature curing insulating die-bonding adhesive, which comprises the following steps:
[0024] S1. Mix the thermosetting resin, acrylic resin, inorganic filler and thermal cationic initiator uniformly according to the ratio until the thermal cationic initiator is completely dissolved to obtain a premix;
[0025] S2, coating the premix on the surface of the protective base film, and drying at 40-80° C. for 5-20 min to obtain a variable temperature curable insulating die-bonding adhesive.
[0026] Preferably, the acrylic resin is obtained by polymerizing at least two of methyl methacrylate, glycidyl methacrylate, butyl methacrylate and methacrylonitrile in an ethyl acetate solvent.
[0027] The above technical solution of the present invention has the following advantages compared with the prior art:
[0028] (1) The variable temperature curable insulating solid crystal adhesive provided by the present invention includes an adhesive, which is prepared from the following raw materials in parts by weight: 5-10 parts of thermosetting resin, 7-15 parts of acrylic resin, 5-10 parts of inorganic filler, and 1-3 parts of thermal cationic initiator. The curing system prepared by the above raw materials has an adjustable curing reaction temperature between 85-150°C, and the curing reaction temperature can be selectively adjusted according to different process requirements. When the chip is mounted, the preheating bonding temperature can be selectively adjusted between 40-85°C according to demand, so as to meet different solid crystal process requirements. At the same time, the variable temperature curable insulating solid crystal adhesive has high bonding strength. During pre-bonding, the bonding strength can reach 10.0N / mm, and the bonding strength after curing can reach 30.0N / mm. After thermal curing, the resistance to moisture and heat aging and cold and hot shock performance is good, and there is no delamination and fracture defects after bonding the chip; the bonding force to silicon wafers and metals is extremely high, and the bonding strength can reach 40-50MPa, which is suitable for chip packaging.
[0029] (2) The method for preparing a variable temperature curable insulating solid crystal adhesive provided by the present invention comprises: S1, mixing a thermosetting resin, an acrylic resin, an inorganic filler and a thermal cationic initiator in accordance with a ratio until the thermal cationic initiator is completely dissolved to obtain a premix; S2, coating the premix on the surface of a protective base film, and drying at 40-80°C for 5-20 minutes to obtain a variable temperature curable insulating solid crystal adhesive. The preparation method has simple steps, mild conditions, and the obtained variable temperature insulating solid crystal adhesive has excellent performance. DETAILED DESCRIPTION
[0030] Example 1
[0031] The present embodiment provides a variable temperature curable insulating die-bonding adhesive, which includes an adhesive. The adhesive is prepared from the following raw materials in parts by weight: 7 parts of thermosetting resin, 11 parts of acrylic resin, 7 parts of inorganic filler, and 3 parts of thermal cationic initiator.
[0032] It also includes a protective base film layer. The above-mentioned adhesive is coated and cured on the protective base film layer to form a variable temperature curing insulating solid crystal adhesive, wherein the protective base film layer adopts a polyester base film.
[0033] The variable temperature curing insulating solid crystal adhesive provided in this embodiment is an adhesive made by using the above-mentioned raw material components, and the curing reaction temperature is adjustable between 85-150°C. According to the bonding and fixing process requirements of different chips and other devices, the curing reaction temperature can be selectively adjusted. Further, when the chip is mounted, the preheating bonding temperature can be selectively adjusted between 40-85°C according to demand. At the same time, the variable temperature curing insulating solid crystal adhesive has high bonding strength. During pre-bonding, the bonding strength can reach 10.0N / mm, and under this preheating bonding process condition, the epoxy functional group in the system does not react under the chemical composition analysis test method. After curing, the bonding strength can reach 30.0N / mm, and the resistance to moisture and heat aging and cold and hot shock performance after thermal curing is good. Under the "double 85" test conditions (temperature 85±2°C, humidity 85%±5%), there is no delamination and fracture defects after bonding the silicon-based chip, and the bonding force remains above 95% before the test. The curing system formed by the above raw materials also has the advantage of a long storage period. After being stored at room temperature for more than 30 days, the conversion rate of epoxy functional groups in the curing system is still less than 5%.
[0034] The glass transition temperature (Tg) of the variable temperature curing insulating die-cement adhesive can reach above 150°C, and the bonding strength to silicon chips and metals is extremely high. After bonding the silicon chip and the copper substrate with the adhesive, the bonding strength can reach 40-50MPa, and the bonding strength can reach above 30MPa after the moisture sensitivity level test MSL1 (temperature 85°C, humidity 85% RH aging treatment for 7 days), and the high pressure cooking test (121°C, 2atm. water vapor environment) 24h bonding strength is above 30MPa. After 200 rounds of cold and hot shock 65-150°C, the bonding strength does not change much.
[0035] In this embodiment, the thermosetting resin is an alicyclic epoxy resin, specifically 3,4-epoxycyclohexylmethyl 3,4-epoxycyclohexylcarboxylate. The acrylic resin is prepared by copolymerizing two or more of methyl methacrylate, glycidyl methacrylate, butyl methacrylate and methacrylonitrile in an ethyl acetate solvent. In the polymer product solution, the weight parts of the acrylic resin are 11 parts and the weight parts of the ethyl acetate solvent are 72 parts. The acrylic resin has a repeating unit structure shown in the following general formula (I):
[0036]
[0037] In the general formula (I), R1, R2, R3, and R4 are all selected from the following substituents: -COOCH3, -CN, -COOC4H9,
[0038] The general formula (I) contains at least two of the above substituents. Specifically, in this embodiment, the acrylate has the following structure:
[0039]
[0040] The polyol is obtained by copolymerizing methyl methacrylate, glycidyl methacrylate, butyl methacrylate and methacrylonitrile, has a weight average molecular weight of 750,000-1,000,000 g / mol, and a glass transition temperature Tg of 3-7°C.
[0041] The thermal cationic initiator has the structure shown in the following general formula (II):
[0042]
[0043] In this embodiment, the thermal cationic initiator is (4-hydroxyphenyl)(methyl)(benzyl)sulfonium hexafluoroantimonate, and its structural formula is:
[0044]
[0045] Furthermore, the filler is an inorganic filler, specifically a silica filler, and the silica filler is a mixture of silica particles with a particle size of 5-10 μm. Within this particle size range, the silica filler has a concentrated particle size distribution and a good spherical structure, so that the formed insulating solid crystal adhesive has good fluidity and a low linear expansion coefficient. In this embodiment, preferably, the silica is also hydrophobically treated. Specifically, the silica can be surface-hydrophobically treated with a coupling agent and a leveling agent, so that the inorganic filler can be well dispersed in the resin system, not easy to agglomerate, and the viscosity change is less than 20% when stored in a sealed state at room temperature for 3 days, and it will not affect the coating of the solid crystal adhesive.
[0046] The variable temperature curing insulating die-bonding adhesive provided in this embodiment is prepared by the following steps:
[0047] S1. According to the above weight ratio, prepare the following raw materials: 7 parts of 3,4-epoxycyclohexylmethyl 3,4-epoxycyclohexyl carboxylate, 83 parts of acrylic resin solution (including 11 parts of acrylic resin and 72 parts of ethyl acetate solvent, the acrylic resin solution is obtained by polymerizing methyl methacrylate, glycidyl methacrylate, butyl methacrylate and methacrylonitrile in ethyl acetate), 7 parts of silica filler, and 3 parts of (4-hydroxyphenyl)(methyl)(benzyl)sulfonium hexafluoroantimonate thermal cationic initiator. Add the raw materials into a stirring kettle, stir and mix them evenly under heating until the thermal cationic initiator is fully dissolved to obtain a premix, then stop heating and cool to 25°C for standby use.
[0048] S2. The premix is coated on the surface of the polyester base film layer by a coating device, and the gap between the coating head and the polyester base film layer is set to 100 μm. After coating, it is dried in an oven at 60° C. for 20 minutes to remove the ethyl acetate solvent to obtain a variable temperature curable insulating solid crystal adhesive film.
[0049] Example 2
[0050] The present embodiment provides a variable temperature curable insulating die-bonding adhesive, which includes an adhesive. The adhesive is prepared from the following raw materials in parts by weight: 5 parts of thermosetting resin, 7 parts of acrylic resin, 5 parts of inorganic filler, and 1 part of thermal cationic initiator.
[0051] It also includes a protective base film layer. The above-mentioned adhesive is coated and cured on the protective base film layer to form a variable temperature curing insulating solid crystal adhesive, wherein the protective base film layer adopts a polyester base film.
[0052] In this embodiment, the thermosetting resin is an alicyclic epoxy resin, specifically 3,4-epoxycyclohexylmethyl 3,4-epoxycyclohexylcarboxylate. The acrylic resin is prepared by copolymerizing two or more of methyl methacrylate, glycidyl methacrylate, butyl methacrylate and methacrylonitrile in an ethyl acetate solvent. In the polymer product solution, the weight parts of the acrylic resin are 7 parts and the weight parts of the ethyl acetate solvent are 65 parts. The acrylic resin has a repeating unit structure shown in the following general formula (I):
[0053]
[0054] In the general formula (I), R1, R2, R3, and R4 are all selected from the following substituents: -COOCH3, -CN, -COOC4H9,
[0055] The general formula (I) contains at least two of the above substituents. In this embodiment, the acrylic resin has the following structure:
[0056]
[0057] It is prepared by polymerization of methyl methacrylate, glycidyl methacrylate and methacrylonitrile, has a weight average molecular weight of 750,000-1,000,000 g / mol, and a glass transition temperature Tg of 3-7°C.
[0058] The thermal cationic initiator has a structure shown in the following general formula (II):
[0059]
[0060] In this embodiment, the thermal cationic initiator is a mixture of (4-hydroxyphenyl)(methyl)(benzyl)sulfonium hexafluoroantimonate and (4-acetoxyphenyl)(dimethyl)sulfonium hexafluoroantimonate, the mass ratio of the two is 1:1, and the structural formula is:
[0061]
[0062] Furthermore, the filler is an inorganic filler, specifically a silica filler, and the silica filler is a mixture of silica particles with a particle size of 5-10 μm. In this embodiment, preferably, the silica is also subjected to a hydrophobic treatment.
[0063] The variable temperature curing insulating die-bonding adhesive provided in this embodiment is prepared by the following steps:
[0064] S1. According to the above weight ratio, prepare the following raw materials: 5 parts of 3,4-epoxycyclohexylmethyl 3,4-epoxycyclohexyl carboxylate, 72 parts of acrylic resin solution (including 7 parts of acrylic resin and 65 parts of ethyl acetate solvent, the acrylic resin solution is obtained by polymerizing at least two of methyl methacrylate, glycidyl methacrylate and methacrylonitrile in ethyl acetate), 5 parts of silica filler, 0.5 parts of (4-hydroxyphenyl)(methyl)(benzyl)sulfonium hexafluoroantimonate thermal cationic initiator, and 0.5 parts of (4-acetoxyphenyl)(dimethyl)sulfonium hexafluoroantimonate thermal cationic initiator. Add the raw materials into a stirring kettle, stir and mix them evenly under heating until the thermal cationic initiator is fully dissolved to obtain a premix, then stop heating and cool to 25°C for standby use.
[0065] S2. The premix is coated on the surface of the polyester base film layer by a coating device, and the gap between the coating head and the polyester base film layer is set to 100 μm. After coating, it is dried in an oven at 40° C. for 15 minutes to remove the ethyl acetate solvent to obtain a variable temperature curing insulating solid crystal adhesive film.
[0066] Example 3
[0067] The present embodiment provides a variable temperature curable insulating die-bonding adhesive, which includes an adhesive. The adhesive is prepared from the following raw materials in parts by weight: 10 parts of thermosetting resin, 15 parts of acrylic resin, 10 parts of inorganic filler, and 2 parts of thermal cationic initiator.
[0068] It also includes a protective base film layer. The above-mentioned adhesive is coated and cured on the protective base film layer to form a variable temperature curing insulating solid crystal adhesive, wherein the protective base film layer adopts a polyester base film.
[0069] In this embodiment, the thermosetting resin is an alicyclic epoxy resin, specifically 3,4-epoxycyclohexylmethyl 3,4-epoxycyclohexylcarboxylate. The acrylic resin is prepared by copolymerizing two or more of methyl methacrylate, glycidyl methacrylate, butyl methacrylate and methacrylonitrile in an ethyl acetate solvent. In the polymer product solution, the weight parts of the acrylic resin are 15 parts and the weight parts of the ethyl acetate solvent are 75 parts. The acrylic resin has a repeating unit structure shown in the following general formula (I):
[0070]
[0071] In the general formula (I), R1, R2, R3, and R4 are all selected from the following substituents: -COOCH3, -CN, -COOC4H9,
[0072] The general formula (I) contains at least two of the above substituents. In this embodiment, the structural formula of the acrylic resin is:
[0073]
[0074] The polyol is obtained by polymerizing methyl methacrylate, butyl methacrylate and methacrylonitrile, has a weight average molecular weight of 750,000-1,000,000 g / mol, and a glass transition temperature Tg of 3-7°C.
[0075] The thermal cationic initiator has the structure shown in the following general formula (II):
[0076]
[0077] In this embodiment, the thermal cationic initiator is a mixture of (4-hydroxyphenyl)(methyl)(benzyl)sulfonium hexafluoroantimonate and (4-acetoxyphenyl)(dimethyl)sulfonium hexafluoroantimonate, the mass ratio of the two is 1:3, and the structural formula is:
[0078]
[0079] Furthermore, the filler is an inorganic filler, specifically a silica filler, and the silica filler is a mixture of silica particles with a particle size of 5-10 μm. In this embodiment, preferably, the silica is also subjected to a hydrophobic treatment.
[0080] The variable temperature curing insulating die-bonding adhesive provided in this embodiment is prepared by the following steps:
[0081] S1. According to the above weight ratio, prepare the following raw materials: 10 parts of 3,4-epoxycyclohexylmethyl 3,4-epoxycyclohexyl carboxylate, 90 parts of acrylic resin solution (including 15 parts of acrylic resin and 75 parts of ethyl acetate solvent, the acrylic resin solution is obtained by polymerizing methyl methacrylate, butyl methacrylate and methacrylonitrile in ethyl acetate), 10 parts of silica filler, 0.5 parts of (4-hydroxyphenyl)(methyl)(benzyl)sulfonium hexafluoroantimonate thermal cationic initiator, and 1.5 parts of (4-acetoxyphenyl)(dimethyl)sulfonium hexafluoroantimonate thermal cationic initiator. Add the raw materials into a stirring kettle, stir and mix evenly under heating until the thermal cationic initiator is fully dissolved to obtain a premix, then stop heating and cool to 25°C for standby use.
[0082] S2. The premix is coated on the surface of the polyester base film layer by a coating device, and the gap between the coating head and the polyester base film layer is set to 100 μm. After coating, it is dried in an oven at 80° C. for 5 minutes to remove the ethyl acetate solvent to obtain a variable temperature curable insulating solid crystal adhesive film.
[0083] Example 4
[0084] The present embodiment provides a variable temperature curable insulating die-bonding adhesive, which includes an adhesive. The adhesive is prepared from the following raw materials in parts by weight: 8 parts of thermosetting resin, 12 parts of acrylic resin, 6 parts of inorganic filler, and 3 parts of thermal cationic initiator.
[0085] It also includes a protective base film layer. The above-mentioned adhesive is coated and cured on the protective base film layer to form a variable temperature curing insulating solid crystal adhesive, wherein the protective base film layer adopts a polyester base film.
[0086] In this embodiment, the thermosetting resin is an alicyclic epoxy resin, specifically 3,4-epoxycyclohexylmethyl 3,4-epoxycyclohexylcarboxylate. The acrylic resin is prepared by copolymerizing two or more of methyl methacrylate, glycidyl methacrylate, butyl methacrylate and methacrylonitrile in an ethyl acetate solvent. In the polymer product solution, the weight parts of the acrylic resin are 12 parts and the weight parts of the ethyl acetate solvent are 70 parts. The acrylic resin has a repeating unit structure shown in the following general formula (I):
[0087]
[0088] In the general formula (I), R1, R2, R3, and R4 are all selected from the following substituents: -COOCH3, -CN, -COOC4H9,
[0089] The general formula (I) contains at least two of the above substituents, has a weight average molecular weight of 750,000-1,000,000 g / mol, and a glass transition temperature Tg of 3-7°C.
[0090] The thermal cationic initiator has a structure shown in the following general formula (II):
[0091]
[0092] In this embodiment, the thermal cationic initiator is a mixture of (4-hydroxyphenyl)(methyl)(benzyl)sulfonium hexafluoroantimonate and (4-acetoxyphenyl)(dimethyl)sulfonium hexafluoroantimonate, the mass ratio of the two is 2:1, and the structural formula is:
[0093]
[0094] Furthermore, the filler is an inorganic filler, specifically a silica filler, and the silica filler is a mixture of silica particles with a particle size of 5-10 μm. In this embodiment, preferably, the silica is also subjected to a hydrophobic treatment.
[0095] The variable temperature curing insulating die-bonding adhesive provided in this embodiment is prepared by the following steps:
[0096] S1. According to the above weight ratio, prepare the following raw materials: 8 parts of 3,4-epoxycyclohexylmethyl 3,4-epoxycyclohexyl carboxylate, 82 parts of acrylic resin solution (including 12 parts of acrylic resin and 70 parts of ethyl acetate solvent, the acrylic resin solution is obtained by polymerizing at least two of methyl methacrylate, glycidyl methacrylate, butyl methacrylate and methacrylonitrile in ethyl acetate), 6 parts of silica filler, 2 parts of (4-hydroxyphenyl)(methyl)(benzyl)sulfonium hexafluoroantimonate thermal cationic initiator, and 1 part of (4-acetoxyphenyl)(dimethyl)sulfonium hexafluoroantimonate thermal cationic initiator. Add the raw materials into a stirring kettle, stir and mix evenly under heating until the thermal cationic initiator is fully dissolved to obtain a premix, then stop heating and cool to 25°C for standby use.
[0097] S2. The premix is coated on the surface of the polyester base film layer by a coating device, and the gap between the coating head and the polyester base film layer is set to 100 μm. After coating, it is dried in an oven at 60° C. for 20 minutes to remove the ethyl acetate solvent to obtain a variable temperature curable insulating solid crystal adhesive film.
[0098] Example 5
[0099] The present embodiment provides a variable temperature curable insulating die-bonding adhesive, which includes an adhesive. The adhesive is prepared from the following raw materials in parts by weight: 9 parts of thermosetting resin, 8 parts of acrylic resin, 8 parts of inorganic filler, and 2 parts of thermal cationic initiator.
[0100] It also includes a protective base film layer. The above-mentioned adhesive is coated and cured on the protective base film layer to form a variable temperature curing insulating solid crystal adhesive, wherein the protective base film layer adopts a polyester base film.
[0101] In this embodiment, the thermosetting resin is an alicyclic epoxy resin, specifically 3,4-epoxycyclohexylmethyl 3,4-epoxycyclohexylcarboxylate. The acrylic resin is prepared by copolymerizing two or more of methyl methacrylate, glycidyl methacrylate, butyl methacrylate and methacrylonitrile in an ethyl acetate solvent. In the polymer product solution, the weight parts of the acrylic resin are 8 parts and the weight parts of the ethyl acetate solvent are 69 parts. The acrylic resin has a repeating unit structure shown in the following general formula (I):
[0102]
[0103] In the general formula (I), R1, R2, R3, and R4 are all selected from the following substituents: -COOCH3, -CN, -COOC4H9,
[0104] The general formula (I) contains at least two of the above substituents, has a weight average molecular weight of 750,000-1,000,000 g / mol, and a glass transition temperature Tg of 3-7°C.
[0105] The thermal cationic initiator has a structure shown in the following general formula (II):
[0106]
[0107] In this embodiment, the thermal cationic initiator is (4-hydroxyphenyl)(methyl)(benzyl)sulfonium hexafluoroantimonate, and its structural formula is:
[0108]
[0109] Furthermore, the filler is an inorganic filler, specifically a silica filler, and the silica filler is a mixture of silica particles with a particle size of 5-10 μm. In this embodiment, preferably, the silica is also subjected to a hydrophobic treatment.
[0110] The variable temperature curing insulating die-bonding adhesive provided in this embodiment is prepared by the following steps:
[0111] S1. According to the above weight ratio, prepare the following raw materials: 9 parts of 3,4-epoxycyclohexylmethyl 3,4-epoxycyclohexyl carboxylate, 77 parts of acrylic resin solution (including 8 parts of acrylic resin and 69 parts of ethyl acetate solvent, the acrylic resin solution is obtained by polymerizing at least two of methyl methacrylate, glycidyl methacrylate, butyl methacrylate and methacrylonitrile in ethyl acetate), 6 parts of silica filler, and 2 parts of (4-hydroxyphenyl)(methyl)(benzyl)sulfonium hexafluoroantimonate thermal cationic initiator. Add the raw materials into a stirring kettle, stir and mix evenly under heating until the thermal cationic initiator is fully dissolved to obtain a premix, then stop heating and cool to 25°C for standby use.
[0112] S2. The premix is coated on the surface of the polyester base film layer by a coating device, and the gap between the coating head and the polyester base film layer is set to 100 μm. After coating, it is dried in an oven at 70° C. for 10 minutes to remove the ethyl acetate solvent to obtain a variable temperature curable insulating solid crystal adhesive film.
[0113] Experimental example
[0114] (1) Testing the thermal curing reaction temperature and optimal temperature of the variable temperature curing insulating die-bonding adhesive provided in the embodiments of the present application: Using differential scanning calorimetry (DSC) to measure the reaction exotherm of the variable temperature curing insulating die-bonding adhesive provided in embodiments 1 to 5 in the temperature range of 60-150°C, the starting position of the reaction exotherm is measured as the reaction starting temperature, and the temperature at the maximum value of the exothermic peak is the optimal thermal curing reaction temperature.
[0115] (2) Testing the glass transition temperature Tg of the variable temperature curing insulating die-bonding adhesive provided in Examples 1 to 5 of the present application after being fully cured at the optimal curing temperature: dynamic thermal analysis DMA is used for testing.
[0116] (3) Testing the bonding strength of the variable temperature curable insulating die-bonding adhesive provided in Examples 1 to 5 of the present application: The insulating die-bonding adhesive provided in the examples was bonded to the back of a silicon chip with a size of 2 mm*2 mm, and fully preheated and bonded for 2 minutes at the target temperature (60°C). A universal mechanical testing machine was used to perform a crystal pushing test to test the bonding strength during preheating and bonding. Further testing was performed to determine the bonding strength of the die-bonding adhesive to the chip after it was fully thermally cured at the target temperature.
[0117] (4) Testing the high-temperature baking adhesion stability of the variable temperature curing insulating die-bonding adhesive provided in Examples 1 to 5 of the present application: After the sample obtained by bonding in the above experimental example (3) is placed at 175°C and baked for 100 hours, the bonding strength test is performed again. If the bonding strength can be maintained at more than 85% of the strength before high-temperature baking, the test is judged to have passed.
[0118] (5) Test the high and low temperature impact resistance (hot and cold shock resistance) of the variable temperature curing insulating die-cement adhesive provided in Examples 1 to 5 of the present application: Place the sample obtained by bonding in the above experimental example (3) at ±70°C and cycle for 200 rounds, then perform a bonding strength test again. If the bonding strength can be maintained at more than 85% of the strength before the high and low temperature impact test, the test is judged to have passed.
[0119] The above test results are shown in Table 1 below.
[0120] Table 1
[0121]
[0122]
[0123] It can be seen from the above test results that the variable temperature curing insulating solid crystal adhesive provided in the present application has excellent bonding performance, high bonding strength, long storage period, good resistance to moisture and heat aging and resistance to cold and heat shock, and the curing reaction temperature can be selected and adjusted between 85-150°C according to the actual needs of the packaging process, thereby meeting the processability and reliability requirements of different packages.
[0124] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the present invention.
Claims
1. A variable temperature curing insulating die-bonding adhesive, characterized in that: The adhesive comprises an adhesive, which is prepared from the following raw materials in parts by weight: 5-10 parts of thermosetting resin, 7-15 parts of acrylic resin, 5-10 parts of inorganic filler, and 1-3 parts of thermal cationic initiator.
2. The variable temperature curing insulating die-bonding adhesive according to claim 1, characterized in that: The acrylic resin has a structure shown in general formula (I): In the general formula (I), R1, R2, R3, and R4 are all selected from the following substituents: -COOCH3, -CN, -COOC4H9, And the general formula (I) contains at least two of the above substituents.
3. The variable temperature curing insulating die-bonding adhesive according to claim 1, characterized in that: The thermal cationic initiator has a structure shown in general formula (II): In the general formula (II), R 1 Select from the following substituents: HO- R 2 Select from the following substituents: H; When R 1 for When R 2 for R 1 When HO-, R 2 for Any of; R 1 for When R 2 For H.
4. The variable temperature curing insulating die-bonding adhesive according to claim 1, characterized in that: The thermosetting resin is an alicyclic epoxy resin, and the alicyclic epoxy resin is 3,4-epoxycyclohexylmethyl 3,4-epoxycyclohexylcarboxylate.
5. The variable temperature curing insulating die-bonding adhesive according to claim 1, characterized in that: The filler is silicon dioxide, and the particle size of the silicon dioxide is 5-10 μm.
6. The variable temperature curing insulating die-bonding adhesive according to claim 2, characterized in that: The acrylic resin is a copolymer of two or more of methyl methacrylate, glycidyl methacrylate, butyl methacrylate and methacrylonitrile, the weight average molecular weight of the acrylic resin is 750000-1000000 g / mol, and the glass transition temperature of the acrylic resin is 3-7°C.
7. The variable temperature curing insulating die-bonding adhesive according to claim 3, characterized in that: The thermal cationic initiator is at least one of (4-acetoxyphenyl)(dimethyl)sulfonium hexafluoroantimonate and (4-hydroxyphenyl)(methyl)(benzyl)sulfonium hexafluoroantimonate. When the thermal cationic initiator is a mixture of (4-acetoxyphenyl)(dimethyl)sulfonium hexafluoroantimonate and (4-hydroxyphenyl)(methyl)(benzyl)sulfonium hexafluoroantimonate, the mass ratio of the two is 1:3-3:
1.
8. The variable temperature curing insulating die-bonding adhesive according to any one of claims 1 to 7, characterized in that: The variable temperature curable insulating die-bonding adhesive further comprises a protective base film layer, and the adhesive is coated and cured on the protective base film layer.
9. A method for preparing the variable temperature curing insulating die-bonding adhesive as claimed in claim 8, characterized in that: The steps include: S1. Mix the thermosetting resin, acrylic resin, inorganic filler and thermal cationic initiator uniformly according to the ratio until the thermal cationic initiator is completely dissolved to obtain a premix; S2, coating the premix on the surface of the protective base film, and drying at 40-80° C. for 5-20 min to obtain a variable temperature curable insulating die-bonding adhesive.
10. The method for preparing the adhesive for curing insulating die-bonding film at variable temperature according to claim 9, characterized in that: The acrylic resin is obtained by polymerizing at least two of methyl methacrylate, glycidyl methacrylate, butyl methacrylate and methacrylonitrile in an ethyl acetate solvent.
Citation Information
Patent Citations
Epoxy die-bonding adhesive and preparation method thereof and multi-chip embedded flexible printed circuit board
CN104559883A
Die bonding adhesive and preparation method thereof
CN107760240A
Adhesive composition
WO2011055588A1