Insulating paste for BC battery and preparation method of insulating paste
By adding specific epoxy resin and modified materials to the solar cell insulating glue, the component proportion and curing agent combination of the insulating glue are optimized, and the acid and alkali resistance and warping resistance of the insulating glue in high temperature and high humidity environments are solved. Improves the insulation performance and service life of battery backplane components.
Patent Information
- Application Number
- CN202411329502.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-24
- Publication Date
- 2024-12-03
AI Technical Summary
The existing solar cell insulating glue has poor acid resistance and alkali resistance in high temperature and high humidity environments, which can easily lead to reduced insulation performance of battery backplane components, and may even have short circuits. The shrinkage rate during curing is large, resulting in a curing layer. and cracking, affecting battery life and safety.
A kind of insulating glue for BC batteries was designed. By adding bisphenol A epoxy resin, multifunctional epoxy resin and dimer acid modified epoxy resin to the insulating glue system, its mass ratio is controlled, and QS-BE and DEG Nitrile rubber modified epoxy resin, optimized curing agent is a combination of modified aromatic amine and modified fatty amine, controls the mass ratio of component A and component B, and improves the hardness, adhesion and aging resistance of the insulating glue.
Effectively improve the hardness and aging resistance of insulating glue, avoid cracking, bulging and other defects under high temperature, high humidity and high temperature conditions, extend the service life of the battery, and meet the needs of screen printing technology, suitable for large-scale industrial promotion .
Smart Images

Figure BDA0005056409830000101 
Figure BDA0005056409830000111
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of C09J163 / 00, in particular to an insulating adhesive for BC batteries and a preparation method thereof. Background Art
[0002] A solar cell is a photoelectric semiconductor sheet that uses sunlight to generate electricity directly. As long as it is illuminated by light that meets certain illumination conditions, it can instantly output voltage and generate current in the presence of a circuit. In the field of battery manufacturing technology, especially in the manufacturing process of solar cells, the insulation performance of the battery backplane assembly is crucial. The main function of the battery backplane assembly is to protect the battery from environmental factors such as moisture, oxygen and ultraviolet rays, thereby extending the service life of the battery. In the existing solar cell manufacturing technology, insulating glue is usually used to achieve electrical isolation of different parts inside the battery. This insulating glue is usually made of polymer materials and has good insulating properties. In the prior art, the screen printing process is usually used to apply the insulating glue on the surface of the negative electrode grid of the battery cell, thereby improving the insulation performance of the battery backplane assembly. However, this method still has some problems in practical applications. Although the existing insulating glue has a certain temperature resistance, its acid resistance and alkali resistance will be significantly reduced in a high temperature and high humidity environment, resulting in reduced insulation performance of the battery backplane assembly and even possible short circuit. In addition, the existing insulating adhesive is prone to internal stress during the curing process due to its large shrinkage rate, which leads to problems such as warping and cracking of the insulating layer in the battery backplane assembly. These problems not only affect the insulation performance of the battery backplane assembly, but may also shorten the service life of the battery and even cause safety accidents. For example, a Chinese patent (publication number CN116463094A) discloses an insulating adhesive for IBC solar cells and a preparation method thereof, which mainly improves the resistance of the insulating adhesive to aluminum wire penetration by introducing a hyperbranched structure as a toughening agent in the epoxy resin system, but does not further explore the acid and alkali resistance and warping resistance of the product. Therefore, how to improve the acid and alkali resistance and warping resistance of the insulating adhesive is a problem that needs to be solved urgently in the current battery manufacturing technology field and the insulating adhesive preparation technology field. Summary of the invention
[0003] In order to solve the above problems, the present invention provides an insulating glue for BC batteries, which solves the problem that the existing insulating glue has poor aging resistance and is prone to bulging, stratification, bubbles, discoloration and other adverse phenomena in the insulating layer of the battery assembly under high temperature and high humidity or high and low temperature conditions for a long time, seriously affecting the reliability and service life of the battery.
[0004] On the one hand, the present invention provides an insulating glue for BC batteries, including component A and component B; in parts by weight, component A includes at least the following components: 40-60 parts of bisphenol A epoxy resin, 5-30 parts of multifunctional epoxy resin, 15-25 parts of dimer acid modified epoxy resin, 5-10 parts of toughening agent A, 10-20 parts of toughening agent B, 1-3 parts of coupling agent A, 0.5-2 parts of leveling agent, 0.3-1 parts of defoaming agent, and 0-2 parts of pigment; in parts by weight, component B includes at least the following components: 5-15 parts of modified fatty amine, 5-15 parts of modified aromatic amine, and 1-3 parts of coupling agent B.
[0005] As a preferred technical solution, the mass ratio of component A to component B is (3-7):1, preferably (4-6):1, and most preferably 5:1.
[0006] As a preferred technical solution, the functionality of the multifunctional epoxy resin is 3-4, preferably at least one of AG-80 (4.4-diaminodiphenylmethane tetraglycidylamine), AFG-90 (4-(2,3-epoxypropoxy)-N,N-bis(2,3-epoxypropyl)aniline), TDF-85 (4,5-epoxyhexane-1,2-dicarboxylic acid diglycidyl ester), and TGIC (triglycidyl isocyanurate), preferably AFG-90 (4-(2,3-epoxypropoxy)-N,N-bis(2,3-epoxypropyl)aniline).
[0007] As a preferred technical solution, the bisphenol A epoxy resin is selected from at least one of E44, E51, and E54, preferably E51.
[0008] As a preferred technical solution, the mass ratio of the bisphenol A epoxy resin, the multifunctional epoxy resin, and the dimer acid-modified epoxy resin is 6:(1.5-2.5):(1-3), preferably 6:(1.8-2.2):(1.8-2.2), and most preferably 3:1:1.
[0009] As a preferred technical solution, the toughening agent A is at least one of Beijing Jindao Qishi QS-BE, QS-14435, QS-BC, QS-N(08), QS-P24F, and QS-VA, preferably QS-BE.
[0010] As a preferred technical solution, the toughening agent B is a nitrile rubber modified epoxy resin toughening agent, preferably Huntsman RA1340.
[0011] As a preferred technical solution, the total mass of the toughener A and the toughener B accounts for 15-22% of the total mass of the epoxy resin (bisphenol A epoxy resin + multifunctional epoxy resin + dimer acid modified epoxy resin), preferably 20%.
[0012] As a preferred technical solution, the coupling agent A is KH560 and / or KH570, preferably KH560 (γ-glycidyloxypropyltrimethoxysilane).
[0013] As a preferred technical solution, the leveling agent is a silicone leveling agent, preferably BYK-378.
[0014] As a preferred technical solution, the defoamer is a non-silicon defoamer, preferably at least one of BYK-530 and BYK-6800, preferably BYK-530.
[0015] As a preferred technical solution, the modified fatty amine is selected from at least one of modified diethylenetriamine, modified triethylenetetramine, modified ethylenediamine, and modified hexamethylenediamine, preferably modified diethylenetriamine (Rich Chemical R-2281).
[0016] As a preferred technical solution, the modified aromatic amine is selected from at least one of modified meta-phenylenediamine, modified meta-phenylenediamine, modified dimethylthiotoluenediamine (Zhangjiagang Yarui Chemical E-300), and modified diaminodiphenylmethane, preferably modified dimethylthiotoluenediamine (Zhangjiagang Yarui Chemical E-300).
[0017] As a preferred technical solution, the coupling agent B is an amino silane coupling agent, selected from at least one of KH550, Evonik 1146, and Evonik 203, preferably KH550 (γ-aminopropyltriethoxysilane).
[0018] The present invention designs an insulating adhesive system including bisphenol A epoxy resin, multifunctional epoxy resin and dimer acid modified epoxy resin, and especially controls the mass ratio of bisphenol A epoxy resin, multifunctional epoxy resin and dimer acid modified epoxy resin to be 6:(1.8-2.2):(1.8-2.2), thereby effectively improving the hardness, adhesion and aging resistance of the insulating adhesive, and preventing defects such as cracking and bulging from occurring under high temperature, high humidity and high and low temperature impacts.
[0019] Furthermore, by introducing QS-BE and nitrile rubber modified epoxy resin, especially controlling the total mass of the toughener A and the toughener B to account for 15-22% of the total mass of the epoxy resin (bisphenol A epoxy resin + multifunctional epoxy resin + dimer acid modified epoxy resin), the product's tolerance to environmental factors is improved, and the product's bonding strength, low-temperature crack resistance, and resistance to cold and hot shocks are guaranteed.
[0020] Furthermore, the present invention optimizes the curing agent in the system to be a combination of modified aromatic amine and modified fatty amine, and controls the mass ratio of component A to component B to be (3-7):1 to ensure the adhesion of the insulating adhesive, balance the hardness and toughness of the insulating adhesive, avoid subsequent cracking and bulging problems, and help extend the service life of the battery.
[0021] The insulating adhesive preparation method provided by the invention is simple, easy to use, has excellent adhesion to silver and EVA substrates, the product performance is less affected by environmental factors, meets the requirements of screen printing technology, and is easy to achieve large-scale industrial promotion.
[0022] On the other hand, the present invention provides a method for preparing insulating glue for BC batteries, which comprises at least the following steps: stirring and dispersing bisphenol A epoxy resin, multifunctional epoxy resin, dimer acid modified epoxy resin, toughening agent A, toughening agent B, coupling agent A, leveling agent, defoaming agent and pigment, and filtering and packaging after vacuum treatment to obtain component A; stirring and dispersing modified fatty amine, modified aromatic amine and coupling agent B, and filtering and packaging after vacuum treatment to obtain component B; and stirring and mixing component A and component B when using.
[0023] As a preferred technical solution, the preparation method of component A is specifically as follows: bisphenol A epoxy resin, multifunctional epoxy resin, dimer acid modified epoxy resin, toughener A, toughener B, coupling agent A, leveling agent, defoamer, and pigment are added to a double planetary disperser, first stirred at 600-1200r / min for 3-6min, then stirred at 1500-2500r / min for 20-30min, keeping the temperature in the stirring kettle below 60°C, and after stirring and dispersing, vacuum (-0.01MPa) treatment for 5-15min, and then filtered and packaged to obtain component A.
[0024] As a preferred technical solution, the preparation method of the B component is specifically as follows: add the modified fatty amine, the modified aromatic amine, and the coupling agent B into a double planetary disperser, first stir at 600-1200r / min for 3-6min, then stir at 1000-2000r / min for 20-30min, keep the temperature in the stirring kettle below 60°C, and after stirring and dispersing, vacuum (-0.01MPa) for 5-15min, and then filter and package to obtain the B component.
[0025] Beneficial Effects
[0026] 1. The present invention provides an insulating glue for BC batteries, which solves the problem that the existing insulating glue has poor aging resistance and is prone to cause bulging, stratification, bubbles, discoloration and other adverse phenomena in the insulating layer of the battery assembly under high temperature and high humidity or high and low temperature conditions for a long time, seriously affecting the reliability and service life of the battery.
[0027] 2. The present invention designs an insulating adhesive system including bisphenol A epoxy resin, multifunctional epoxy resin, and dimer acid modified epoxy resin, and especially controls the mass ratio of bisphenol A epoxy resin, multifunctional epoxy resin, and dimer acid modified epoxy resin to be 6:(1.8-2.2):(1.8-2.2), thereby effectively improving the hardness, adhesion, and aging resistance of the insulating adhesive, and will not cause defects such as cracking and bulging under high temperature, high humidity, and high and low temperature impacts.
[0028] 3. The present invention introduces QS-BE and nitrile rubber to modify the epoxy resin, especially controls the total mass of the toughener A and the toughener B to account for 15-22% of the total mass of the epoxy resin (bisphenol A epoxy resin + multifunctional epoxy resin + dimer acid modified epoxy resin), thereby improving the product's tolerance to environmental factors and ensuring the product's bonding strength, low-temperature crack resistance, and resistance to cold and hot shocks.
[0029] 4. The present invention optimizes the curing agent in the system to be a combination of modified aromatic amine and modified fatty amine, and controls the mass ratio of component A to component B to be (3-7):1 to ensure the adhesion of the insulating glue, balance the hardness and toughness of the insulating glue, avoid subsequent cracking and bulging problems, and help extend the service life of the battery.
[0030] 5. The preparation method of the insulating adhesive provided by the present invention is simple, easy to use, has excellent adhesion to silver and EVA substrates, the product performance is less affected by environmental factors, meets the requirements of screen printing technology, and is easy to achieve large-scale industrial promotion. DETAILED DESCRIPTION
[0031] Example 1
[0032] Embodiment 1 of the present invention provides an insulating glue for BC battery, which is composed of component A and component B; in parts by weight, component A is composed of the following components: 60 parts of bisphenol A epoxy resin, 15 parts of multifunctional epoxy resin, 10 parts of dimer acid modified epoxy resin, 10 parts of toughening agent A, 10 parts of toughening agent B, 1 part of coupling agent A, 0.3 parts of leveling agent, 1 part of defoaming agent, and 0.3 parts of pigment; in parts by weight, component B is composed of the following components: 10 parts of modified fatty amine, 5 parts of modified aromatic amine, and 1 part of coupling agent B.
[0033] The mass ratio of component A to component B is 5:1.
[0034] The multifunctional epoxy resin is AFG-90 (4-(2,3-epoxypropoxy)-N,N-di(2,3-epoxypropyl)aniline).
[0035] The bisphenol A epoxy resin is E51.
[0036] The toughening agent A is Beijing Jindao Qishi QS-BE.
[0037] The toughening agent B is a nitrile rubber modified epoxy resin toughening agent, Huntsman RA1340.
[0038] The coupling agent A is KH560 (γ-glycidyloxypropyltrimethoxysilane).
[0039] The leveling agent is an organosilicon leveling agent BYK-378.
[0040] The defoamer is non-silicon defoamer BYK-530.
[0041] The modified fatty amine is modified diethylenetriamine (Richi Chemical R-2281).
[0042] The modified aromatic amine is modified dimethylthiotoluenediamine (Zhangjiagang Yarui Chemical E-300).
[0043] The coupling agent B is amino silane coupling agent KH550 (γ-aminopropyltriethoxysilane).
[0044] On the other hand, Example 1 of the present invention provides a method for preparing insulating glue for BC batteries, comprising the following steps: stirring and dispersing bisphenol A epoxy resin, multifunctional epoxy resin, dimer acid modified epoxy resin, toughening agent A, toughening agent B, coupling agent A, leveling agent, defoaming agent, and pigment, and filtering and packaging after vacuum treatment to obtain component A; stirring and dispersing modified fatty amine, modified aromatic amine, and coupling agent B, and filtering and packaging after vacuum treatment to obtain component B; and stirring and mixing component A and component B when in use.
[0045] The preparation method of the component A is specifically as follows: bisphenol A epoxy resin, multifunctional epoxy resin, dimer acid modified epoxy resin, toughener A, toughener B, coupling agent A, leveling agent, defoamer, and pigment are added to a double planetary disperser, first stirred at 800 r / min for 5 min, then stirred at 1800 r / min for 25 min, keeping the temperature in the stirring kettle below 60°C, and after stirring and dispersing, vacuum (-0.01 MPa) treated for 10 min, and then filtered and packaged to obtain component A.
[0046] The preparation method of the B component is specifically as follows: adding modified fatty amine, modified aromatic amine and coupling agent B into a double planetary disperser, stirring at 800 r / min for 5 min, then stirring at 1300 r / min for 20 min, keeping the temperature in the stirring kettle below 60° C., and after stirring and dispersing, vacuum (-0.01 MPa) treatment for 10 min, and then filtering and packaging to obtain the B component.
[0047] Example 2
[0048] Embodiment 2 of the present invention provides an insulating glue for BC battery, which is composed of component A and component B; in parts by weight, component A is composed of the following components: 60 parts of bisphenol A epoxy resin, 15 parts of multifunctional epoxy resin, 10 parts of dimer acid modified epoxy resin, 15 parts of toughening agent A, 15 parts of toughening agent B, 1 part of coupling agent A, 0.3 parts of leveling agent, 1 part of defoaming agent, and 0.3 parts of pigment; in parts by weight, component B is composed of the following components: 10 parts of modified fatty amine, 5 parts of modified aromatic amine, and 1 part of coupling agent B.
[0049] The mass ratio of component A to component B is 5:1.
[0050] The multifunctional epoxy resin is AFG-90 (4-(2,3-epoxypropoxy)-N,N-di(2,3-epoxypropyl)aniline).
[0051] The bisphenol A epoxy resin is E51.
[0052] The toughening agent A is Beijing Jindao Qishi QS-BE.
[0053] The toughening agent B is a nitrile rubber modified epoxy resin toughening agent, Huntsman RA1340.
[0054] The coupling agent A is KH560 (γ-glycidyloxypropyltrimethoxysilane).
[0055] The leveling agent is an organosilicon leveling agent BYK-378.
[0056] The defoamer is non-silicon defoamer BYK-530.
[0057] The modified fatty amine is modified diethylenetriamine (Richi Chemical R-2281).
[0058] The modified aromatic amine is modified dimethylthiotoluenediamine (Zhangjiagang Yarui Chemical E-300).
[0059] The coupling agent B is amino silane coupling agent KH550 (γ-aminopropyltriethoxysilane).
[0060] On the other hand, Example 2 of the present invention provides a method for preparing insulating glue for BC batteries, comprising the following steps: stirring and dispersing bisphenol A epoxy resin, multifunctional epoxy resin, dimer acid modified epoxy resin, toughening agent A, toughening agent B, coupling agent A, leveling agent, defoaming agent, and pigment, and filtering and packaging after vacuum treatment to obtain component A; stirring and dispersing modified fatty amine, modified aromatic amine, and coupling agent B, and filtering and packaging after vacuum treatment to obtain component B; and stirring and mixing component A and component B when in use.
[0061] The preparation method of the component A is specifically as follows: bisphenol A epoxy resin, multifunctional epoxy resin, dimer acid modified epoxy resin, toughener A, toughener B, coupling agent A, leveling agent, defoamer, and pigment are added to a double planetary disperser, first stirred at 800 r / min for 5 min, then stirred at 1500 r / min for 25 min, keeping the temperature in the stirring kettle below 60°C, and after stirring and dispersing, vacuum (-0.01 MPa) treated for 10 min, and then filtered and packaged to obtain component A.
[0062] The preparation method of the B component is specifically as follows: adding modified fatty amine, modified aromatic amine and coupling agent B into a double planetary disperser, stirring at 800 r / min for 5 min, then stirring at 1500 r / min for 20 min, keeping the temperature in the stirring kettle below 60° C., and after stirring and dispersing, vacuum (-0.01 MPa) treatment for 10 min, and then filtering and packaging to obtain the B component.
[0063] Example 3
[0064] Embodiment 3 of the present invention provides an insulating glue for BC battery, which is composed of component A and component B; in parts by weight, component A is composed of the following components: 60 parts of bisphenol A epoxy resin, 15 parts of multifunctional epoxy resin, 10 parts of dimer acid modified epoxy resin, 15 parts of toughening agent A, 15 parts of toughening agent B, 1 part of coupling agent A, 0.3 parts of leveling agent, 1 part of defoaming agent, and 0.3 parts of pigment; in parts by weight, component B is composed of the following components: 10 parts of modified fatty amine, 10 parts of modified aromatic amine, and 1 part of coupling agent B.
[0065] The mass ratio of component A to component B is 8:1.
[0066] The multifunctional epoxy resin is AFG-90 (4-(2,3-epoxypropoxy)-N,N-di(2,3-epoxypropyl)aniline).
[0067] The bisphenol A epoxy resin is E51.
[0068] The toughening agent A is Beijing Jindao Qishi QS-BE.
[0069] The toughening agent B is a nitrile rubber modified epoxy resin toughening agent, Huntsman RA1340.
[0070] The coupling agent A is KH560 (γ-glycidyloxypropyltrimethoxysilane).
[0071] The leveling agent is an organosilicon leveling agent BYK-378.
[0072] The defoamer is non-silicon defoamer BYK-530.
[0073] The modified fatty amine is modified diethylenetriamine (Richi Chemical R-2281).
[0074] The modified aromatic amine is modified dimethylthiotoluenediamine (Zhangjiagang Yarui Chemical E-300).
[0075] The coupling agent B is amino silane coupling agent KH550 (γ-aminopropyltriethoxysilane).
[0076] On the other hand, Example 3 of the present invention provides a method for preparing insulating glue for BC batteries, comprising the following steps: stirring and dispersing bisphenol A epoxy resin, multifunctional epoxy resin, dimer acid modified epoxy resin, toughening agent A, toughening agent B, coupling agent A, leveling agent, defoaming agent, and pigment, and filtering and packaging after vacuum treatment to obtain component A; stirring and dispersing modified fatty amine, modified aromatic amine, and coupling agent B, and filtering and packaging after vacuum treatment to obtain component B; stirring and mixing component A and component B when in use.
[0077] The preparation method of the component A is specifically as follows: bisphenol A epoxy resin, multifunctional epoxy resin, dimer acid modified epoxy resin, toughener A, toughener B, coupling agent A, leveling agent, defoamer, and pigment are added to a double planetary disperser, first stirred at 800 r / min for 5 min, then stirred at 1700 r / min for 25 min, keeping the temperature in the stirring kettle below 60°C, and after stirring and dispersing, vacuum (-0.01 MPa) treated for 10 min, and then filtered and packaged to obtain component A.
[0078] The preparation method of the B component is specifically as follows: adding modified fatty amine, modified aromatic amine and coupling agent B into a double planetary disperser, stirring at 800 r / min for 5 min, then stirring at 1500 r / min for 20 min, keeping the temperature in the stirring kettle below 60° C., and after stirring and dispersing, vacuum (-0.01 MPa) treatment for 10 min, and then filtering and packaging to obtain the B component.
[0079] Example 4
[0080] Embodiment 4 of the present invention provides an insulating glue for BC battery, which is composed of component A and component B; in parts by weight, component A is composed of the following components: 60 parts of bisphenol A epoxy resin, 20 parts of multifunctional epoxy resin, 20 parts of dimer acid modified epoxy resin, 10 parts of toughening agent A, 10 parts of toughening agent B, 1 part of coupling agent A, 0.3 parts of leveling agent, 1 part of defoaming agent, and 0.3 parts of pigment; in parts by weight, component B is composed of the following components: 10 parts of modified fatty amine, 5 parts of modified aromatic amine, and 1 part of coupling agent B.
[0081] The mass ratio of component A to component B is 5:1.
[0082] The multifunctional epoxy resin is AFG-90 (4-(2,3-epoxypropoxy)-N,N-di(2,3-epoxypropyl)aniline).
[0083] The bisphenol A epoxy resin is E51.
[0084] The toughening agent A is Beijing Jindao Qishi QS-BE.
[0085] The toughening agent B is a nitrile rubber modified epoxy resin toughening agent, Huntsman RA1340.
[0086] The coupling agent A is KH560 (γ-glycidyloxypropyltrimethoxysilane).
[0087] The leveling agent is an organosilicon leveling agent BYK-378.
[0088] The defoamer is non-silicon defoamer BYK-530.
[0089] The modified fatty amine is modified diethylenetriamine (Richi Chemical R-2281).
[0090] The modified aromatic amine is modified dimethylthiotoluenediamine (Zhangjiagang Yarui Chemical E-300).
[0091] The coupling agent B is amino silane coupling agent KH550 (γ-aminopropyltriethoxysilane).
[0092] On the other hand, Example 4 of the present invention provides a method for preparing insulating glue for BC batteries, comprising the following steps: stirring and dispersing bisphenol A epoxy resin, multifunctional epoxy resin, dimer acid modified epoxy resin, toughening agent A, toughening agent B, coupling agent A, leveling agent, defoaming agent, and pigment, and filtering and packaging after vacuum treatment to obtain component A; stirring and dispersing modified fatty amine, modified aromatic amine, and coupling agent B, and filtering and packaging after vacuum treatment to obtain component B; and stirring and mixing component A and component B when in use.
[0093] The preparation method of the component A is specifically as follows: bisphenol A epoxy resin, multifunctional epoxy resin, dimer acid modified epoxy resin, toughener A, toughener B, coupling agent A, leveling agent, defoamer, and pigment are added to a double planetary disperser, first stirred at 800 r / min for 5 min, then stirred at 1800 r / min for 25 min, keeping the temperature in the stirring kettle below 60°C, and after stirring and dispersing, vacuum (-0.01 MPa) treated for 10 min, and then filtered and packaged to obtain component A.
[0094] The preparation method of the B component is specifically as follows: adding modified fatty amine, modified aromatic amine and coupling agent B into a double planetary disperser, stirring at 800 r / min for 5 min, then stirring at 1200 r / min for 20 min, keeping the temperature in the stirring kettle below 60° C., and after stirring and dispersing, vacuum (-0.01 MPa) treatment for 10 min, and then filtering and packaging to obtain the B component.
[0095] Example 5
[0096] Embodiment 5 of the present invention provides an insulating glue for BC battery, which is composed of component A and component B; in parts by weight, component A is composed of the following components: 60 parts of bisphenol A epoxy resin, 20 parts of multifunctional epoxy resin, 10 parts of dimer acid modified epoxy resin, 15 parts of toughening agent A, 10 parts of toughening agent B, 1 part of coupling agent A, 0.3 parts of leveling agent, 1 part of defoaming agent, and 0.3 parts of pigment; in parts by weight, component B is composed of the following components: 10 parts of modified fatty amine, 5 parts of modified aromatic amine, and 1 part of coupling agent B.
[0097] The mass ratio of component A to component B is 8:1.
[0098] The multifunctional epoxy resin is AFG-90 (4-(2,3-epoxypropoxy)-N,N-di(2,3-epoxypropyl)aniline).
[0099] The bisphenol A epoxy resin is E51.
[0100] The toughening agent A is Beijing Jindao Qishi QS-BE.
[0101] The toughening agent B is a nitrile rubber modified epoxy resin toughening agent, Huntsman RA1340.
[0102] The coupling agent A is KH560 (γ-glycidyloxypropyltrimethoxysilane).
[0103] The leveling agent is an organosilicon leveling agent BYK-378.
[0104] The defoamer is non-silicon defoamer BYK-530.
[0105] The modified fatty amine is modified diethylenetriamine (Richi Chemical R-2281).
[0106] The modified aromatic amine is modified dimethylthiotoluenediamine (Zhangjiagang Yarui Chemical E-300).
[0107] The coupling agent B is amino silane coupling agent KH550 (γ-aminopropyltriethoxysilane).
[0108] On the other hand, Example 5 of the present invention provides a method for preparing insulating glue for BC batteries, comprising the following steps: stirring and dispersing bisphenol A epoxy resin, multifunctional epoxy resin, dimer acid modified epoxy resin, toughening agent A, toughening agent B, coupling agent A, leveling agent, defoaming agent, and pigment, and filtering and packaging after vacuum treatment to obtain component A; stirring and dispersing modified fatty amine, modified aromatic amine, and coupling agent B, and filtering and packaging after vacuum treatment to obtain component B; and stirring and mixing component A and component B when using.
[0109] The preparation method of the component A is specifically as follows: bisphenol A epoxy resin, multifunctional epoxy resin, dimer acid modified epoxy resin, toughener A, toughener B, coupling agent A, leveling agent, defoamer, and pigment are added to a double planetary disperser, first stirred at 800 r / min for 5 min, then stirred at 1800 r / min for 25 min, keeping the temperature in the stirring kettle below 60°C, and after stirring and dispersing, vacuum (-0.01 MPa) treated for 10 min, and then filtered and packaged to obtain component A.
[0110] The preparation method of the B component is specifically as follows: adding modified fatty amine, modified aromatic amine and coupling agent B into a double planetary disperser, stirring at 800 r / min for 5 min, then stirring at 1300 r / min for 20 min, keeping the temperature in the stirring kettle below 60° C., and after stirring and dispersing, vacuum (-0.01 MPa) treatment for 10 min, and then filtering and packaging to obtain the B component.
[0111] Performance Testing Methods
[0112] The insulating glue provided in the embodiment was screen-printed onto the surface of a silicon wafer battery (a substrate containing silicon and silver), cured at 130°C for 15 minutes, and the film thickness was 50 μm. The hardness, adhesion, and aging resistance of the insulating glue for BC batteries were tested. The test results are shown in Table 1.
[0113] Table 1
[0114]
[0115]
Claims
1. An insulating adhesive for BC battery, characterized in that: It comprises component A and component B; component A comprises at least the following components by weight: 40-60 parts of bisphenol A epoxy resin, 5-30 parts of multifunctional epoxy resin, 15-25 parts of dimer acid modified epoxy resin, 5-10 parts of toughening agent A, 10-20 parts of toughening agent B, 1-3 parts of coupling agent A, 0.3-2 parts of leveling agent, 0.5-1 parts of defoaming agent, and 0-2 parts of pigment; Calculated by weight, component B at least includes the following components: 5-15 parts of modified fatty amine, 5-15 parts of modified aromatic amine, and 1-3 parts of coupling agent B.
2. The insulating adhesive for BC battery according to claim 1, characterized in that: The mass ratio of component A to component B is (3-7):
1.
3. The insulating adhesive for BC battery according to claim 1 or 2, characterized in that: The mass ratio of the bisphenol A epoxy resin, the multifunctional epoxy resin and the dimer acid modified epoxy resin is 6:(1.5-2.5):(1-3).
4. The insulating adhesive for BC battery according to claim 3, characterized in that: The functionality of the multifunctional epoxy resin is 3-4.
5. The insulating adhesive for BC battery according to claim 4, characterized in that: The total mass of the toughening agent A and the toughening agent B accounts for 15-22% of the total mass of the epoxy resin.
6. The insulating adhesive for BC battery according to claim 5, characterized in that: The toughening agent B is a nitrile rubber modified epoxy resin toughening agent.
7. The insulating adhesive for BC battery according to claim 5, characterized in that: The modified fatty amine is selected from at least one of modified diethylenetriamine, modified triethylenetetramine, modified ethylenediamine and modified hexamethylenediamine.
8. The insulating adhesive for BC battery according to claim 5, characterized in that: The modified aromatic amine is selected from at least one of modified meta-phenylenediamine, modified meta-phenylenediamine, modified dimethylthiotoluenediamine and modified diaminodiphenylmethane.
9. The insulating adhesive for BC battery according to claim 8, characterized in that: The coupling agent B is an amino silane coupling agent.
10. A method for preparing the insulating adhesive for BC batteries according to any one of claims 1 to 9, characterized in that: At least the following steps are included: bisphenol A epoxy resin, multifunctional epoxy resin, dimer acid modified epoxy resin, toughening agent A, toughening agent B, coupling agent A, leveling agent, defoaming agent, and pigment are stirred and dispersed, vacuum treated, filtered and packaged to obtain component A; The modified fatty amine, the modified aromatic amine and the coupling agent B are stirred and dispersed, vacuum treated, filtered and packaged to obtain the B component; When using, stir and mix component A and component B.
Citation Information
Patent Citations
Insulation paste for IBC solar cell and preparation method thereof
CN116463094A
Cited By
Insulation paste composition, insulation paste layer and back contact battery
CN121718296A