Modified medium-temperature magnesium oxide powder additive as well as modification method and application thereof
Through baking of talc powder and boric acid and coating technology of painted silicone resin and epoxy modified silicone resin, the modified medium-temperature magnesium oxide powder solves the problem of insufficient performance of existing medium-temperature magnesium oxide powder, significantly improving the insulation. Voltage resistance and current leakage resistance meet the needs of high-quality heating pipes.
Patent Information
- Application Number
- CN202411184522.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-12-03
AI Technical Summary
The existing medium-temperature magnesium oxide powder has shortcomings in insulation, voltage resistance, current leakage resistance and fluidity, and it is difficult to meet the high standard requirements of high-quality heating pipes for electrically grade magnesium oxide powder.
Use talc powder and boric acid to bake at 800℃~850℃, and then coated with painted silicone resin and epoxy modified silicone resin to prepare modified medium temperature magnesium oxide powder. This method improves the moisture absorption resistance of magnesium oxide particles. , resistance to hydration, insulation and current leakage resistance, and improve voltage resistance in thermal state.
Modified medium-temperature magnesium oxide powder significantly improves resistance to moisture absorption, hydration resistance, insulation and current leakage resistance, enhances thermal pressure resistance, and meets the high standard requirements of high-quality heating pipes for electrically-grade magnesium oxide powder.
Smart Images

Figure BDA0005013143650000081 
Figure BDA0005013143650000091
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of magnesium oxide fire-resistant electrical insulating materials, and in particular relates to a modified medium-temperature magnesium oxide powder additive and a modification method and application thereof. Background Art
[0002] Electrical grade magnesium oxide is a vital refractory insulating material in electric heating equipment. In the electric heating product market, it is widely used in various electric heating equipment, such as electric heating tubes. With the continuous development of electrical equipment, the demand for high-quality electrical grade magnesium oxide is also growing.
[0003] Electrical grade magnesium oxide needs to have a variety of characteristics: First, it should have high thermal conductivity at the working temperature so that the heat can be quickly transferred to the surface of the tube, so that the resistance wire and the tube wall temperature are closer. Secondly, when the temperature rises to the working temperature, it must maintain good insulation performance. In addition, in order to ensure a good filling effect, magnesium oxide must have a certain particle size, and the shape should usually be round rather than flaky, because round particles have a high filling density and good fluidity. At the same time, no matter at room temperature or high temperature, there should be no corrosion to the heating wire material and the tube. There are also strict regulations on water absorption. For example, the water absorption of medium temperature moisture-proof type is usually not higher than 0.10%.
[0004] However, the existing electrical grade magnesium oxide powder for heating tubes still has some deficiencies in certain performance aspects, such as poor insulation, pressure resistance, current leakage resistance and fluidity.
[0005] In order to overcome the shortcomings of existing electrical grade magnesium oxide powder and improve its performance, scientific researchers are constantly conducting research and exploration. A common method is to perform surface activation treatment on magnesium oxide powder or adopt a specific preparation process. For example, by adding substances such as silicone moisture-proof liquid and controlling the proportion of each component and the processing conditions, the insulation and fluidity of magnesium oxide powder can be improved. In this way, electrical grade magnesium oxide powder can improve the insulation performance under different conditions such as normal state, wet state and after immersion in water, while improving fluidity and appropriate filling density, which is more conducive to its application in electric heating pipes.
[0006] However, with the widespread application of electric heating equipment in various fields, the requirements for the performance of electrical grade magnesium oxide powder are also constantly increasing, and existing materials are increasingly difficult to fully meet the high standards of high-quality heating tubes for electrical grade magnesium oxide powder. Therefore, it is necessary to further optimize the application of medium-temperature magnesium oxide powder in electrical grade magnesium oxide, and continue to innovate and improve the preparation process to meet the growing needs of the market and industry. Summary of the invention
[0007] Due to the limitations of raw materials and processes, the existing medium-temperature magnesium oxide powder has deficiencies in insulation, pressure resistance, current leakage resistance and fluidity. It is increasingly difficult for existing materials to fully meet the high standards of high-quality heating tubes for electrical-grade magnesium oxide powder. The present invention provides a modified medium-temperature magnesium oxide powder additive and its modification method and application, which uses talcum powder and boric acid as raw materials, bakes at 800°C to 850°C, and then sequentially coats with lacquer silicone resin and epoxy-modified silicone resin to prepare the additive, and coats the additive on the surface of magnesium oxide particles. The obtained modified medium-temperature magnesium oxide powder has excellent anti-moisture absorption, anti-hydration, insulation and anti-current leakage properties, and can well improve hot withstand voltage and prevent high-voltage current breakdown. The specific technical scheme is as follows:
[0008] A modified medium-temperature magnesium oxide powder additive, the additive is made of the following raw materials in parts by mass: 20 to 25 parts of talc, 1 to 1.5 parts of boric acid, 1.5 to 2 parts of lacquer silicone resin, and 1.5 to 2 parts of epoxy-modified silicone resin;
[0009] The preparation method of the additive is:
[0010] S1: talcum powder and boric acid are mixed according to mass fractions, baked at 800°C to 850°C for 1h to 1.5h, and then cooled to obtain baking material A;
[0011] S2: spraying silicone resin onto the surface of the baked material A particles according to the mass ratio, and then baking at 200°C to 250°C for 40min to 60min, and after cooling, breaking up to obtain the coating material B;
[0012] S3: Spray epoxy-modified silicone resin onto the particle surface of coating material B according to the mass ratio, and then bake at 200°C to 250°C for 30min to 40min. After cooling, break it up, sieve it, and take the sieved material to obtain the additive.
[0013] In the above technical solution, the particle size of the talcum powder is passed through a 325-mesh sieve; the particle size of the boric acid is passed through a 325-mesh sieve.
[0014] In the above technical solution, the model of the paint silicone resin is SH-9, the main component is methylphenyl polysilicone resin, the solid content is 50%; and the high temperature resistance is 800°C.
[0015] In the above technical solution, the epoxy modified silicone resin has a model of SJ-804, a solid content of 50%, and a high temperature resistance of 800°C.
[0016] In S3 of the preparation method of the above technical solution, the screening is through a 325-mesh sieve.
[0017] A method for modifying medium-temperature magnesium oxide powder, using the above-mentioned modified medium-temperature magnesium oxide powder additive, the modification method comprises the following steps:
[0018] According to the mass ratio, magnesium oxide: additive: talcum powder: thermosetting epoxy resin = (90-95): (5-10): (0.1-0.3): (1.5-2.5), firstly mix the additive and talcum powder evenly, then mix with magnesium oxide and thermosetting epoxy resin, modify at 250°C-300°C for 1h-2h, cool, break up, sieve, take the sieve under the sieve, and obtain modified medium-temperature magnesium oxide powder.
[0019] In the above modification method, the particle size of the magnesium oxide is through a 60-mesh sieve; the magnesium oxide is light-burned magnesium oxide, which is obtained by calcining magnesite at 700°C to 800°C.
[0020] In the above modification method, the particle size of the talc powder is passed through a 325-mesh sieve; and the talc powder is talc powder sintered at 800° C. to 850° C.
[0021] In the above modification method, the mesh number of the sieving sieve is 60 meshes.
[0022] In the above modification method, the modified medium-temperature magnesium oxide powder is electrical grade magnesium oxide powder, which is used to prepare heating tubes.
[0023] The modified medium-temperature magnesium oxide powder additive and its modification method and application provided by the present invention have the following beneficial effects compared with the prior art:
[0024] 1. The additive of the present invention uses talcum powder and boric acid as raw materials, and bakes at 800°C to 850°C for 1h to 1.5h to obtain a composite of talcum powder and boric oxide with reduced porosity, namely baked material A, wherein the reduced porosity of talcum powder can effectively improve the moisture absorption and hydration resistance, and the boric oxide can improve the insulation, current leakage prevention and hot pressure resistance.
[0025] 2. Spraying the surface of the baked material A particles with lacquer silicone resin, and then baking at 200°C to 250°C, a lacquer silicone resin coating material, i.e., coating material B, can be obtained. The lacquer silicone resin coating layer can improve the material's resistance to moisture absorption, resistance to hydration, insulation and anti-current leakage properties.
[0026] 3. Spraying epoxy-modified silicone resin on the particle surface of coating material B and then baking at 200°C to 250°C can obtain epoxy-modified silicone resin coating material, which can further improve the material's anti-hygroscopicity, anti-hydration, insulation and anti-current leakage properties. In addition, spraying epoxy-modified silicone resin can also make up for the surface defects of coating material B, that is, make up for the defects of paint silicone resin spraying.
[0027] 4. The combination of paint silicone resin and epoxy modified silicone resin has a good synergistic effect, which can greatly improve the material's anti-moisture absorption, anti-hydration, insulation and anti-current leakage properties.
[0028] 5. In the modification method of medium-temperature magnesium oxide powder, magnesium oxide, additives, talcum powder and thermosetting epoxy resin are mixed in a certain proportion, modified at 250℃~300℃, and the adhesiveness of thermosetting epoxy resin is used to coat the additives and talcum powder on the surface of magnesium oxide particles, and the surface of magnesium oxide is modified. The obtained modified medium-temperature magnesium oxide powder has excellent anti-hygroscopic, anti-hydration, insulation and anti-current leakage properties, and can well improve the hot withstand voltage and prevent high-voltage current breakdown. It can meet the use requirements of high-quality heating tubes for electrical grade magnesium oxide powder.
[0029] 6. Designing a uniform mixture of additives and talcum powder can improve the dispersion and fluidity of the additives, improve the homogeneity of the additive coating, and ensure the quality of the coating layer. DETAILED DESCRIPTION
[0030] The present invention is further described below in conjunction with specific implementation cases, but the present invention is not limited to these embodiments.
[0031] Example 1
[0032] A modified medium-temperature magnesium oxide powder additive is prepared from the following raw materials in parts by mass: 22 parts of talcum powder, 1.2 parts of boric acid, 1.8 parts of lacquer silicone resin, and 1.6 parts of epoxy modified silicone resin; wherein the particle size of the talcum powder is through a 325-mesh sieve; and the particle size of the boric acid is through a 325-mesh sieve.
[0033] The preparation method of the additive is:
[0034] S1: talcum powder and boric acid were mixed according to mass fractions, baked at 820°C for 1h, and cooled to obtain baking material A;
[0035] S2: spraying silicone resin onto the surface of the baked material A particles according to the mass ratio, and then baking at 220°C for 50 minutes. After cooling, breaking up, and obtaining the coating material B;
[0036] S3: Spray epoxy-modified silicone resin onto the particle surface of coating material B according to the mass ratio, then bake at 220°C for 35 min, and after cooling, break it up, pass it through a 325-mesh sieve, and take the sieve residue to obtain an additive.
[0037] A method for modifying medium-temperature magnesium oxide powder, using the above-mentioned modified medium-temperature magnesium oxide powder additive, the modification method comprises the following steps:
[0038] According to the mass ratio, magnesium oxide: additive: talcum powder: thermosetting epoxy resin = 92:8:0.2:2, the additive and talcum powder are first mixed evenly, and then mixed with magnesium oxide and thermosetting epoxy resin, modified at 280°C for 1.5h, cooled, broken up, passed through a 60-mesh sieve, and the sieve under the sieve is taken to obtain modified medium-temperature magnesium oxide powder;
[0039] The particle size of magnesium oxide is through a 60-mesh sieve, and the magnesium oxide is light-burned magnesium oxide, which is obtained by calcining magnesite at 750° C. The particle size of talc powder is through a 325-mesh sieve, and the talc powder is talc powder sintered at 850° C.
[0040] The modified medium-temperature magnesium oxide powder prepared in this embodiment is electrical grade magnesium oxide powder, which is used to prepare heating tubes.
[0041] Example 2
[0042] A modified medium-temperature magnesium oxide powder additive is prepared from the following raw materials in parts by mass: 20 parts of talcum powder, 1 part of boric acid, 1.5 parts of lacquer silicone resin, and 1.5 parts of epoxy-modified silicone resin; wherein the particle size of the talcum powder is through a 325-mesh sieve; and the particle size of the boric acid is through a 325-mesh sieve.
[0043] The preparation method of the additive is:
[0044] S1: talcum powder and boric acid are mixed according to mass fractions, baked at 800°C for 1h, and cooled to obtain baking material A;
[0045] S2: spraying silicone resin onto the surface of the baked material A particles according to the mass ratio, and then baking at 200°C for 40 minutes. After cooling, breaking up, and obtaining the coating material B;
[0046] S3: Spray epoxy-modified silicone resin onto the particle surface of coating material B according to the mass ratio, then bake at 200°C for 30 min, and after cooling, break it up, pass it through a 325-mesh sieve, and take the sieve to obtain the additive.
[0047] A method for modifying medium-temperature magnesium oxide powder, using the above-mentioned modified medium-temperature magnesium oxide powder additive, the modification method comprises the following steps:
[0048] According to the mass ratio, magnesium oxide: additive: talcum powder: thermosetting epoxy resin = 90:5:0.1:1.5, the additive and talcum powder are first mixed evenly, and then mixed with magnesium oxide and thermosetting epoxy resin, modified at 250°C for 1h, cooled, broken up, passed through a 60-mesh sieve, and the sieve under the sieve is taken to obtain modified medium-temperature magnesium oxide powder;
[0049] The particle size of magnesium oxide is through a 60-mesh sieve, and the magnesium oxide is light-burned magnesium oxide, which is obtained by calcining magnesite at 700° C. The particle size of talc powder is through a 325-mesh sieve, and the talc powder is talc powder sintered at 800° C.
[0050] The modified medium-temperature magnesium oxide powder prepared in this embodiment is electrical grade magnesium oxide powder, which is used to prepare heating tubes.
[0051] Example 3
[0052] A modified medium-temperature magnesium oxide powder additive is prepared from the following raw materials in parts by mass: 21 parts of talcum powder, 1.1 parts of boric acid, 1.6 parts of lacquer silicone resin, and 1.7 parts of epoxy modified silicone resin; wherein the particle size of the talcum powder is through a 325-mesh sieve; and the particle size of the boric acid is through a 325-mesh sieve.
[0053] The preparation method of the additive is:
[0054] S1: talcum powder and boric acid were mixed according to mass fractions, baked at 810°C for 1h, and cooled to obtain baking material A;
[0055] S2: spraying silicone resin onto the surface of the baked material A particles according to the mass ratio, and then baking at 210°C for 45 minutes. After cooling, breaking up, and obtaining the coating material B;
[0056] S3: According to the mass ratio, epoxy modified silicone resin is sprayed onto the particle surface of coating material B, and then baked at 210°C for 32 minutes. After cooling, the particles are broken up and passed through a 325 mesh sieve, and the particles under the sieve are taken to obtain an additive.
[0057] A method for modifying medium-temperature magnesium oxide powder, using the above-mentioned modified medium-temperature magnesium oxide powder additive, the modification method comprises the following steps:
[0058] According to the mass ratio, magnesium oxide: additive: talcum powder: thermosetting epoxy resin = 91:6:0.15:1.8, the additive and talcum powder are first mixed evenly, and then mixed with magnesium oxide and thermosetting epoxy resin, modified at 260°C for 1h, cooled, broken up, passed through a 60-mesh sieve, and the sieve under the sieve is taken to obtain modified medium-temperature magnesium oxide powder;
[0059] The particle size of magnesium oxide is through a 60-mesh sieve, and the magnesium oxide is light-burned magnesium oxide, which is obtained by calcining magnesite at 720° C. The particle size of talc powder is through a 325-mesh sieve, and the talc powder is talc powder sintered at 850° C.
[0060] The modified medium-temperature magnesium oxide powder prepared in this embodiment is electrical grade magnesium oxide powder, which is used to prepare heating tubes.
[0061] Example 4
[0062] A modified medium-temperature magnesium oxide powder additive is prepared from the following raw materials in parts by mass: 24 parts of talcum powder, 1.4 parts of boric acid, 1.8 parts of lacquer silicone resin, and 1.8 parts of epoxy-modified silicone resin; wherein the particle size of the talcum powder is through a 325-mesh sieve; and the particle size of the boric acid is through a 325-mesh sieve.
[0063] The preparation method of the additive is:
[0064] S1: talcum powder and boric acid were mixed according to mass fractions, baked at 840°C for 1.5h, and cooled to obtain baking material A;
[0065] S2: spraying silicone resin onto the surface of the baked material A particles according to the mass ratio, and then baking at 240°C for 55 minutes. After cooling, breaking up, and obtaining the coating material B;
[0066] S3: Spray epoxy-modified silicone resin onto the particle surface of coating material B according to the mass ratio, then bake at 240°C for 38 minutes, and after cooling, break it up, pass it through a 325-mesh sieve, and take the sieve residue to obtain an additive.
[0067] A method for modifying medium-temperature magnesium oxide powder, using the above-mentioned modified medium-temperature magnesium oxide powder additive, the modification method comprises the following steps:
[0068] According to the mass ratio, magnesium oxide: additive: talcum powder: thermosetting epoxy resin = 94:8:0.25:2.2, the additive and talcum powder are first mixed evenly, and then mixed with magnesium oxide and thermosetting epoxy resin, modified at 290°C for 2h, cooled, broken up, passed through a 60-mesh sieve, and the sieve under the sieve is taken to obtain modified medium-temperature magnesium oxide powder;
[0069] The particle size of magnesium oxide is through a 60-mesh sieve, and the magnesium oxide is light-burned magnesium oxide, which is obtained by calcining magnesite at 780° C. The particle size of talc powder is through a 325-mesh sieve, and the talc powder is talc powder sintered at 800° C.
[0070] The modified medium-temperature magnesium oxide powder prepared in this embodiment is electrical grade magnesium oxide powder, which is used to prepare heating tubes.
[0071] Example 5
[0072] A modified medium-temperature magnesium oxide powder additive is prepared from the following raw materials in parts by mass: 25 parts of talcum powder, 1.5 parts of boric acid, 2 parts of lacquer silicone resin, and 2 parts of epoxy-modified silicone resin; wherein the particle size of the talcum powder is through a 325-mesh sieve; and the particle size of the boric acid is through a 325-mesh sieve.
[0073] The preparation method of the additive is:
[0074] S1: talcum powder and boric acid were mixed according to mass fractions, baked at 850°C for 1.5h, and cooled to obtain baking material A;
[0075] S2: spraying silicone resin onto the surface of the baked material A particles according to the mass ratio, and then baking at 250°C for 60 minutes. After cooling, breaking up, and obtaining the coating material B;
[0076] S3: Spray epoxy-modified silicone resin onto the particle surface of coating material B according to the mass ratio, then bake at 250°C for 40 min, and after cooling, break it up, pass it through a 325-mesh sieve, and take the sieve residue to obtain an additive.
[0077] A method for modifying medium-temperature magnesium oxide powder, using the above-mentioned modified medium-temperature magnesium oxide powder additive, the modification method comprises the following steps:
[0078] According to the mass ratio, magnesium oxide: additive: talcum powder: thermosetting epoxy resin = 95:10:0.3:2.5, the additive and talcum powder are first mixed evenly, and then mixed with magnesium oxide and thermosetting epoxy resin, modified at 300°C for 2h, cooled, broken up, passed through a 60-mesh sieve, and the sieve under the sieve is taken to obtain modified medium-temperature magnesium oxide powder;
[0079] The particle size of magnesium oxide is through a 60-mesh sieve, and the magnesium oxide is light-burned magnesium oxide, which is obtained by calcining magnesite at 800° C. The particle size of talc powder is through a 325-mesh sieve, and the talc powder is talc powder sintered at 820° C.
[0080] The modified medium-temperature magnesium oxide powder prepared in this embodiment is electrical grade magnesium oxide powder, which is used to prepare heating tubes.
[0081] Example 6
[0082] A modified medium-temperature magnesium oxide powder additive is prepared from the following raw materials in parts by mass: 20 parts of talcum powder, 1.5 parts of boric acid, 1.5 parts of lacquer silicone resin, and 2 parts of epoxy-modified silicone resin; wherein the particle size of the talcum powder is through a 325-mesh sieve; and the particle size of the boric acid is through a 325-mesh sieve.
[0083] The preparation method of the additive is:
[0084] S1: talcum powder and boric acid were mixed according to mass fractions, baked at 800°C for 1.5h, and cooled to obtain baking material A;
[0085] S2: spraying silicone resin onto the surface of the baked material A particles according to the mass ratio, and then baking at 200°C for 60 minutes. After cooling, breaking up, and obtaining the coating material B;
[0086] S3: Spray epoxy-modified silicone resin onto the particle surface of coating material B according to the mass ratio, then bake at 200°C for 40 min, and after cooling, break it up, pass it through a 325-mesh sieve, and take the sieve residue to obtain an additive.
[0087] A method for modifying medium-temperature magnesium oxide powder, using the above-mentioned modified medium-temperature magnesium oxide powder additive, the modification method comprises the following steps:
[0088] According to the mass ratio, magnesium oxide: additive: talcum powder: thermosetting epoxy resin = 90:10:0.1:2.5, the additive and talcum powder are first mixed evenly, and then mixed with magnesium oxide and thermosetting epoxy resin, modified at 250°C for 2h, cooled, broken up, passed through a 60-mesh sieve, and the sieve under the sieve is taken to obtain modified medium-temperature magnesium oxide powder;
[0089] The particle size of magnesium oxide is through a 60-mesh sieve, and the magnesium oxide is light-burned magnesium oxide, which is obtained by calcining magnesite at 700° C. The particle size of talc powder is through a 325-mesh sieve, and the talc powder is talc powder sintered at 850° C.
[0090] The modified medium-temperature magnesium oxide powder prepared in this embodiment is electrical grade magnesium oxide powder, which is used to prepare heating tubes.
[0091] Example 7
[0092] A modified medium-temperature magnesium oxide powder additive is prepared from the following raw materials in parts by mass: 25 parts of talcum powder, 1 part of boric acid, 2 parts of lacquer silicone resin, and 1.5 parts of epoxy modified silicone resin; wherein the particle size of the talcum powder is through a 325-mesh sieve; and the particle size of the boric acid is through a 325-mesh sieve.
[0093] The preparation method of the additive is:
[0094] S1: talcum powder and boric acid were mixed according to mass fractions, baked at 850°C for 1h, and cooled to obtain baking material A;
[0095] S2: spraying silicone resin onto the surface of the baked material A particles according to the mass ratio, and then baking at 250°C for 40 minutes. After cooling, breaking up, and obtaining the coating material B;
[0096] S3: Spray epoxy-modified silicone resin onto the particle surface of coating material B according to the mass ratio, then bake at 250°C for 30 min, and after cooling, break it up, pass it through a 325-mesh sieve, and take the sieve to obtain the additive.
[0097] A method for modifying medium-temperature magnesium oxide powder, using the above-mentioned modified medium-temperature magnesium oxide powder additive, the modification method comprises the following steps:
[0098] According to the mass ratio, magnesium oxide: additive: talcum powder: thermosetting epoxy resin = 95:5:0.3:1.5, the additive and talcum powder are first mixed evenly, and then mixed with magnesium oxide and thermosetting epoxy resin, modified at 300°C for 1h, cooled, broken up, passed through a 60-mesh sieve, and the sieve under the sieve is taken to obtain modified medium-temperature magnesium oxide powder;
[0099] The particle size of magnesium oxide is through a 60-mesh sieve, and the magnesium oxide is light-burned magnesium oxide, which is obtained by calcining magnesite at 800° C. The particle size of talc powder is through a 325-mesh sieve, and the talc powder is talc powder sintered at 800° C.
[0100] The modified medium-temperature magnesium oxide powder prepared in this embodiment is electrical grade magnesium oxide powder, which is used to prepare heating tubes.
[0101] The paint silicone resin used in the above-mentioned embodiments 1 to 7 is the paint silicone resin of Hubei Xinsihai Chemical Co., Ltd., model SH-9, and the main component is methylphenyl polysilicone resin; the index parameters are, appearance: liquid; (150°C, 2h) solid content: 50%; (Tu-4 cup, 25°C) viscosity: 12s; (200°C) drying time: 40min; (400°C, 3h) thermal weight loss: 4.2%; (20±5°C) normal electrical breakdown strength: 68KV / mm; (200±2°C) high temperature electrical breakdown strength: 35KV / mm; (20±5°C, relative humidity 95%, after 24h) damp electrical breakdown strength: 46KV / mm; (20±5°C) normal volume resistance: 10 15 Ω·cm; (200±2℃) High temperature volume resistance: 10 12 Ω·cm; (20±5℃, relative humidity 95, after 24h) volume resistance when wet: 10 13 Ω·cm; Performance: High temperature resistance 800℃.
[0102] The epoxy-modified silicone resin used in the above-mentioned Examples 1 to 7 is the epoxy-modified silicone resin of Congyang County Sanjin Pigment Co., Ltd., model SJ-804, (150°C, 2h) solid content: 50%; (200°C) drying time: 30min; (Tu-4 cup, 23°C) viscosity: 30s; high temperature resistance 800°C.
[0103] Comparative Example 1
[0104] No boric acid is added to the additive, and the boric acid component is replaced by talcum powder. Other parameters and methods are the same as in Example 1.
[0105] Comparative Example 2
[0106] No silicone resin is added to the additives, that is, S2 is omitted, and no coating material B is prepared; in S3, coating material B is directly replaced by baking material A. Other parameters and methods are the same as in Example 1.
[0107] Comparative Example 3
[0108] No epoxy modified silicone resin is added to the additive, that is, S3 is omitted; in S2, the coating material B is cooled, broken up, passed through a 325 mesh sieve, and the sieve underfill is taken to obtain the additive. Other parameters and methods are the same as those in Example 1.
[0109] Comparative Example 4
[0110] No lacquer silicone resin or epoxy modified silicone resin is added to the additive, that is, S2 and S3 are omitted, and after the baking material A is cooled, it is broken up and passed through a 325 mesh sieve, and the sieve underfill is taken to obtain the additive. Other parameters and methods are the same as those in Example 1.
[0111] Comparative Example 5
[0112] In the method for modifying the medium-temperature magnesium oxide powder, no thermosetting epoxy resin is added, magnesium oxide, additives and talcum powder are directly mixed, passed through a 60-mesh sieve, and the sieve underflow is taken to obtain modified medium-temperature magnesium oxide powder. Other parameters and methods are the same as in Example 1.
[0113] According to the test method of "Electrical Grade Magnesium Oxide" JB / T 8508, the performance of the modified medium-temperature magnesium oxide powder prepared in the above embodiments and comparative examples was tested, wherein the leakage current was 9W / cm 2 The withstand voltage was tested at 2 mA, 50 Hz, and after heating for 60 seconds. The test results are shown in Table 1.
[0114] Table 1 Performance test results
[0115]
[0116]
[0117] From the above results, it can be seen that the modified medium-temperature magnesium oxide prepared in Examples 1 to 7 has good resistance to moisture absorption, hydration, insulation and current leakage, and has high hot voltage resistance. From the comparison of the results of Example 1 and Comparative Examples 1 to 4, it can be seen that the addition of boric acid can improve the insulation and current leakage resistance of the material, as well as the hot voltage resistance; the coating of lacquer silicone resin and the coating of epoxy-modified silicone resin can both improve the material's resistance to moisture absorption, hydration, insulation and current leakage; the use of lacquer silicone resin and epoxy-modified silicone resin has a good synergistic effect, which can greatly improve the material's resistance to moisture absorption, hydration, insulation and current leakage.
[0118] From the comparison of the results of Example 1 and Comparative Example 5, it can be seen that the modification of magnesium oxide powder by coating the additive can well improve the various properties of the material. However, when the additive is simply mixed with magnesium oxide powder, the various properties are significantly reduced.
Claims
1. A modified medium temperature magnesium oxide powder additive, It is characterized in that The additive is made of the following raw materials in parts by mass: 20 to 25 parts of talc, 1 to 1.5 parts of boric acid, 1.5 to 2 parts of lacquer silicone resin, and 1.5 to 2 parts of epoxy modified silicone resin; The preparation method of the additive is: S1: talcum powder and boric acid are mixed according to mass fractions, baked at 800°C to 850°C for 1h to 1.5h, and then cooled to obtain baking material A; S2: spraying silicone resin onto the surface of the baked material A particles according to the mass ratio, and then baking at 200°C to 250°C for 40min to 60min, and after cooling, breaking up to obtain the coating material B; S3: Spray epoxy-modified silicone resin onto the particle surface of coating material B according to the mass ratio, and then bake at 200°C to 250°C for 30min to 40min. After cooling, break it up, sieve it, and take the sieved material to obtain the additive.
2. A modified medium-temperature magnesium oxide powder additive according to claim 1, It is characterized in that The particle size of the talc powder is through a 325-mesh sieve; the particle size of the boric acid is through a 325-mesh sieve.
3. A modified medium-temperature magnesium oxide powder additive according to claim 1, It is characterized in that The model of the paint silicone resin is SH-9, the main component of which is methylphenyl polysilicone resin, with a solid content of 50% and a high temperature resistance of 800°C.
4. A modified medium-temperature magnesium oxide powder additive according to claim 1, It is characterized in that The epoxy modified organic silicon resin has a model of SJ-804, a solid content of 50%, and a high temperature resistance of 800°C.
5. A modified medium-temperature magnesium oxide powder additive according to claim 1, It is characterized in that In S3 of the preparation method, the screening is through a 325-mesh sieve.
6. A method for modifying medium-temperature magnesium oxide powder, using the modified medium-temperature magnesium oxide powder additive according to claim 1, It is characterized in that The modification method comprises the following steps: According to the mass ratio, magnesium oxide: additive: talcum powder: thermosetting epoxy resin = (90-95): (5-10): (0.1-0.3): (1.5-2.5), firstly mix the additive and talcum powder evenly, then mix with magnesium oxide and thermosetting epoxy resin, modify at 250°C-300°C for 1h-2h, cool, break up, sieve, take the sieve under the sieve, and obtain modified medium-temperature magnesium oxide powder.
7. A method for modifying medium-temperature magnesium oxide powder according to claim 6, It is characterized in that The particle size of the magnesium oxide is through a 60-mesh sieve; the magnesium oxide is light-burned magnesium oxide, which is obtained by calcining magnesite at 700° C. to 800° C.
8. A method for modifying medium-temperature magnesium oxide powder according to claim 6, It is characterized in that The particle size of the talc powder is 325 mesh sieve; the talc powder is sintered at 800° C. to 850° C.
9. A method for modifying medium-temperature magnesium oxide powder according to claim 6, It is characterized in that The mesh number of the sieve is 60 meshes.
10. A method for modifying medium-temperature magnesium oxide powder according to claim 6, It is characterized in that The modified medium-temperature magnesium oxide powder is electrical grade magnesium oxide powder and is used for preparing heating tubes.