AOD (Argon Oxygen Decarburization) rapid deep dephosphorization method for chromium-nickel pig iron melt

By desilicate and dechromatize the chromium-nickel pig iron melt in the AOD furnace, the problem of difficulty in deep dephosphorization of AOD smelting is solved, and the rapid deep dephosphorization of cheap chromium-nickel pig iron is achieved, and the production can be used for low-cost chromium-nickel pig iron is achieved. Ultra-low phosphochromium nickel pig iron melt of phosphorus special stainless steel simplifies the process and reduces costs.

CN119061223AActive Publication Date: 2024-12-03SHANXI TAIGANG STAINLESS STEEL CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410980508.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-12-03
Estimated Expiration
2044-07-22

AI Technical Summary

Technical Problem

The AOD smelting process is difficult to achieve deep dephosphorization, resulting in the inability to mass-used chromium nickel pig iron premelting for the production of special stainless steel varieties with complex processes and high smelting costs.

Method used

After desilicate and dechromatize in the AOD furnace with chromium-nickel pig iron melt, deep dephosphorization operation is achieved by controlling the addition of oxygen and lime slag, and the phosphorus content is gradually reduced to ultra-low levels.

Benefits of technology

The production process is simplified, the smelting cost is reduced, and the rapid deep dephosphorization of cheap chromium-nickel pig iron is achieved. It produces ultra-low phosphium-nickel pig iron melt that can be used for low-phosphorus special stainless steel, which has good promotion value and economic benefits.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses an AOD (Argon Oxygen Decarburization) rapid deep dephosphorization method for chromium-nickel pig iron melt, which comprises the following steps of: adding the chromium-nickel pig iron melt into an AOD furnace, carrying out desiliconization and dechromization operation, supplying oxygen by an AOD top lance, blowing O2 and N2 gas by a side lance, and adding lime for slagging in batches; and after desilicication and dechroming are finished, slag is removed, AOD deep dephosphorization operation is carried out, an AOD top lance supplies oxygen, a side lance supplies O2 and N2 gas, limestone is added for slagging in the deep dephosphorization process, and ultra-low-phosphorus chromium-nickel pig iron melt is produced. The technical problem that AOD deep dephosphorization is difficult is solved, the purposes that the ultralow-phosphorus chromium-nickel pig iron melt is prepared through AOD rapid deep dephosphorization by adopting cheap chromium-nickel pig iron as a main raw material, and the ultralow-phosphorus chromium-nickel pig iron melt is used as the stainless steel mother liquor to produce the low-phosphorus special stainless steel variety are achieved, the production process is simplified, and the production cost is reduced. And the smelting cost is reduced, the short-process green low-cost low-phosphorus special stainless steel smelting process method is developed, and good popularization value and economic benefits are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of stainless steel production, and in particular relates to a method for rapid deep dephosphorization of chromium-nickel pig iron melt by AOD. Background Art

[0002] AOD (Argon Oxygen Decarburization) smelting process is an argon oxygen decarburization process method. It is the most commonly used process for producing stainless steel. Currently, about 75% of stainless steel is produced by AOD process. AOD process relies on the good kinetic conditions of side blowing, and achieves decarburization and chromium preservation by increasing the process temperature and reducing the partial pressure of CO gas. It has many advantages such as simple equipment structure, convenient operation, the use of cheap high-carbon ferrochrome and return stainless steel, and easy production of low-carbon and ultra-low-carbon stainless steel. However, since stainless steel does not have the ability to dephosphorize during smelting, AOD smelting of stainless steel can only use pre-treated dephosphorized iron water as stainless steel mother liquor, which has complicated procedures and high smelting costs.

[0003] At present, with the promotion of the process of producing chromium-nickel pig iron from laterite nickel ore through RKEF (Rotary Klin Electric Furnace), the low-priced nickel pig iron has become the main raw material of stainless steel and is widely used in the production of ordinary stainless steel, reducing the cost of stainless steel smelting. However, nickel pig iron contains relatively high residual elements such as P, S, Si, and Cr, which cannot achieve deep dephosphorization of stainless steel.

[0004] Chinese patent application 201210212501.7 entitled "A method for producing stainless steel mother liquor" discloses a method for dephosphorization of high-phosphorus chromium-nickel pig iron by melting in an electric furnace, and the phosphorus content of the produced stainless steel mother liquor is as low as 0.020%. In Chinese patent application 201110220308.3 entitled "A method for dephosphorizing high-phosphorus chromium-nickel pig iron", after desiliconization to 0.05-1.0% by electric furnace, AOD is added for dephosphorization, and the final P of AOD is ≤0.04%. The chromium-nickel pig iron pre-melt produced in the above-mentioned prior art cannot achieve deep dephosphorization by AOD, and further dephosphorization is difficult, so the chromium-nickel pig iron pre-melt cannot be used in batches as stainless steel mother liquor to produce low-phosphorus special stainless steel varieties. Summary of the invention

[0005] In order to solve the above-mentioned technical problems existing in the prior art, the present invention develops a method for rapid deep dephosphorization of chromium-nickel pig iron melt by AOD, which realizes the purpose of preparing ultra-low-phosphorus chromium-nickel pig iron melt by AOD rapid deep dephosphorization of chromium-nickel pig iron pre-melt produced by RKEF, and using the ultra-low-phosphorus chromium-nickel pig iron melt as stainless steel mother liquor to produce low-phosphorus special stainless steel varieties.

[0006] The method for rapid deep dephosphorization of chromium-nickel pig iron melt by AOD of the present invention comprises the following steps:

[0007] Step 1: The chromium-nickel pig iron melt is added into the AOD furnace for desiliconization and dechromization operations, wherein the AOD top gun supplies oxygen, the side guns spray O2 and N2 gases, and lime is added in batches to make slag;

[0008] Step 2: After desiliconization and dechromization, the slag is removed and AOD deep dephosphorization operation is carried out. The AOD top gun supplies oxygen, and the side gun supplies O2 and N2 gases. Limestone is added to form slag during the deep dephosphorization process to produce ultra-low phosphorus chromium-nickel pig iron melt.

[0009] Further, in the above-mentioned method for rapid deep dephosphorization of chromium-nickel pig iron melt by AOD:

[0010] During the desiliconization and dechromization operation in step 1, the oxygen flow rate of the AOD top gun is controlled to be 1.0-1.4 Nm / ton of steel. 3 / min, the oxygen lance position is controlled at 2300-2500mm, and the total flow rate of O2 and N2 gas supply per ton of steel is controlled at 0.6-0.8Nm 3 / min, the ratio of O2 and N2 is controlled to be O2:N2=3:1; lime is added in batches to make slag, the basicity of desiliconized slag is controlled to be 1.3-1.5, and nickel pig iron is added during desiliconization and dechromization to adjust the temperature of molten steel, and the temperature of molten steel is controlled to be 1350-1450℃;

[0011] In step 2, when Si≤0.03% and Cr≤0.50% in the molten steel, the desiliconization and dechromization operations are stopped, and the AOD deep dephosphorization operation is carried out after removing ≥75% of the desiliconization slag;

[0012] In the AOD deep dephosphorization operation of step 2, the oxygen flow rate of the AOD top gun is controlled to be 1.2-1.5 Nm / ton of steel. 3 / min, the oxygen lance position is controlled at 2000-2300mm, and the total flow rate of O2 and N2 gas supply per ton of steel is controlled at 0.8-1.0Nm 3 / min, the ratio of O2 and N2 is controlled to be O2:N2=1:6; limestone is added in batches from a high position to make slag, the basicity of the dephosphorization slag is controlled to be 5-8, the CO2 generated by the decomposition of limestone strengthens the stirring of the molten steel and decomposes and absorbs heat to control the temperature of the molten steel, and the temperature of the molten steel is controlled at 1500-1550℃;

[0013] In step 2, when P in the molten steel is less than or equal to 0.001%, the AOD deep dephosphorization operation is terminated, the top gun stops blowing oxygen, and the side guns all spray N2 gas for strong stirring. The N2 gas flow rate per ton of steel is controlled to be 1.1-1.3Nm 3 / min, stir for 3 to 5 minutes, and remove ≥85% of the dephosphorized slag.

[0014] Further, in the above-mentioned method for rapid deep dephosphorization of chromium-nickel pig iron melt by AOD, during the desiliconization and dechromization operation in step 1, the total oxygen blowing amount of the AOD top gun oxygen supply and the side gun blowing of O2 and N2 gases is controlled as follows: total oxygen blowing amount in the desiliconization and dechromization process = [weight of chromium-nickel pig iron melt × (Si%-0.03%) × 0.8 + weight of chromium-nickel pig iron melt × (Cr%-0.50%) × 0.323] / oxygen utilization rate % × 1000, wherein the unit of the total oxygen blowing amount in the desiliconization and dechromization process is Nm 3 The unit of weight of chromium-nickel pig iron melt is ton, and the oxygen utilization rate is 85%.

[0015] Furthermore, in the above-mentioned method for rapid deep dephosphorization of chromium-nickel pig iron melt by AOD, during the desiliconization and dechromization operation of step 1, the total amount of lime added in batches for slagging is controlled as follows: total amount of lime added = [weight of chromium-nickel pig iron melt × (Si% in furnace - 0.03%)] × 2.14 × 1.4 / CaO percentage content in lime, wherein the unit of the total amount of lime added is ton, the unit of the weight of the chromium-nickel pig iron melt is ton, and the CaO percentage content in the lime is 86%.

[0016] Furthermore, in the above-mentioned method for rapid deep dephosphorization of chromium-nickel pig iron melt by AOD, in the AOD deep dephosphorization operation of step 2, the total amount of limestone added in batches from a high position for slagging is controlled to be 80-90 kg per ton of steel.

[0017] Furthermore, in the above-mentioned method for rapid deep dephosphorization of chromium-nickel pig iron melt by AOD, in the AOD deep dephosphorization operation of step 2, the dephosphorization slag is a FeO-CaO-SiO2-MgO slag system, and its composition is controlled as follows: FeO: 20-25%, CaO: 45-55%, SiO2: 6-8%, MgO: 6-9%.

[0018] Furthermore, in the above-mentioned method for rapid deep dephosphorization of chromium-nickel pig iron melt by AOD, during the desiliconization and dechromization operation in step 1, the oxygen pressure of the AOD top gun oxygen supply is controlled to be 1.0 MPa.

[0019] Furthermore, in the above-mentioned method for rapid deep dephosphorization of chromium-nickel pig iron melt by AOD, in step 1, the chromium-nickel pig iron melt is a chromium-nickel pig iron melt produced by RKEF process.

[0020] Furthermore, in the above-mentioned method for rapid deep dephosphorization of chromium-nickel pig iron melt by AOD, in step 1, the composition of the chromium-nickel pig iron melt is: C≤3.0%, Si: 0.5~2.5%, Cr≤3.5%, P≤0.060%, Ni: 6~18%, and the rest is iron and residual elements.

[0021] The method for AOD deep dephosphorization of chromium-nickel pig iron melt of the present invention has the following advantages and beneficial effects: the present invention solves the technical problem of the difficulty of AOD deep dephosphorization, realizes the purpose of using cheap chromium-nickel pig iron as the main raw material to prepare ultra-low phosphorus chromium-nickel pig iron melt through AOD rapid deep dephosphorization, and using the ultra-low phosphorus chromium-nickel pig iron melt as stainless steel mother liquor to produce low-phosphorus special stainless steel varieties, simplifies the production process, reduces the smelting cost, develops a short-process green and low-cost smelting low-phosphorus special stainless steel process method, and has good promotion value and economic benefits. DETAILED DESCRIPTION

[0022] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the specific embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0023] The present invention aims to solve the technical problem of the difficulty of AOD deep dephosphorization, and develops a method for rapid deep dephosphorization of chromium-nickel pig iron melt by AOD. The specific process is: the chromium-nickel pig iron melt is added into an AOD furnace, and desiliconization and dechromization operations are first performed, wherein the AOD top gun supplies oxygen, the side gun sprays O2 and N2 gases, and lime is added in batches to make slag; after the desiliconization and dechromization are completed, the slag is removed for deep dephosphorization, the AOD top gun supplies oxygen, the side gun supplies O2 and N2 gases, limestone is added in the process to make slag, and high-basicity slag is made for deep dephosphorization, so as to quickly produce ultra-low phosphorus stainless steel mother liquor.

[0024] Specifically, the method for rapid deep dephosphorization of chromium-nickel pig iron melt by AOD of the present invention comprises the following steps:

[0025] (1) A chromium-nickel pig iron melt is added into an AOD furnace, wherein the composition of the chromium-nickel pig iron melt is: C≤3.0%, Si: 0.5-2.5%, Cr≤3.5%, P≤0.060%, Ni: 6-18%, and the rest is iron and residual elements, wherein the chromium-nickel pig iron melt can be, for example, a chromium-nickel pig iron melt produced by a RKEF process.

[0026] (2) Desiliconization and dechroming operations are performed in the AOD. The AOD top gun supplies oxygen, the oxygen pressure is controlled at 1.0 MPa, and the oxygen flow rate per ton of steel is controlled at 1.0-1.4 Nm 3 / min, the oxygen lance position is controlled at 2300-2500mm, the side lance sprays O2 and N2 gases, and the total flow rate of O2 and N2 gas supply per ton of steel is controlled at 0.6-0.8Nm 3 / min, the ratio of O2 and N2 is controlled as O2:N2=3:1, and the total oxygen blowing amount in the desiliconization and dechromization process is controlled as follows: the total oxygen blowing amount in the desiliconization and dechromization process = [the weight of the chromium-nickel pig iron melt × (Si%-0.03%) × 0.8 + the weight of the chromium-nickel pig iron melt × (Cr%-0.50%) × 0.323] / oxygen utilization rate % × 1000, wherein the unit of the total oxygen blowing amount in the desiliconization and dechromization process is Nm 3 The unit of the weight of the chromium-nickel pig iron melt is ton, and the oxygen utilization rate is 85%; lime is added in batches to make slag, and the total amount of lime added is controlled as follows: total amount of lime added = [weight of the chromium-nickel pig iron melt × (Si% into the furnace - 0.03%)] × 2.14 × 1.4 / percentage content of CaO in the lime, wherein the unit of the total amount of lime added is ton, the unit of the weight of the chromium-nickel pig iron melt is ton, and the percentage content of CaO in the lime is 86%. By adding lime in batches to make slag, the basicity of the desiliconized slag is controlled to 1.3-1.5, and nickel pig iron is added in the process to adjust the temperature of the molten steel, and the temperature of the molten steel is controlled to 1350-1450°C.

[0027] (3) When Si≤0.03% and Cr≤0.50% in the molten steel, stop desiliconization and dechromization, and carry out AOD slag removal operation to remove most of the desiliconization slag, and the proportion of slag removal to the total slag volume is ≥75%.

[0028] (4) After AOD slagging is completed, AOD deep dephosphorization operation is carried out, in which AOD top gun supplies oxygen, and the oxygen flow rate per ton of steel is controlled to be 1.2-1.5Nm 3 / min, the oxygen lance position is controlled at 2000-2300mm, the side lance sprays O2 and N2 gases, and the total flow rate of O2 and N2 gas supply per ton of steel is controlled at 0.8-1.0Nm 3 / min, the ratio of O2 and N2 is controlled to be O2:N2=1:6, limestone (CaCO3) is added in batches from a high position during the dephosphorization process, the total amount of limestone added is controlled to be 80-90kg per ton of steel, and deep dephosphorization is carried out on dephosphorization slag with an alkalinity of 5-8. The dephosphorization slag is a FeO-CaO-SiO2-MgO slag system, and its composition is controlled to be: FeO: 20-25%, CaO: 45-55%, SiO2: 6-8%, MgO: 6-9%. Limestone decomposes to produce CO2 (CaCO3=CaO+CO2↑) to enhance the stirring of the molten steel, and at the same time decomposes and absorbs heat to control the temperature of the molten steel, and the temperature of the molten steel is controlled at 1500-1550℃.

[0029] (5) When P in molten steel is less than or equal to 0.001%, dephosphorization is terminated, oxygen blowing from the top gun stops, and N2 gas is sprayed from all side guns for strong stirring to promote uniform temperature and composition of molten steel. The N2 gas flow rate is controlled at 1.1-1.3 Nm / ton of steel. 3 / min, stir for 3-5min, remove most of the dephosphorization slag, the slag removal amount accounts for ≥85% of the total slag, and produce ultra-low phosphorus stainless steel mother liquor, which can be used for refining low-phosphorus special stainless steel in AOD furnace later.

[0030] The method for rapid deep dephosphorization of chromium-nickel pig iron melt by AOD of the present invention is described in detail below in conjunction with the specific embodiments of the present invention.

[0031] Example 1

[0032] Example 1 of the present invention is used to use a 180-ton AOD furnace to perform AOD rapid deep dephosphorization of chromium-nickel pig iron melt to produce ultra-low phosphorus stainless steel mother liquor. The specific implementation process is as follows:

[0033] (1) The chromium-nickel pig iron melt is added into the AOD furnace. The composition of the chromium-nickel pig iron melt is: C: 2.5%, Si: 1.5%, Cr: 3.0%, P: 0.050%, Ni: 12%, and the rest is iron and residual elements.

[0034] (2) Desiliconization and dechroming operations are performed in the AOD, wherein the AOD top gun supplies oxygen with an oxygen pressure of 1.0 MPa and an oxygen flow rate of 240 Nm 3 / min, the oxygen lance position is 2500mm, the side lance sprays O2 and N2 gases, and the total flow rate of O2 and N2 gas supply is 126Nm 3 / min, the ratio of O2 and N2 is O2: N2 = 3:1, and the total oxygen blowing amount in the desiliconization and dechromization process is controlled as follows: Total oxygen blowing amount = [180 × (1.5% - 0.03%) × 0.8 + 180 × (3.0% - 0.50%) × 0.323] / 85% × 1000 = 4200 Nm 3 , add lime in batches to make slag, the total amount of lime added is controlled as follows: total amount of lime added = [180×(1.5%-0.03%)]×2.14×1.4 / 86%=9.2 tons, the basicity of the desiliconized slag is controlled to 1.4, nickel pig iron is added during the smelting process to adjust the temperature of the molten steel, and the temperature of the molten steel is controlled at 1400-1450°C.

[0035] (3) When Si≤0.03% and Cr≤0.50% in the molten steel, stop desiliconization and dechromization, and carry out AOD slag removal operation to remove 75% of the desiliconization slag.

[0036] (4) After the AOD slagging is completed, oxygen is blown to carry out the AOD deep dephosphorization operation. The oxygen flow rate of the AOD top gun is 250Nm 3 / min, the oxygen lance position is 2100mm, the side lance sprays O2 and N2 gases, and the total flow rate of O2 and N2 gas supply is 180Nm 3 / min, the ratio of O2 and N2 is O2:N2=1:6. During the dephosphorization process, limestone is added in batches from a high position. The limestone decomposes to produce CO2, thereby enhancing the stirring of the molten steel. At the same time, it decomposes and absorbs heat to control the temperature of the molten steel. The temperature of the molten steel is controlled at 1500-1550℃. The total amount of limestone added is 15 tons. Dephosphorization slag with an alkalinity of 7 is made for deep dephosphorization. The dephosphorization slag is a FeO-CaO-SiO2-MgO slag system, and its composition is: FeO: 25%, CaO: 50%, SiO2: 7%, MgO: 9%.

[0037] (5) When P in the molten steel is less than or equal to 0.001%, dephosphorization is terminated, the top gun stops blowing oxygen, and the side guns all spray N2 gas for strong stirring to promote uniform temperature and composition of the molten steel. The N2 gas flow rate is 215Nm 3 / min, stir for 5min, remove 85% of the dephosphorization slag, and produce ultra-low phosphorus stainless steel mother liquor.

[0038] By using Example 1, 182 tons of ultra-low phosphorus chromium-nickel pig iron melt was finally prepared, and the steel composition was: C: 1.8%, Si: 0.01%, P: 0.001%, Ni: 13%, Cr: 0.06%. The ultra-low phosphorus chromium-nickel pig iron melt can be directly used as a stainless steel mother liquor to continue refining low-phosphorus special stainless steel in an AOD furnace.

[0039] Example 2

[0040] Example 2 of the present invention is used to use a 90-ton AOD furnace to perform AOD rapid deep dephosphorization of chromium-nickel pig iron melt to produce ultra-low phosphorus stainless steel mother liquor. The specific implementation process is as follows:

[0041] (1) The chromium-nickel pig iron melt is added into the AOD furnace. The composition of the chromium-nickel pig iron melt is: C: 2.0%, Si: 1.0%, Cr: 2.5%, P: 0.045%, Ni: 17%, and the rest is iron and residual elements.

[0042] (2) Desiliconization and dechroming operations are performed in the AOD, wherein the AOD top gun supplies oxygen with an oxygen pressure of 1.0 MPa and an oxygen flow rate of 120 Nm 3 / min, the oxygen lance position is 2300mm, the side lance sprays O2 and N2 gases, and the total flow rate of O2 and N2 gas supply is 66Nm 3 / min, the ratio of O2 and N2 is O2:N2=3:1, and the total oxygen blowing amount in the desiliconization and dechromization process is controlled as follows: Total oxygen blowing amount=[90×(1.0%-0.03%)×0.8+90×(2.5%-0.50%)×0.323] / 85%×1000=1506Nm 3, add lime in batches to make slag, the total amount of lime added is controlled as follows: total amount of lime added = [90 × (1.0% - 0.03%)] × 2.14 × 1.4 / 86% = 3 tons, the basicity of the desiliconized slag is controlled to 1.5, nickel pig iron is added during the smelting process to adjust the temperature of the molten steel, and the temperature of the molten steel is controlled at 1420 ~ 1450 ° C.

[0043] (3) When Si≤0.03% and Cr≤0.50% in the molten steel, stop desiliconization and dechromization, and carry out AOD slag removal operation to remove 75% of the desiliconization slag.

[0044] (4) After the AOD slagging is completed, oxygen is blown to carry out the AOD deep dephosphorization operation. The oxygen flow rate of the AOD top gun is 130Nm 3 / min, the oxygen lance position is 2200mm, the side lance sprays O2 and N2 gases, and the total flow rate of O2 and N2 gas supply is 90Nm 3 / min, the ratio of O2 and N2 is O2:N2=1:6. During the dephosphorization process, limestone is added in batches from a high position. The limestone decomposes to produce CO2, thereby enhancing the stirring of the molten steel. At the same time, it decomposes and absorbs heat to control the temperature of the molten steel. The temperature of the molten steel is controlled at 1530-1550℃. The total amount of limestone added is 7.2 tons. Dephosphorization slag with alkalinity of 6 is made for deep dephosphorization. The dephosphorization slag is FeO-CaO-SiO2-MgO slag system, and its composition is: FeO: 22%, CaO: 49%, SiO2: 7.5%, MgO: 8.5%.

[0045] (5) When P in the molten steel is less than or equal to 0.001%, dephosphorization is terminated, the top gun stops blowing oxygen, and the side guns all spray N2 gas for strong stirring to promote uniform temperature and composition of the molten steel. The N2 gas flow rate is 105Nm 3 / min, stirring for 4min, removing 85% of the dephosphorization slag to produce ultra-low phosphorus stainless steel mother liquor.

[0046] By using Example 2, 89 tons of ultra-low phosphorus chromium-nickel pig iron melt was finally prepared, and the steel composition was: C: 1.0%, Si: 0.01%, P: 0.001%, Ni: 17%, Cr: 0.08%. The ultra-low phosphorus chromium-nickel pig iron melt can be directly used as a stainless steel mother liquor to continue refining low-phosphorus special stainless steel in an AOD furnace.

[0047] In summary, the method for rapid deep dephosphorization of chromium-nickel pig iron melt by AOD takes chromium-nickel pig iron melt as raw material, and rapidly produces ultra-low phosphorus chromium-nickel pig iron melt by desiliconization and dechromization in AOD and then deep dephosphorization by AOD. The ultra-low phosphorus chromium-nickel pig iron melt has an AOD endpoint phosphorus content of P≤0.001%, and can be directly used as stainless steel mother liquor to continue refining low-phosphorus special stainless steel in an AOD furnace.

[0048] Compared with the prior art, the method for AOD rapid deep dephosphorization of chromium-nickel pig iron melt of the present invention has the following advantages and beneficial effects: the present invention solves the technical problem of the difficulty of AOD deep dephosphorization, realizes the purpose of using cheap chromium-nickel pig iron as the main raw material to prepare ultra-low phosphorus chromium-nickel pig iron melt through AOD rapid deep dephosphorization, and using the ultra-low phosphorus chromium-nickel pig iron melt as stainless steel mother liquor to produce low-phosphorus special stainless steel varieties, simplifies the production process, reduces the smelting cost, develops a short-process green and low-cost smelting process method for low-phosphorus special stainless steel, and has good promotion value and economic benefits.

[0049] It should be noted that, in this article, the term "comprise" or any other variation thereof is intended to cover non-exclusive inclusion, so that an article or device including a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such article or device.

[0050] It should also be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the present invention.

Claims

1. A method for rapid deep dephosphorization of chromium-nickel pig iron melt by AOD, characterized in that: The steps include: Step 1: The chromium-nickel pig iron melt is added into the AOD furnace for desiliconization and dechromization operations, wherein the AOD top gun supplies oxygen, the side guns spray O2 and N2 gases, and lime is added in batches to make slag; Step 2: After desiliconization and dechromization, the slag is removed and AOD deep dephosphorization operation is carried out. The AOD top gun supplies oxygen, and the side gun supplies O2 and N2 gases. Limestone is added to form slag during the deep dephosphorization process to produce ultra-low phosphorus chromium-nickel pig iron melt.

2. The method for rapid deep dephosphorization of chromium-nickel pig iron melt by AOD as claimed in claim 1, characterized in that: During the desiliconization and dechromization operation in step 1, the oxygen flow rate of the AOD top gun is controlled to be 1.0-1.4 Nm / ton of steel. 3 / min, the oxygen lance position is controlled at 2300-2500mm, and the total flow rate of O2 and N2 gas supply per ton of steel is controlled at 0.6-0.8Nm 3 / min, the ratio of O2 and N2 is controlled to be O2:N2=3:1; lime is added in batches to make slag, the basicity of desiliconized slag is controlled to be 1.3-1.5, and nickel pig iron is added during desiliconization and dechromization to adjust the temperature of molten steel, and the temperature of molten steel is controlled to be 1350-1450℃; In step 2, when Si≤0.03% and Cr≤0.50% in the molten steel, the desiliconization and dechromization operations are stopped, and the AOD deep dephosphorization operation is carried out after removing ≥75% of the desiliconization slag; In the AOD deep dephosphorization operation of step 2, the oxygen flow rate of the AOD top gun is controlled to be 1.2-1.5 Nm / ton of steel. 3 / min, the oxygen lance position is controlled at 2000-2300mm, and the total flow rate of O2 and N2 gas supply per ton of steel is controlled at 0.8-1.0Nm 3 / min, the ratio of O2 and N2 is controlled to be O2:N2=1:6; limestone is added in batches from a high position to make slag, the basicity of the dephosphorization slag is controlled to be 5-8, the CO2 generated by the decomposition of limestone strengthens the stirring of the molten steel and decomposes and absorbs heat to control the temperature of the molten steel, and the temperature of the molten steel is controlled at 1500-1550℃; In step 2, when P in the molten steel is less than or equal to 0.001%, the AOD deep dephosphorization operation is terminated, the top gun stops blowing oxygen, and the side guns all spray N2 gas for strong stirring. The N2 gas flow rate per ton of steel is controlled to be 1.1-1.3Nm 3 / min, stir for 3 to 5 minutes, and remove ≥85% of the dephosphorized slag.

3. The method for rapid deep dephosphorization of chromium-nickel pig iron melt by AOD as claimed in claim 2, characterized in that: During the desiliconization and dechromization operation of step 1, the total oxygen blowing amount of the AOD top gun oxygen supply and the side gun blowing of O2 and N2 gases is controlled as follows: the total oxygen blowing amount during the desiliconization and dechromization process = [the weight of the chromium-nickel pig iron melt × (Si%-0.03%) × 0.8 + the weight of the chromium-nickel pig iron melt × (Cr%-0.50%) × 0.323] / oxygen utilization rate % × 1000, wherein the unit of the total oxygen blowing amount during the desiliconization and dechromization process is Nm 3 The unit of weight of chromium-nickel pig iron melt is ton, and the oxygen utilization rate is 85%.

4. The method for rapid deep dephosphorization of chromium-nickel pig iron melt by AOD as claimed in claim 2, characterized in that: During the desiliconization and dechromization operation of step 1, the total amount of lime added in batches for slagging is controlled as follows: total amount of lime added = [weight of chromium-nickel pig iron melt × (Si% entering the furnace - 0.03%)] × 2.14 × 1.4 / percentage of CaO in lime, wherein the unit of the total amount of lime added is ton, the unit of the weight of the chromium-nickel pig iron melt is ton, and the percentage of CaO in the lime is 86%.

5. The method for rapid deep dephosphorization of chromium-nickel pig iron melt by AOD as claimed in claim 2, characterized in that: In the AOD deep dephosphorization operation of step 2, the total amount of limestone added in batches from a high position for slagging is controlled to be 80-90 kg per ton of steel.

6. The method for rapid deep dephosphorization of chromium-nickel pig iron melt by AOD as claimed in claim 2, characterized in that: In the AOD deep dephosphorization operation of step 2, the dephosphorization slag is a FeO-CaO-SiO2-MgO slag system, and its composition is controlled as follows: FeO: 20-25%, CaO: 45-55%, SiO2: 6-8%, MgO: 6-9%.

7. The method for rapid deep dephosphorization of chromium-nickel pig iron melt by AOD as claimed in claim 2, characterized in that: During the desiliconization and dechromization operation in step 1, the oxygen pressure supplied by the AOD top gun is controlled to be 1.0 MPa.

8. The method for rapid deep dephosphorization of chromium-nickel pig iron melt by AOD according to claim 1 or 2, characterized in that: In step 1, the chromium-nickel pig iron melt is a chromium-nickel pig iron melt produced by the RKEF process.

9. The method for rapid deep dephosphorization of chromium-nickel pig iron melt by AOD according to claim 1 or 2, characterized in that: In step 1, the composition of the chromium-nickel pig iron melt is: C≤3.0%, Si: 0.5-2.5%, Cr≤3.5%, P≤0.060%, Ni: 6-18%, and the rest is iron and residual elements.

Citation Information

Patent Citations

  • Dephosphorization method of high-phosphorous chromium-nickel pig iron

    CN102312033A

  • Method for smelting stainless steel by using ultrahigh silicon-carbon-chromium melt

    CN110894565A

  • Smelting method of 310S heat-resistant stainless steel

    CN116926408A

  • Process method for smelting duplex stainless steel at low cost

    CN117344086A

  • Method for smelting low-phosphorus stainless steel by adopting electric furnace deep dephosphorization process