Metal nickel strip preparation process capable of eliminating surface wave and wrinkle defects

Through electron beam smelting and precision cold rolling technology, the surface wave and wrinkle defects of nickel strips in the new energy battery field are solved, the quality and performance of nickel strips are improved, and high purity and stability are achieved.

CN119061277APending Publication Date: 2024-12-03JIANGSU YUANHANG PRECISION ALLOY TECH +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411100258.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

In the field of new energy batteries, there are surface waves and wrinkle defects in the preparation of pure metal nickel strips, which affects the quality of the material and the performance of the final product.

Method used

The electron beam smelting process is used to prepare high-purity metal nickel ingot billets, and combined with precision cold rolling technology, through multi-pass rolling and annealing treatment, the deformation amount is controlled and the surface defects are removed, and the surface waves and wrinkles are gradually eliminated.

Benefits of technology

It significantly improves the surface quality of metal nickel strips, improves material purity and performance stability, reduces internal stress, and enhances the service life of the product.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a metal nickel strip preparation process capable of eliminating surface wave and wrinkle defects. The method comprises the steps of burdening, charging, electron beam smelting, forging forming, machining, hot rolling and cold rolling. Compared with a traditional preparation process, the pure metal nickel is smelted through the electron beam, the metal purity is further improved, the problems of surface waves, folding and the like of the strip are solved, and the material quality is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of new energy battery preparation, in particular to high-quality pure nickel metal strip preparation technology, and specifically relates to a processing method for eliminating surface wave and wrinkle defects and improving the surface quality of metal nickel strip materials. Background Art

[0002] Pure nickel metal has the characteristics of corrosion resistance, good plasticity, excellent thermal and electrical conductivity, and is widely used in aerospace, electronics, new energy batteries and other fields. In recent years, the application of pure nickel strips has continued to expand and the demand has continued to increase. However, due to the gap in preparation technology level compared with foreign countries, some high-end nickel strips still need to be imported. Therefore, it is of great economic and social benefit to improve the quality level of pure nickel strip foil in my country as soon as possible and replace imported materials.

[0003] The usual preparation process of metal nickel strip is vacuum induction melting, ingot casting, forging, hot rolling, cold rolling, annealing, pickling, etc. Due to the presence of solidification shrinkage holes, harmful inclusion elements, and non-metallic inclusions inside the metal nickel ingot during casting, the subsequent pure nickel strip has a high inclusion content, large performance fluctuations, and difficult to control the plate quality, which affects the performance of the product. Electron beam melting is a vacuum melting process that converts the kinetic energy of high-speed electron flow into thermal energy under high vacuum and uses it as a heat source for melting. It has the characteristics of high melting temperature, adjustable melting power and heating speed, and high product purity. High-purity metal nickel ingots can be prepared by electron beam melting, and pure metal nickel ingots with high purity and a certain oriented structure can be prepared.

[0004] In addition to the purity requirements, new energy batteries and other fields have increasingly higher requirements for the surface and internal quality of nickel strips and foils. On the one hand, from the perspective of use, the surface of the strips and foils is required to be flat, without defects such as wavy curvature, scarring, tearing, cracks, inclusions and folding and pressing. The above defects will not only damage the quality of the strips, but also often reduce the performance of the final product; on the other hand, the internal quality of the nickel strips is high. The quality of the internal metallurgical quality of the nickel strip has a great impact on the performance and service life of the products and components. The internal quality of the metal nickel strip is closely related to the smelting method, rolling forming, heat treatment, etc. The important process measure for quality control of the internal defects of the nickel strip is ultrasonic testing. Ultrasonic testing can detect both surface defects of materials or components and internal defects, especially for planar defects such as cracks and delamination of metal plates and strips. It has strong reliability and detection capabilities. The unstable rolling force of the rolling mill, the asymmetric wear of the working rolls, and the deformation of the hot-rolled plates all affect the surface waves and wrinkles of the nickel strips, so the rolling process also needs to be further optimized. Summary of the invention

[0005] The purpose of the present invention is to solve the problems of surface wave and wrinkle defects existing in the preparation of high-purity metal nickel strips used in the field of new energy batteries. The present invention proposes a metal nickel strip preparation process for eliminating surface wave and wrinkle defects, thereby improving the surface quality of pure metal nickel strips and effectively eliminating surface wave and wrinkle defects.

[0006] The technical solution of the present invention is:

[0007] A process for preparing a metal nickel strip for eliminating surface wave and wrinkle defects, the method comprising the following steps:

[0008] (1) Ingredients: Ingredients are prepared according to the ingredients of the metal nickel strip product;

[0009] (2) Charging the furnace: placing a nickel block into the crucible of an electron beam melting furnace, and placing a nickel-boron Ni-B master alloy and carbon C into the charging chamber;

[0010] (3) Electron beam melting: evacuate the electron beam melting furnace; turn on the power and open the electron gun for melting, and use the electron beam to bombard the metal nickel in the crucible; after the metal nickel is cleared, add the nickel-boron Ni-B master alloy and carbon through the charging chamber, and continue to melt until the added master alloy and carbon are completely melted and uniform; turn off the electron gun, turn off the vacuum system after cooling, open the furnace door, and take out the metal nickel ingot;

[0011] (4) Forging: Place the nickel ingot into a heating furnace, keep it warm after reaching the set temperature, and then forge it out of the furnace to form a nickel flat ingot;

[0012] (5) Machining: Removing holes, cracks and impurities on the surface of the nickel flat ingot by machining;

[0013] (6) Hot rolling: hot rolling the flat nickel ingot after surface machining using a hot rolling mill to obtain a nickel plate, annealing to relieve stress, cooling to room temperature, and grinding the plate surface to remove oxide scale;

[0014] (7) Cold rolling: The metal nickel sheet is rolled to a preset deformation amount in multiple passes using a cold rolling mill, and then annealed to reduce internal stress to obtain a finished nickel strip.

[0015] Furthermore, in the step (1), the ingredients are prepared according to the composition of the metal nickel strip product; wherein the main element content is prepared according to the midline configured corresponding to the finished product content range; the element boron B is added according to 1.1 to 1.15 times the upper limit, and is added in the form of a nickel-boron Ni-B master alloy.

[0016] Furthermore, the ingredients in step (1) are specifically as follows: the components of the metal nickel strip are Ni: 99.6; C: 0.1; Mn: 0.15-0.16; Mg: 0.05-0.06; Fe: 0.08-0.09; B: 0.01-0.02; the B element is added in the form of a nickel-boron Ni-B master alloy.

[0017] Furthermore, in the step (3), the vacuum degree of the electron beam melting furnace is lower than 0.05Pa, and the vacuum degree of the electron gun chamber is less than 0.003Pa.

[0018] Furthermore, in the step (3), when the electron beam bombards the metal nickel in the water-cooled copper crucible, the electron gun beam current energy is 500mA to 2000mA, and the metal nickel smelting time is 20min to 30min;

[0019] Furthermore, in the step (3), the smelting time is continued for 10 minutes to 15 minutes.

[0020] Furthermore, in the step (3), the cooling time is 10 min to 15 min.

[0021] Furthermore, in the step (4), the set temperature of the heating furnace is 1000° C. to 1050° C., and the insulation time is 1 h to 2 h.

[0022] Furthermore, in the step (6), the thickness of the metal nickel plate obtained after hot rolling is 3 mm to 8 mm.

[0023] Furthermore, in the step (7), the deformation amount of each rolling pass is 20% to 30%, and when the deformation amount reaches 70%, annealing is performed to relieve stress.

[0024] Beneficial effects of the present invention:

[0025] The present invention adopts the pure metal nickel electron smelting process. The usual vacuum induction furnace smelts pure metal nickel, mainly using alumina crucibles or magnesia-alumina mixed crucibles, which will cause some harmful elements such as Ca, Mg, O to enter the metal nickel melt. When the content of impurity element O exceeds 70ppm, the cold working performance of the metal nickel strip is sharply reduced. Compared with the traditional preparation process, the present invention adopts electron beam melting of pure metal nickel, which not only further improves the purity of the metal, but also helps to eliminate the problems of strip surface waves, folds, etc., and improves the material quality.

[0026] The present invention adopts the precision cold rolling technology of controlling the deformation amount, and effectively eliminates the preparation defect problems of surface waves and wrinkles of the metal nickel strip by controlling the deformation amount of each rolling pass and the total deformation amount, thereby improving the material yield.

[0027] Other features and advantages of the present invention will be described in detail in the following detailed description. DETAILED DESCRIPTION

[0028] The preferred embodiments of the present invention will be described in more detail below with reference to examples. Although preferred embodiments of the present invention are shown, it should be understood that the present invention can be implemented in various forms and should not be limited to the embodiments set forth herein.

[0029] Embodiment 1:

[0030] The ingredients are as follows: Ni: 99.6; C: 0.1; Mn: 0.16; Mg: 0.05; Fe: 0.08; B: 0.01; B element is added in the form of Ni-B master alloy; the main element metal nickel block is placed in the crucible of the electron beam melting furnace, and the nickel-boron master alloy and carbon C are placed in the charging chamber; the electron beam melting furnace is evacuated to a vacuum degree of 0.02Pa, and the vacuum degree of the electron gun chamber is 0.002Pa; the power is turned on to start the electron gun melting, and the metal nickel plate in the water-cooled copper crucible is bombarded by an electron beam, and the electron gun beam energy is increased to 500mA, and the metal nickel is melted for 20min. After the metal is cleared, the nickel-boron master alloy and the carbon rod are added to the metal molten pool through the charging chamber. The melting is continued for 10min to make the added master alloy and carbon rod completely melted and uniform. Turn off the electron gun, and after the metal nickel ingot cools for 10 minutes, turn off the vacuum system, open the furnace door, and take out the metal nickel ingot; put the nickel ingot into the heating furnace, heat it to 1000℃, keep it warm for 1 hour, take it out of the furnace for forging, and forge the ingot into a flat ingot suitable for hot rolling; remove the holes, cracks and impurities on the surface of the metal nickel flat ingot by machining; use the hot rolling mill to hot roll the metal nickel ingot after surface machining, and the thickness of the plate is 3mm after hot rolling. The plate after hot rolling is annealed to relieve stress. After cooling to room temperature, the surface of the plate is ground to remove the oxide scale; the cold rolling mill is used to roll the metal nickel strip for multiple passes, and the deformation of each rolling pass is 20%. When the deformation reaches 70%, annealing is performed to reduce the internal stress. The metal nickel strip is rolled to the size and thickness required by the product; the surface quality of the metal nickel strip after rolling is inspected, and it is packaged and stored after passing.

[0031] Embodiment 2:

[0032] The ingredients are as follows: Ni: 99.6; C: 0.1; Mn: 0.13; Mg: 0.06; Fe: 0.08; B: 0.02 in weight percentage. The B element is added in the form of a nickel-boron (Ni-B) master alloy; a nickel block of the main element is placed in a crucible of an electron beam melting furnace, and a nickel-boron master alloy and carbon C are placed in a charging chamber; the electron beam melting furnace is evacuated to a vacuum degree of 0.03 Pa, and the vacuum degree of the electron gun chamber is 0.001 Pa; the power is turned on to start the electron gun melting, and an electron beam is used to bombard the metal nickel plate in the water-cooled copper crucible, and the electron gun beam energy is increased to 2000 mA. The metal nickel is melted for 30 minutes. After the metal is cleared, the nickel-boron master alloy and the carbon rod are added to the metal molten pool through the charging chamber. The melting is continued for 15 minutes to make the added master alloy and carbon rod completely melted and uniform. Turn off the electron gun, and after the metal nickel ingot cools for 15 minutes, turn off the vacuum system, open the furnace door, and take out the metal nickel ingot; put the nickel ingot into the heating furnace, heat it to 1050℃, keep it warm for 2 hours, take it out of the furnace for forging, and forge the ingot into a flat ingot suitable for hot rolling; remove the holes, cracks and impurities on the surface of the metal nickel flat ingot by machining; use the hot rolling mill to hot roll the metal nickel ingot after surface machining, and the thickness of the plate is 8mm after hot rolling. The plate after hot rolling is annealed to relieve stress. After cooling to room temperature, the surface of the plate is ground to remove the oxide scale; the cold rolling mill is used to roll the metal nickel strip for multiple passes, and the deformation of each rolling pass is 30%. When the deformation reaches 70%, annealing is performed to reduce the internal stress. The metal nickel strip is rolled to the required size and thickness of the product; the surface quality of the metal nickel strip after rolling is inspected, and it is packaged and stored after passing.

[0033] The product test results of Example 1 and Example 2 compared with the traditional method are shown in Table 1.

[0034] Table 1

[0035] Process Category Nickel metal purity Surface waves Wrinkles Traditional methods 99.6% A small amount exists A small amount exists Example 1 Method Greater than 99.9% none none Example 2 Method Greater than 99.8% none none

[0036] The above traditional method steps are as follows:

[0037] The ingredients are as follows: Ni: 99.6; C: 0.1; Mn: 0.12; Fe: 0.08; B: 0.01. Put the pure nickel metal (purity 999.6%) cut into blocks into the crucible of the vacuum induction melting furnace, evacuate the equipment to about 0.5Pa, and send induction heating until the metal nickel is completely melted. The melting temperature range is controlled to 1450℃, and the insulation time is 20min; put the steel ingot mold into the ingot mold room of the vacuum induction melting furnace, and then evacuate the vacuum to prepare for casting; add trace elements Mn and B into the crucible. After the alloy is smelted, it is cast into the ingot mold, and the cooled ingot is processed by the casting machine.

[0038] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.

Claims

1. A process for preparing a metal nickel strip for eliminating surface wave and wrinkle defects, characterized in that: The method comprises the following steps: (1) Ingredients: Ingredients are prepared according to the ingredients of the metal nickel strip product; (2) Charging the furnace: placing a nickel block into the crucible of an electron beam melting furnace, and placing a nickel-boron Ni-B master alloy and carbon C into the charging chamber; (3) Electron beam melting: evacuate the electron beam melting furnace; turn on the power and open the electron gun for melting, and use the electron beam to bombard the metal nickel in the crucible; after the metal nickel is cleared, add the nickel-boron Ni-B master alloy and carbon through the charging chamber, and continue to melt until the added master alloy and carbon are completely melted and uniform; turn off the electron gun, turn off the vacuum system after cooling, open the furnace door, and take out the metal nickel ingot; (4) Forging: Place the nickel ingot into a heating furnace, keep it warm after reaching the set temperature, and then forge it out of the furnace to form a nickel flat ingot; (5) Machining: Removing holes, cracks and impurities on the surface of the nickel flat ingot by machining; (6) Hot rolling: hot rolling the flat nickel ingot after surface machining using a hot rolling mill to obtain a nickel plate, annealing to relieve stress, cooling to room temperature, and grinding the plate surface to remove oxide scale; (7) Cold rolling: The metal nickel sheet is rolled to a preset deformation amount in multiple passes using a cold rolling mill, and then annealed to reduce internal stress to obtain a finished nickel strip.

2. The process for preparing a metal nickel strip with surface wave and wrinkle defects eliminated according to claim 1, characterized in that In the step (1), the ingredients are prepared according to the composition of the metal nickel strip product; wherein the main element content is prepared according to the midline of the content range of the finished product; the element boron B is added according to 1.1 to 1.15 times the upper limit and is added in the form of a nickel-boron Ni-B master alloy.

3. The process for preparing a metal nickel strip for eliminating surface wave and wrinkle defects according to claim 2, characterized in that The ingredients in step (1) are specifically as follows: the composition of the metal nickel strip is Ni:99.6 in weight percentage; C:0.1; Mn: 0.15-0.16; Mg: 0.05-0.06; Fe: 0.08-0.09; B: 0.01-0.02; the B element is added in the form of a nickel-boron Ni-B master alloy.

4. The process for preparing a metal nickel strip with surface wave and wrinkle defects eliminated according to claim 1, characterized in that In the step (3), the vacuum degree of the electron beam melting furnace is lower than 0.05Pa, and the vacuum degree of the electron gun chamber is less than 0.003Pa.

5. The process for preparing a metal nickel strip with surface wave and wrinkle defects eliminated according to claim 1, characterized in that In the step (3), when the electron beam bombards the metal nickel in the water-cooled copper crucible, the electron gun beam current energy is 500mA to 2000mA, and the metal nickel smelting time is 20min to 30min.

6. The process for preparing a metal nickel strip with surface wave and wrinkle defects eliminated according to claim 1, characterized in that In the step (3), the smelting time is continued for 10 minutes to 15 minutes.

7. The process for preparing a metal nickel strip with surface wave and wrinkle defects eliminated according to claim 1, characterized in that In the step (3), the cooling time is 10 min to 15 min.

8. The process for preparing a metal nickel strip with surface wave and wrinkle defects eliminated according to claim 1, characterized in that In the step (4), the setting temperature of the heating furnace is 1000°C to 1050°C, and the insulation time is 1h to 2h.

9. The process for preparing a metal nickel strip with surface wave and wrinkle defects eliminated according to claim 1, characterized in that In the step (6), the thickness of the metal nickel plate obtained after hot rolling is 3 mm to 8 mm.

10. The process for preparing a metal nickel strip with surface wave and wrinkle defects eliminated according to claim 1, characterized in that In the step (7), the deformation amount of each rolling process is 20% to 30%. When the deformation amount reaches 70%, annealing is performed to relieve stress.

Citation Information

Cited By

  • Continuous casting and continuous forging method for smelting metal by using electron beam cold bed furnace

    CN119662992A