High-temperature molten salt corrosion resistant alloy for photo-thermal power generation equipment and manufacturing method of high-temperature molten salt corrosion resistant alloy

By using specific components of high-temperature molten salt corrosion alloys in photothermal power generation equipment, combined with vacuum induction smelting, electroslag remelting and forging processes, the problem of insufficient performance of existing materials at 800℃ is solved, and the high temperature of the alloy is achieved The performance improvement and corrosion resistance improve the safety and reliability requirements of photothermal power generation equipment.

CN119061292APending Publication Date: 2024-12-03ZHENSHI GROUP EASTERN SPECIAL STEEL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411158470.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing photothermal power generation equipment materials cannot meet the design requirements of complex devices at high temperatures of 800℃, and are not resistant to high-temperature chloride corrosion, resulting in heat traces, stress corrosion and cracking. The existing manufacturing methods are not suitable for photothermal power generation equipment. Corrosion of alloys with high temperature resistant molten salts.

Method used

Using specific components of high-temperature molten salt corrosion alloys, including 6.0-8.0% Cr, 3.0-5.0% Fe, 0.04-0.08% C, etc., through vacuum induction smelting, electroslag remelting, multiple forging and fire rolling The manufacturing process produces alloys with excellent mechanical properties.

Benefits of technology

It has achieved the improvement of the high-temperature performance and mechanical processing performance of alloys at 800℃, meets the safety and reliability requirements of photothermal power generation equipment, and provides a more resistant solution to high-temperature molten salt corrosion.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to a high-temperature molten salt corrosion resistant alloy for photo-thermal power generation equipment and a manufacturing method of the high-temperature molten salt corrosion resistant alloy, and belongs to the field of high-temperature molten salt corrosion resistant alloys. The high-temperature molten salt corrosion resistant alloy for the photo-thermal power generation equipment comprises the following components in percentage by mass (%): 6.0-8.0% of Cr, 3.0-5.0% of Fe, 0.04-0.08% of C, less than or equal to 0.20% of Co, less than or equal to 1.0% of Mn, less than or equal to 1.0% of Si, 1.0-2.0% of W, 15.0-18.0% of Mo, less than or equal to 0.015% of P, less than or equal to 0.020% of S, less than or equal to 0.50% of Ti + Al, less than or equal to 0.010% of B and the balance of Ni and inevitable impurities. The invention further provides a manufacturing method of the high-temperature molten salt corrosion resistant alloy for the photo-thermal power generation equipment. The high-temperature molten salt corrosion resistant alloy for the photo-thermal power generation equipment has good machining performance and excellent mechanical performance in a solid solution state, has high high-temperature performance at the temperature of 800 DEG C, and meets use requirements.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an alloy and a manufacturing method thereof, in particular to a high-temperature molten salt corrosion resistant alloy for photothermal power generation equipment and a manufacturing method thereof, and belongs to the field of high-temperature molten salt corrosion resistant alloys. Background Art

[0002] The current mainstream solar thermal technology - the second generation of solar thermal power generation technology uses nitrate as a heat transfer and storage medium, and has a relatively low operating temperature (560°C); compared with other types of power stations, the power generation cost and grid-connected electricity price are relatively high. The next generation of solar thermal collection technology (represented by high-temperature chloride molten salt, high-temperature molten salt corrosion alloy, and high-efficiency supercritical carbon dioxide power generation) can increase the operating temperature of solar thermal power generation devices to 700°C-800°C, which is expected to significantly improve power generation efficiency; on the other hand, 800°C high-grade heat can significantly improve hydrogen production efficiency and achieve low-cost solar-hydrogen energy conversion.

[0003] The high-temperature and corrosion-resistant materials used for tank pipes in the current nitrate solar thermal power generation devices in service and under construction are mainly 304H, 316H, and 347H stainless steels, and the heat-absorbing gas pipes are mainly 347H stainless steel, Inconel 625 alloy, and Haynes230 alloy. Although it has been successfully applied in the project, there are still cases of improper thermal traces leading to local overheating and damage or stress corrosion cracking. If these materials are applied to future 800℃ solar thermal power generation devices, there is no engineering experience to rely on. On the other hand, although some standards allow these materials to serve at high temperatures of around 800℃, their allowable stress is very low and can hardly meet the design requirements of complex devices.

[0004] In addition, stainless steel cannot withstand high-temperature chloride corrosion at 800°C and is difficult to meet engineering requirements. All other mature high-strength heat-resistant engineering materials with a maximum allowable temperature above 800°C (Incoloy 800H, Haynes 230, Hastelloy X, Inconel 617, Inconel 625, etc.) are not developed for molten salt conditions and cannot meet the requirements for resistance to high-temperature molten chloride salt corrosion.

[0005] A Chinese patent with a publication date of April 5, 2024 and a publication number of CN117821834A discloses an invention patent entitled "A method for manufacturing a superalloy for nuclear power plant fasteners". The patent includes raw material preparation; vacuum induction VIM smelting; vacuum consumable smelting; forging; ultrasonic flaw detection; rolling; solution heat treatment; pickling. The superalloy produced by this patent is more resistant to molten salt corrosion, more resistant to intergranular corrosion, has better radiation resistance, is more resistant to high temperature and high pressure, and has a longer service life. It can fully meet the use requirements of fourth-generation nuclear power plant fasteners, but the above-mentioned manufacturing method is not suitable for high-temperature molten salt corrosion-resistant alloys for solar thermal power generation equipment in this application.

[0006] Therefore, providing a high-temperature molten salt corrosion-resistant alloy for solar thermal power generation equipment has positive significance for improving the safety and reliability of solar thermal power generation. Summary of the invention

[0007] The purpose of the present invention is to overcome the above-mentioned deficiencies in the prior art and to provide a high-temperature molten salt corrosion-resistant alloy for a photothermal power generation device having better comprehensive performance and meeting engineering requirements, and a method for manufacturing the same.

[0008] The technical solution adopted by the present invention to solve the above-mentioned problem is: the high temperature molten salt corrosion resistant alloy for the solar thermal power generation equipment is characterized in that: its components are composed according to the following mass percentage (%): 6.0-8.0% Cr, 3.0-5.0% Fe, 0.04-0.08% C, ≤0.20% Co, ≤1.0 Mn%, ≤1.0 Si%, 1.0-2.0% W, 15.0-18.0% Mo, ≤0.015% P, ≤0.020% S, ≤0.50% Ti+Al, ≤0.010% B, and the rest is Ni and unavoidable impurities.

[0009] Preferably, the present invention has the following components in percentage by mass (%): 7.0% Cr, 4.0% Fe, 0.06% C, 0.17% Co, 0.8% Mn, 0.5% Si, 1.5% W, 16.0% Mo, 0.015% P, 0.020% S, 0.36% Ti+Al, 0.001% B, and the remainder is Ni and unavoidable impurities.

[0010] The present invention also provides a method for manufacturing a high temperature molten salt corrosion resistant alloy for a photothermal power generation device, using the high temperature molten salt corrosion resistant alloy for a photothermal power generation device as claimed in claim 1 or 2, characterized in that it comprises the following steps: S1) According to the formula of high temperature molten salt corrosion resistant alloy, raw materials are provided and smelted to obtain alloy vacuum induction smelting. The raw materials must be clean, dust-free, dry and oil-free; S2) electroslag remelting the alloy ingot to obtain an electroslag ingot, and the alloy smelting process is a double smelting process, including vacuum induction melting (VIM) + electroslag remelting (ESR); S3) forging the alloy ingot multiple times to obtain the alloy forging billet; S4) performing multi-fire rolling on the alloy ingot to obtain a hot-rolled finished product of a high temperature molten salt corrosion resistant alloy for a solar thermal power generation device.

[0011] Preferably, in step S1) of the present invention, vacuum induction melting is adopted, including full melting, first refining and second refining, Ni, Cr, W, Si base materials are put into the full melting, the melting temperature is 1520-1540°C, and the vacuum degree does not exceed 50Pa; the vacuum degree of the first refining does not exceed 5Pa, the melting temperature is 1530-1550°C, the C content is finely adjusted, and stirring is performed; after H, O, and N are qualified, a second refining is performed, Zr and Mn are put into the second refining and stirring is performed, the melting temperature is 1530-1550°C, and Ar3000Pa is filled; after the components are qualified, the temperature is adjusted to 1500-1520°C under argon protection for casting; the two refining processes can control the O and N contents. If the above-mentioned gas requirements are not met, stirring and sampling and analysis of the gas are continued until the above-mentioned gas requirements are met and subsequent operations are performed.

[0012] Preferably, in step S2) of the present invention, the electroslag composition includes CaF2, Al2O3, CaO, and MgO in a ratio of 65:20:10:5, and an appropriate amount of aluminum powder is added to the slag as appropriate; a nickel-based plate is used, Ar gas is filled for 15 minutes before arcing, and the melting rate is controlled, and the melting rate in the smelting stage is controlled at 180kg / h.

[0013] Preferably, in step S3) of the present invention, the electroslag ingot is subjected to a heat preservation treatment at 1100° C.-1250° C. for 5-120 min before forging.

[0014] Preferably, in step S3) of the present invention, open forging is first performed, and whether to perform open forging of the alloy ingot once is selected according to the ingot height-to-diameter ratio. The open forging method is upsetting, and the forged billet is air-cooled; an anvil with a diameter much larger than the material is used during upsetting, and the billet needs to be chamfered after upsetting.

[0015] Preferably, in step S3) of the present invention, intermediate forging is further performed, and the billet obtained after the blanking forging is heated and kept warm at a heating temperature of 1100° C.-1250° C. for a holding time of 5-30 min, followed by multiple fire forging.

[0016] Preferably, in step S3) of the present invention, the finished product is forged at last, and the billet after the intermediate forging is subjected to the final forging or drawing forming at a temperature lower than the phase transformation point to ensure the size requirements and ensure that the alloy reaches the corresponding uniformity and grain size. The forged billet is air-cooled to finally obtain a forged billet that meets the specifications.

[0017] Preferably, in step S4) of the present invention, the processed plate blank is placed in a heat treatment furnace and heated to 1000-1250°C, kept warm for 5-60 minutes, taken out and immediately subjected to the first round of rolling, with a rolling speed of 20mm / s-180mm / s, and a deformation of 5%-25% of the initial thickness, and then placed in a heat treatment furnace and kept warm for 25-30 minutes, and then taken out and the above rolling steps are repeated until the set total deformation is reached after several passes, and finally the blank is slowly air-cooled.

[0018] Compared with the prior art, the present invention has the following advantages and effects: through the proportion of the high temperature molten salt corrosion resistant alloy, the alloy has good machining performance and excellent mechanical properties in the solid solution state, and has higher high temperature performance at 800°C. DETAILED DESCRIPTION

[0019] The present invention will be further described in detail below by way of examples. The following examples are provided to explain the present invention but the present invention is not limited to the following examples.

[0020] Example

[0021] The high temperature molten salt corrosion resistant alloy used in the solar thermal power generation equipment of this embodiment has the following components in mass percentage (%): 7.0% Cr, 4.0% Fe, 0.06% C, 0.17% Co, 0.8% Mn, 0.5% Si, 1.5% W, 16.0% Mo, 0.015% P, 0.020% S, 0.36% Ti+Al, 0.001% B, and the rest is Ni and unavoidable impurities.

[0022] Calculated by mass percentage (%), Fe≤0.1%, Pb≤0.001%, Sn≤0.0012%, As≤0.0025%, Sb≤0.0025%, Bi≤0.0001%, O≤15ppm, and N≤30ppm in the high-temperature molten salt corrosion-resistant alloy used in solar thermal power generation equipment; if these elements exceed the limit, harmful precipitation phases will be formed, which will have a significant adverse effect on the plasticity and toughness of the alloy.

[0023] The manufacturing method of the high temperature molten salt corrosion resistant alloy for the solar thermal power generation equipment of this embodiment comprises the following steps: S1) providing raw materials and smelting them according to the formula of the high temperature molten salt corrosion resistant alloy to obtain the alloy vacuum induction smelting, and the raw materials must be clean, dust-free, dry and oil-free; S2) electroslag remelting the alloy ingot to obtain an electroslag ingot, and the alloy smelting process is a double smelting, including VIM+ESR; S3) forging the alloy ingot multiple times to obtain the alloy forging blank; S4) multi-fire rolling the alloy ingot to obtain a hot-rolled finished product of the high temperature molten salt corrosion resistant alloy for the solar thermal power generation equipment.

[0024] In step S1), vacuum induction melting is adopted, including full melting, first refining and second refining, Ni, Cr, W, Si base materials are put into the full melting, the melting temperature is 1520-1540℃, and the vacuum degree does not exceed 50Pa; the vacuum degree of the first refining does not exceed 5Pa, the melting temperature is 1530-1550℃, the C content is finely adjusted, and stirring is performed; after H, O, and N are qualified, the second refining is performed, Zr and Mn are put into the second refining and stirred, the melting temperature is 1530-1550℃, and Ar3000Pa is filled; after the composition is qualified, the temperature is adjusted to 1500-1520℃ under argon protection for casting; the two refining processes can control the O and N contents. If the above gas requirements are not met, stirring and sampling and analysis of the gas are continued until the above gas requirements are met before subsequent operations are performed.

[0025] In step S2), the electroslag composition includes CaF2, Al2O3, CaO, and MgO in a ratio of 65:20:10:5, and an appropriate amount of aluminum powder is added to the slag as appropriate; a nickel-based substrate is used, Ar gas is filled for 15 minutes before arcing, and the melting rate is controlled. The melting rate in the smelting stage is controlled at 180kg / h.

[0026] In step S3), the electroslag ingot is subjected to a heat preservation treatment at 1100° C.-1250° C. for 5-120 minutes before forging.

[0027] In step S3), firstly, the blank forging is performed. According to the aspect ratio of the ingot, it is selected whether to perform the blank forging once for the alloy ingot. The blank forging method is upsetting, and the forged blank is air-cooled. During upsetting, an anvil with a diameter much larger than the material is used, and the blank needs to be chamfered after upsetting.

[0028] In step S3), intermediate forging is performed again, and the billet obtained after the blank forging is heated and kept warm, the heating temperature is 1100°C-1250°C, the holding time is 5-30 minutes, and then multiple fire forging is performed.

[0029] In step S3), the finished product is forged, and the intermediate forged billet is forged or stretched at a temperature below the phase transition point to ensure the size requirements and the alloy reaches the corresponding uniformity and grain size. The forged billet is air-cooled to obtain a forged billet that meets the specifications.

[0030] In step S4), the processed plate blank is placed in a heat treatment furnace and heated to 1000-1250°C, kept warm for 5-60 minutes, taken out and immediately subjected to the first round of rolling, with a rolling speed of 20mm / s-180mm / s, and a deformation amount of 5%-25% of the initial thickness, and then placed in a heat treatment furnace and kept warm for 25-30 minutes, and then taken out and repeated the above rolling steps until the set total deformation amount is reached after several passes, and finally the blank is slowly air-cooled.

[0031] Through the above description, those skilled in the art can already implement it.

[0032] In addition, it should be noted that the shapes and names of the parts and components of the specific embodiments described in this specification may be different, and the above content described in this specification is only an example of the structure of the present invention. All equivalent changes or simple changes made based on the structure, features and principles described in the patent concept of the present invention are included in the protection scope of the patent of the present invention. Technicians in the technical field to which the present invention belongs can make various modifications or supplements to the specific embodiments described or replace them in a similar manner, as long as they do not deviate from the structure of the present invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.

Claims

1. A high temperature molten salt corrosion resistant alloy for solar thermal power generation equipment, characterized in that: Its components are as follows in mass percentage (%): 6.0-8.0% Cr, 3.0-5.0% Fe, 0.04-0.08% C, ≤0.20% Co, ≤1.0% Mn%, ≤1.0% Si%, 1.0-2.0% W, 15.0-18.0% Mo, ≤0.015% P, ≤0.020% S, ≤0.50% Ti+Al, ≤0.010% B, and the rest is Ni and unavoidable impurities.

2. The high temperature molten salt corrosion resistant alloy for solar thermal power generation equipment according to claim 1, characterized in that: Its composition is as follows in mass percentage (%): 7.0% Cr, 4.0% Fe, 0.06% C, 0.17% Co, 0.8% Mn, 0.5% Si, 1.5% W, 16.0% Mo, 0.015% P, 0.020% S, 0.36% Ti+Al, 0.001% B, and the rest is Ni and unavoidable impurities.

3. A method for manufacturing a high temperature molten salt corrosion resistant alloy for a photothermal power generation device, using the high temperature molten salt corrosion resistant alloy for a photothermal power generation device as claimed in claim 1 or 2, characterized in that: The following steps are involved: S1) According to the formula of high temperature molten salt corrosion resistant alloy, raw materials are provided and smelted to obtain alloy vacuum induction smelting. The raw materials must be clean, dust-free, dry and oil-free; S2) electroslag remelting the alloy ingot to obtain an electroslag ingot, and the alloy smelting process is a double smelting process; S3) forging the alloy ingot multiple times to obtain the alloy forging billet; S4) performing multi-fire rolling on the alloy ingot to obtain a hot-rolled finished product of a high temperature molten salt corrosion resistant alloy for a solar thermal power generation device.

4. The method for manufacturing a high temperature molten salt corrosion resistant alloy for a photothermal power generation device according to claim 1, characterized in that: In the step S1), vacuum induction melting is adopted, including full melting, first refining and second refining, Ni, Cr, W, Si base materials are put into the full melting, the melting temperature is 1520-1540°C, and the vacuum degree does not exceed 50Pa; the vacuum degree of the first refining does not exceed 5Pa, the melting temperature is 1530-1550°C, the C content is finely adjusted, and stirring is performed; after H, O, and N are qualified, the second refining is performed, Zr and Mn are put into the second refining and stirred, the melting temperature is 1530-1550°C, and Ar3000Pa is filled; after the components are qualified, the temperature is adjusted to 1500-1520°C under argon protection for casting; the two refining processes can control the O and N contents. If the above gas requirements are not met, stirring and sampling and analysis of the gas are continued until the above gas requirements are met before subsequent operations are performed.

5. The method for manufacturing a high temperature molten salt corrosion resistant alloy for a photothermal power generation device according to claim 1, characterized in that: In the step S2), the electroslag composition includes CaF2, Al2O3, CaO, and MgO in a ratio of 65:20:10:5, and an appropriate amount of aluminum powder is added to the slag as appropriate; a nickel-based substrate is used, Ar gas is filled for 15 minutes before arcing, and the melting rate is controlled. The melting rate in the smelting stage is controlled at 180kg / h.

6. The method for manufacturing a high temperature molten salt corrosion resistant alloy for a photothermal power generation device according to claim 1, characterized in that: In the step S3), the electroslag ingot is subjected to a heat preservation treatment at 1100° C.-1250° C. for 5-120 minutes before forging.

7. The method for manufacturing a high temperature molten salt corrosion resistant alloy for a photothermal power generation device according to claim 1, characterized in that: In the step S3), firstly, the blank forging is performed, and whether to perform the blank forging once is selected according to the ingot height-diameter ratio. The blank forging method is upsetting, and the forged blank is air-cooled; an anvil with a diameter much larger than the material is used during upsetting, and the blank needs to be chamfered after upsetting.

8. The method for manufacturing a high temperature molten salt corrosion resistant alloy for a photothermal power generation device according to claim 1, characterized in that: In the step S3), intermediate forging is performed again, the blank obtained after the blank forging is heated and kept warm, the heating temperature is 1100° C.-1250° C., the holding time is 5-30 minutes, and then multiple fire forging is performed.

9. The method for manufacturing a high temperature molten salt corrosion resistant alloy for a photothermal power generation device according to claim 1, characterized in that: In the step S3), the finished product is forged at last, and the billet after the intermediate forging is subjected to the final forging or drawing forming when the temperature is lower than the phase transformation point, so as to ensure the size requirements and the corresponding uniformity and grain size of the alloy. The forged billet is air-cooled to finally obtain a forged billet that meets the specifications.

10. The method for manufacturing a high temperature molten salt corrosion resistant alloy for a photothermal power generation device according to claim 1, characterized in that: In the step S4), the processed plate blank is placed in a heat treatment furnace and heated to 1000-1250°C, kept warm for 5-60 minutes, taken out and immediately subjected to the first round of rolling, with a rolling speed of 20mm / s-180mm / s, and a deformation amount of 5%-25% of the initial thickness, and then placed in a heat treatment furnace and kept warm for 25-30 minutes, and then taken out and the above rolling steps are repeated until the set total deformation amount is reached after several passes, and finally the blank is slowly air-cooled.