Low-cost high-toughness aluminum alloy casting blank for plastic forming and preparation method of low-cost high-toughness aluminum alloy casting blank

Through low lithium content Al-Cu-Li alloy ratio, ultrasonic refining and high vacuum die-casting technology, the problems of large grains, composition segregation and high cost in the preparation of aluminum-lithium alloy casting billets are solved, and high strength and toughness and low cost are obtained. Aluminum lithium alloy casting billets are suitable for aerospace.

CN119061301AInactive Publication Date: 2024-12-03HUNAN UNIVERSITY SUZHOU INSTITUTE +2
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411565017.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-11-05
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing preparation methods of aluminum-lithium alloy casting billets have problems such as large grain size, serious segregation of macro-microscopic components, high cost, low operability and easy absorption of hydrogen oxidation of Li elements, which affects its application in the aerospace field.

Method used

Using the Al-Cu-Li alloy ratio with low lithium content, non-ferrous crucible smelting is carried out through a vacuum well furnace. Combined with ultrasonic refining and high vacuum die-casting or extrusion technology, the addition of Li elements and melt degassing is controlled to reduce Li The burning and gas inhalation are obtained to obtain high-quality aluminum lithium alloy casting billets.

Benefits of technology

It realizes the low cost, high strength and toughness and high-quality casting billets of aluminum lithium alloy, reduces production costs, avoids pores and component segregation defects, improves the mechanical properties of aluminum lithium alloy and the surface quality of casting billets, and is suitable for aerospace zero Part material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119061301A_ABST
    Figure CN119061301A_ABST
Patent Text Reader

Abstract

The invention discloses a low-cost high-toughness aluminum alloy casting blank for plastic forming and a preparation method thereof. The preparation method comprises the following steps: S1, selecting pure Al, pure Li, pure Cu, pure Mg and an intermediate alloy as raw materials for preparing an aluminum-lithium alloy; s2, raw materials without pure Li are mixed and smelted in a vacuum pit furnace, and the smelting temperature during smelting is 740-760 DEG C; s3, a pure Li raw material is added into the Li-free alloy melt, a covering agent is added to the surface layer of the aluminum-lithium alloy melt, and the smelting temperature of the stage ranges from 710 DEG C to 730 DEG C; and S4, carrying out ultrasonic refining treatment on the aluminum-lithium alloy melt, and pouring the aluminum-lithium alloy melt into a forming die of a high-vacuum die-casting machine or an extruding machine for die-casting or extrusion forming. According to the method, the low-cost and high-toughness aluminum alloy casting blank can be prepared, the preparation process is simple, the efficiency is high, and the defects of air holes, composition segregation and the like of the aluminum-lithium alloy are overcome.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a low-cost, high-strength and tough aluminum alloy casting blank for plastic forming and a preparation method thereof, belonging to the technical field of metallurgy and casting of metal materials. Background Art

[0002] Aluminum-lithium alloys have attracted extensive attention in cutting-edge fields such as aerospace due to their excellent properties such as high modulus and low density. Due to the special demand for high-performance aluminum-lithium alloy materials in aerospace components, aluminum-lithium alloys no longer pursue low density blindly, and excessive Li content will aggravate the anisotropy of aluminum-lithium alloys. Therefore, low-lithium (<1.3 wt.%) Al-Cu-Li alloys (i.e., the third-generation Al-Li alloys) have become one of the research hotspots in this field. Existing third-generation aluminum-lithium alloys often add micro-alloying elements such as Ag, Re, Sc, Ce, Er, Zn, and Zr to improve the properties of the alloy. However, the addition of these precious (heavy) metal elements such as Ag and Sc will increase costs and have a negative impact on density on the one hand, and too many alloying elements will aggravate the component segregation phenomenon in the solidified structure, and may even damage the toughness of the alloy, and make the alloy solidification and deformation process more complicated.

[0003] At present, plastic deformation processes such as extrusion, rolling, and forging are common methods for preparing high-performance aluminum-lithium alloy profiles for aviation. Their performance mainly depends on process parameters and billet quality, and less attention is paid to the "innate condition" of billet solidification structure. The preparation methods of the original billet required for plastic deformation mainly include: melting casting, spray deposition, and powder metallurgy. At present, the size of aluminum-lithium alloy billets produced in industrialized and stable production in China is limited. Existing aluminum-lithium alloy billets are often prepared by "vacuum melting + gravity casting", but there are the following problems: (1) The grain size is relatively large, reaching hundreds or even hundreds of microns; (2) The macro-micro composition segregation is serious, especially when there are more alloying elements, which will be further aggravated; (3) Because the Li element is extremely active and easy to absorb hydrogen oxidation, the casting process needs to be completed in a vacuum furnace, so the requirements for the vacuum melting furnace are high, and the method is not highly operable (such as unable to remove slag, degassing and refining, etc.), the cost is high, and the billet size is limited. Due to the "genetic effect", it is difficult for the coarse initial grains to be significantly refined through one or two deformation processes, which affects the quality of the ingot, and the quality of the ingot is particularly critical to the performance of aluminum-lithium alloy components. In summary, it is very necessary to study and develop new low-cost, high-strength and tough aluminum-lithium alloys for aviation and the preparation method of their ingots.

[0004] The patent application publication number CN108149087A discloses a method for manufacturing aluminum-lithium alloy and aluminum-lithium alloy profiles for aerospace use, the purpose of which is to solve the problem of difficulty in producing aluminum-lithium alloy and low strength of aluminum-lithium alloy. Aluminum-lithium alloy is composed of Mg, Li, Ti, Zr and Al; Mg: 5.5% to 6.5%, Li: 2.2% to 2.5%, Ti: 0.03% to 0.12%, Zr: 0.15% to 0.20%, Zr+Ti≤ 0.25% and Al as the balance. Method: weighing raw materials, preparing aluminum alloy melt, refining, spray forming, cutting into short bars, blind die extrusion, hot extrusion, quenching, stretching straightening and aging treatment. The invention spray forming solves the problem of difficulty in producing aluminum-lithium alloy and poor quality, with a tensile strength of 485Mpa, a specified non-proportional extension strength of 345Mpa, and an elongation of 10.0%; blind die extrusion can make the ingot more dense. However, the materials used in this invention still involve precious (heavy) metals such as Zr and the Li content is greater than 2wt.%, which is not suitable for the manufacture of low-cost, high-strength and tough aluminum-lithium alloy ingots. Summary of the invention

[0005] In order to solve the above technical problems, the technical solution adopted by the present invention is: Provided is a low-cost, high-strength and tough aluminum alloy ingot for plastic forming, which comprises the following components by mass percentage: Cu 4.0%-5.0%, Li 0.3%-1.2%, Mg 0.2%-0.5%, Mn 0.3%-0.6%, Ti 0.1%-0.3%, impurities less than or equal to 0.2%, and the balance is Al.

[0006] The present invention also provides a method for preparing a low-cost, high-strength and high-toughness aluminum alloy ingot for plastic forming, comprising the following steps: S1. Selecting pure Al, pure Li, pure Cu, pure Mg and a master alloy as raw materials for preparing an aluminum-lithium alloy, wherein the master alloy includes an Al-5Ti-B alloy and an Al-10Mn alloy; S2. Mixing raw materials not containing pure Li and smelting them in a vacuum pit furnace, using a non-iron crucible for smelting during the smelting process to obtain a Li-free alloy melt, and the smelting temperature during the smelting is 740° C. to 760° C.; S3, adding pure Li raw material to the Li-free alloy melt to obtain an aluminum-lithium alloy melt, and adding a covering agent to the surface of the aluminum-lithium alloy melt. The melting temperature of this stage is 710° C. to 730° C.; S4. The aluminum-lithium alloy melt is subjected to ultrasonic refining treatment to obtain a high-quality aluminum-lithium alloy melt, and is poured into a forming mold of a high vacuum die-casting machine or an extruder for die-casting or extrusion forming to obtain the desired aluminum alloy ingot.

[0007] Preferably, in step S2, the raw material not containing pure Li is preheated at 100°C for 10-15 minutes to remove water vapor, and the maximum vacuum degree in the vacuum pit furnace is 100 kPa.

[0008] Preferably, in step S2, after obtaining the Li-free alloy melt, the alloy melt is refined by rotary blowing of inert gas argon or nitrogen to degas and remove impurities from the alloy melt, wherein during the rotary blowing of the inert gas, the temperature of the alloy melt is 710°C to 730°C.

[0009] Preferably, in step S3, during the Li addition process, pure Li particles wrapped in aluminum foil are added to the Li-free alloy melt, and high-purity argon gas is passed into the alloy melt for protection, wherein the temperature of the Li-free alloy melt is 680°C to 700°C.

[0010] Preferably, in step S3, after obtaining the aluminum-lithium alloy melt, the vacuum degree in the vacuum pit furnace is reduced to below 2-5 Pa, and high-purity argon gas is filled in to make the vacuum degree in the vacuum pit furnace 60kPa-80kPa, so as to prevent vacuum evaporation of the Li element.

[0011] Preferably, in step S4, high-purity argon gas is introduced into the aluminum-lithium alloy melt during ultrasonic treatment, the ultrasonic preheating temperature is 200-300°C, the ultrasonic treatment time is 1-3 min, the ultrasonic power is 1.2 kW-1.8 kW, and the ultrasonic temperature is 670-690°C.

[0012] Preferably, in step S4, the preheating temperature of the forming die during the extrusion forming process using an extruder is 200-250°C, the pouring temperature of the aluminum-lithium alloy melt is 670-690°C, the extrusion pressure is 50-400MPa, and the holding time is 10-30 seconds.

[0013] Preferably, in step S4, the preheating temperature of the forming mold during the die-casting process using a high vacuum die-casting machine is 200~250°C, the pouring temperature of the aluminum-lithium alloy melt is 670~690°C, the vacuum degree of the mold cavity is 80kPa~100kPa, and the die-casting pressure is 50~100MPa.

[0014] The beneficial effects of the present invention are as follows: (1) Compared with the existing third-generation aluminum-lithium alloy, the alloy of the present invention uses fewer elements, the Li content in the alloy is as low as 0.3wt.%, and a small amount of common element Ti is used to replace the microalloying effect of various precious (or heavy) metal elements such as Sc, Ag, Zn, and Zr, which can effectively reduce the cost and smelting difficulty of the alloy while making the aluminum-lithium alloy of the present invention have good strength and toughness. It can be used as the original billet for plastic deformation processes such as extrusion, rolling, and forging, and can be used as a component material in the fields of aerospace and the like; (2) The pit-type vacuum furnace used in the alloy smelting process of the present invention can change the ultimate vacuum degree in the furnace according to the different vacuum pumps configured, and the process of opening and closing the furnace cover - vacuuming - filling with argon is easy to operate; at the same time, by controlling the addition order of alloy raw materials (except pure Li) and pure Li, smelting temperature, vacuum degree, amount of high-purity argon gas, and the timing of melt degassing and refining, etc., it can solve the problems of high cost, high equipment dependence, large Li burn-off, and low operability of high-vacuum smelting of aluminum-lithium alloy in industrial production, and finally make the obtained aluminum-lithium alloy melt have the advantages of less air absorption and less Li element burn-off; (3) The present invention uses ultrasonic vibration to degas and refine the aluminum-lithium alloy melt, thereby solving the problem that the existing aluminum-lithium melt cannot be refined by rotating argon or nitrogen blowing, and the ultrasonic treatment can promote the uniform dispersion of solute atoms in the melt; at the same time, the ultrasonic time is short and the efficiency is high, which avoids serious loss of the ultrasonic tool head and improves the quality of the alloy melt; (4) The present invention adopts high vacuum die casting or squeeze casting to prepare aluminum-lithium alloy ingots. Solidification under high pressure will bring about effects that are difficult to obtain by gravity casting, such as rapid cooling, oxidation prevention, grain refinement and second phase, reduction or elimination of porosity, and reduction of segregation. In particular, high vacuum die casting is used to replace gravity casting to prepare aluminum-lithium alloy ingots. Combined with a pit vacuum furnace and an ultrasonic refining method, it can effectively reduce or even eliminate bubbles and dissolved gases generated by the molten metal during the filling and cooling process, prevent hydrogen absorption and oxidation, and thus improve the surface quality, air tightness, and mechanical properties of the ingots. (5) The method for preparing aluminum-lithium alloy ingots provided by the present invention is the first to use a forming technology that combines ultrasonic vibration with high vacuum die casting or extrusion casting to prepare aluminum-lithium alloy ingots. Compared with other aluminum alloys, due to the special properties of aluminum-lithium alloys such as hydrogen absorption and easy oxidation, the technology is more effective in preparing aluminum-lithium alloy ingots. In addition, the preparation process is simple, the efficiency is extremely high, the cost is low, and the ingot yield rate is high. The obtained aluminum-lithium alloy ingots have excellent mechanical properties and are free of defects such as pores and component segregation. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative work, among which: Figure 1 A schematic diagram of a process for preparing a low-cost, high-strength and tough aluminum alloy ingot for plastic forming in an embodiment of the present invention; Figure 2 Schematic diagram of the structure of the vacuum pit furnace used in the embodiment of the present invention; Figure 3is an optical microscope image of the microstructure of the Al-Cu-Li alloy in Example 1 of the present invention; Figure 4 3 is a scanning electron microscope image of the microstructure of the Al-Cu-Li alloy in Example 1 of the present invention.

[0016] In the figure: ① argon gas bottle, ② valve, ③ vacuum gauge, ④ lid opening handle, ⑤ vent valve, ⑥ sealing ring, ⑦ exhaust valve, ⑧ outer wall of melting furnace, ⑨ furnace cavity, ⑩ melt, Crucible, Cooling water, Copper pipe, Vacuum pump. DETAILED DESCRIPTION

[0017] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0018] A low-cost, high-strength and tough aluminum alloy ingot for plastic forming, which comprises the following components by mass percentage: Cu 4.0%-5.0%, Li 0.3%-1.2%, Mg 0.2%-0.5%, Mn 0.3%-0.6%, Ti 0.1%-0.3%, impurities less than or equal to 0.2%, and the balance is Al. The aluminum alloy ingot with this ratio has the advantages of low cost and high toughness, and can be used for plastic forming aerospace materials.

[0019] The present invention also provides a method for preparing a low-cost, high-strength and high-toughness aluminum alloy ingot for plastic forming, which can prepare the above-mentioned low-cost, high-strength and high-toughness aluminum alloy ingot for plastic forming. Example

[0020] refer to Figures 1 to 4 The method for preparing a low-cost, high-strength and high-toughness aluminum alloy ingot for plastic forming of the present invention comprises the following steps: S101: According to the designed alloy component ratio, pure Al, pure Li, pure Cu, pure Mg and Al-5Ti-B, Al-10Mn master alloys with corresponding contents are weighed as raw materials.

[0021] S102: Mix the raw materials except pure Li and put them into a vacuum melting furnace with a vacuum degree of 50 kPa. Melt them at 760°C. After the melting of the Li-free raw materials is completed, adjust the melt temperature to 720°C. Then open the furnace cover, use rotary argon blowing to perform refining treatment for degassing and impurity removal, close the furnace cover, evacuate, and let it stand to obtain a Li-free alloy melt.

[0022] S103: After the temperature of the Li-free alloy melt reaches 680°C, open the furnace cover, add pure Li particles wrapped in aluminum foil into the Li-free alloy melt using a bell jar, and pass high-purity argon gas for protection; after the pure Li particles are completely melted, adjust the temperature of the smelting furnace to 730°C, add a commercially available aluminum-lithium alloy-specific covering agent to the surface of the melt; close the cover, evacuate the furnace, wait for the vacuum degree in the furnace to rise to 100kPa, fill in an appropriate amount of high-purity argon gas, and reduce the vacuum degree in the furnace to 60kPa, so as to prevent vacuum evaporation of the Li element.

[0023] S104: insert the ultrasonic horn preheated at 200°C into the aluminum-lithium alloy melt 10 mm below the liquid surface for ultrasonic refining treatment, the ultrasonic treatment time is 1 min, the ultrasonic power is 1.5 kW, and the ultrasonic temperature is 690°C; then, pour the 690°C alloy melt into a mold preheated at 200°C, and perform extrusion casting to obtain aluminum alloy ingot for plastic deformation, the extrusion pressure is 50 MPa, and the holding time is 30 s. Example

[0024] The alloy composition of the cast aluminum alloy in this embodiment is calculated by mass percentage: Cu 5.0%, Li 0.6%, Mg 0.3%, Mn 0.5%, Ti 0.15%, impurities ≤ 0.2%, and the balance is Al.

[0025] According to another aspect of the present invention, there is provided a method for preparing the above-mentioned aluminum alloy ingot, the method comprising the following steps: S101: According to the designed alloy component ratio, pure Al, pure Li, pure Cu, pure Mg and Al-5Ti-B, Al-10Mn master alloys with corresponding contents are weighed as raw materials.

[0026] S102: Mix the raw materials except pure Li and put them into a vacuum melting furnace with a vacuum degree of 50 kPa. Melt them at 750°C. After the melting of the Li-free raw materials is completed, adjust the melt temperature to 720°C. Then open the furnace cover, use rotary argon blowing to perform refining treatment for degassing and impurity removal, close the furnace cover, evacuate, and let it stand to obtain a Li-free alloy melt.

[0027] S103: After the temperature of the Li-free alloy melt reaches 690°C, open the furnace cover, add pure Li particles wrapped in aluminum foil into the Li-free alloy melt using a bell jar, and pass high-purity argon gas for protection; after the pure Li particles are completely melted, adjust the temperature of the smelting furnace to 720°C, add a commercially available covering agent for aluminum-lithium alloy to the surface of the melt; close the cover, evacuate the furnace, wait for the vacuum degree in the furnace to rise to 100kPa, fill in an appropriate amount of high-purity argon gas, and reduce the vacuum degree in the furnace to 70kPa, so as to prevent vacuum evaporation of the Li element.

[0028] S104: The ultrasonic horn preheated at 250°C was inserted into the aluminum-lithium alloy melt 12 mm below the liquid surface for ultrasonic refining treatment. The ultrasonic treatment time was 2 min, the ultrasonic power was 1.5 kW, and the ultrasonic temperature was 680°C. Then, the alloy melt at 680°C was poured into a mold preheated at 220°C, and high vacuum casting was performed to obtain aluminum alloy ingots for plastic deformation. The vacuum degree of the mold cavity was 80 kPa, and the die-casting pressure was 100 MPa. Example

[0029] The alloy composition of the cast aluminum alloy in this embodiment is calculated by mass percentage: Cu 5.0%, Li 1.2%, Mg 0.3%, Mn 0.5%, Ti 0.15%, impurities ≤ 0.2%, and the balance is Al.

[0030] According to another aspect of the present invention, there is provided a method for preparing the above-mentioned aluminum alloy ingot, the method comprising the following steps: S101: According to the designed alloy component ratio, pure Al, pure Li, pure Cu, pure Mg and Al-5Ti-B, Al-10Mn master alloys with corresponding contents are weighed as raw materials.

[0031] S102: Mix the raw materials except pure Li and put them into a vacuum melting furnace with a vacuum degree of 50 kPa. Melt them at 740°C. After the melting of the Li-free raw materials is completed, adjust the melt temperature to 730°C. Then open the furnace cover, use rotary argon blowing to perform refining treatment for degassing and impurity removal, close the furnace cover, evacuate the furnace, and let it stand to obtain a Li-free alloy melt.

[0032] S103: After the temperature of the Li-free alloy melt reaches 700°C, open the furnace cover, add pure Li particles wrapped in aluminum foil into the Li-free alloy melt using a bell jar, and pass high-purity argon gas for protection; after the pure Li particles are completely melted, adjust the temperature of the smelting furnace to 710°C, add a commercially available covering agent for aluminum-lithium alloy to the surface of the melt; close the cover, evacuate the furnace, wait for the vacuum degree in the furnace to rise to 100kPa, fill in an appropriate amount of high-purity argon gas, and reduce the vacuum degree in the furnace to 80kPa, so as to prevent vacuum evaporation of the Li element.

[0033] S104: The ultrasonic horn preheated at 300°C was inserted into the aluminum-lithium alloy melt 15 mm below the liquid surface for ultrasonic refining treatment. The ultrasonic treatment time was 3 min, the ultrasonic power was 1.5 kW, and the ultrasonic temperature was 670°C. Then, the alloy melt at 670°C was poured into a mold preheated at 250°C, and extrusion casting was performed to obtain aluminum alloy ingots for plastic deformation. The extrusion pressure was 400 MPa and the holding time was 15 s.

[0034] Table 1 shows the composition and as-cast tensile mechanical properties (tensile strength, yield strength and elongation) of the aluminum-lithium alloy ingots and Li-free Al-Cu-Mn-Ti ingots prepared in different embodiments. The results show that the aluminum-lithium alloy provided by the present invention has good toughness, and its as-cast comprehensive mechanical properties are much higher than those of the aluminum-lithium alloy ingots produced by conventional semi-continuous casting or gravity casting, and its as-cast mechanical properties are also much higher than those of the Li-free Al-Cu-Mn-Ti alloy ingots produced by the same process.

[0035] Table 1 Composition and mechanical properties test results of aluminum-lithium alloy ingots prepared in different embodiments and the control group

[0036] The low-cost, high-strength and tough aluminum alloy ingot for plastic forming and the preparation method thereof of the present invention can avoid the hydrogenation and oxidation reaction in the aluminum-lithium alloy smelting process, and the burning loss of lithium in the air environment, thereby improving the utilization rate of the lithium element, overcoming the defects of the aluminum-lithium alloy such as pores and component segregation, having low manufacturing cost, and the obtained aluminum-lithium alloy having good strength and toughness, and can be used as a component material in the fields of aerospace and the like.

[0037] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.

Claims

1. A low-cost, high-strength and high-toughness aluminum alloy ingot for plastic forming, characterized in that: Calculated by mass percentage, it includes the following components: Cu 4.0%~5.0%, Li 0.3%~1.2%, Mg 0.2%~0.5%, Mn 0.3%~0.6%, Ti 0.1%~0.3%, impurities are less than or equal to 0.2%, and the balance is Al.

2. A method for preparing a low-cost, high-strength and tough aluminum alloy ingot for plastic forming, characterized in that: The steps include: S1. Selecting pure Al, pure Li, pure Cu, pure Mg and a master alloy as raw materials for preparing an aluminum-lithium alloy, wherein the master alloy includes an Al-5Ti-B alloy and an Al-10Mn alloy; S2. Mixing raw materials not containing pure Li and smelting them in a vacuum pit furnace, using a non-iron crucible for smelting during the smelting process to obtain a Li-free alloy melt, and the smelting temperature during the smelting is 740° C. to 760° C.; S3, adding pure Li raw material to the Li-free alloy melt to obtain an aluminum-lithium alloy melt, and adding a covering agent to the surface of the aluminum-lithium alloy melt. The melting temperature of this stage is 710° C. to 730° C.; S4. The aluminum-lithium alloy melt is subjected to ultrasonic refining treatment to obtain a high-quality aluminum-lithium alloy melt, and is poured into a forming mold of a high vacuum die-casting machine or an extruder for die-casting or extrusion forming to obtain the desired aluminum alloy ingot.

3. The method for preparing a low-cost, high-strength and tough aluminum alloy ingot for plastic forming according to claim 2, characterized in that: In step S2, the raw material not containing pure Li is preheated at 100°C for 10-15 minutes to remove water vapor, and the maximum vacuum degree in the vacuum pit furnace is 100 kPa.

4. The method for preparing a low-cost, high-strength and tough aluminum alloy ingot for plastic forming according to claim 3, characterized in that: In step S2, after obtaining the Li-free alloy melt, the alloy melt is refined by rotating and blowing an inert gas such as argon or nitrogen to degas and remove impurities from the alloy melt, wherein during the rotating and blowing of the inert gas, the temperature of the alloy melt is 710°C to 730°C.

5. The method for preparing a low-cost, high-strength and tough aluminum alloy ingot for plastic forming according to claim 4, characterized in that: In step S3, during the Li addition process, pure Li particles wrapped in aluminum foil are added into the Li-free alloy melt, and high-purity argon gas is passed into the alloy melt for protection, wherein the temperature of the Li-free alloy melt is 680°C to 700°C.

6. The method for preparing a low-cost, high-strength and tough aluminum alloy ingot for plastic forming according to claim 5, characterized in that: In step S3, after obtaining the aluminum-lithium alloy melt, the vacuum degree in the vacuum pit furnace is reduced to below 2-5 Pa, and high-purity argon gas is filled in to make the vacuum degree in the vacuum pit furnace 60 kPa-80 kPa.

7. The method for preparing a low-cost, high-strength and tough aluminum alloy ingot for plastic forming according to claim 2, characterized in that: In step S4, high-purity argon gas is introduced into the aluminum-lithium alloy melt during ultrasonic treatment, the ultrasonic preheating temperature is 200-300°C, the ultrasonic treatment time is 1-3 min, the ultrasonic power is 1.2 kW-1.8 kW, and the ultrasonic temperature is 670-690°C.

8. The method for preparing a low-cost, high-strength and tough aluminum alloy ingot for plastic forming according to claim 2, characterized in that: In step S4, the preheating temperature of the forming die during the extrusion forming process using the extruder is 200-250°C, the pouring temperature of the aluminum-lithium alloy melt is 670-690°C, the extrusion pressure is 50-400MPa, and the holding time is 10-30 seconds.

9. The method for preparing a low-cost, high-strength and tough aluminum alloy ingot for plastic forming according to claim 2, characterized in that: In step S4, the preheating temperature of the forming mold during the die-casting process using a high vacuum die-casting machine is 200~250°C, the pouring temperature of the aluminum-lithium alloy melt is 670~690°C, the vacuum degree of the mold cavity is 80kPa~100kPa, and the die-casting pressure is 50~100MPa.

Citation Information

Patent Citations

  • Improved method for processing sheet metal made of an al-cu-li alloy

    CA2851592A1

  • Al-cu-li-mg-mn-zn alloy wrought product

    CA3013955A1

  • Medium-strength high-toughness aluminum lithium alloy and preparation method thereof

    CN101967589A

  • High-toughness aluminum lithium alloy and preparation method thereof

    CN102021457A

  • Vacuum high-pressure die-casting forming method for light high-toughness aluminum-lithium alloy casting and product

    CN115846612A