Austenitic stainless steel cold-rolled steel sheet and manufacturing method thereof
By adjusting the chemical composition and process flow of austenitic stainless steel, the problems of insufficient corrosion resistance and pore defects in high chloride ion environments are solved, and austenitic with high corrosion resistance, high strength and low cost are achieved Stainless steel cold rolled steel plate has excellent yield strength, tensile strength and elongation.
Patent Information
- Application Number
- CN202411563946.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-11-05
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-11-05
AI Technical Summary
The existing austenitic stainless steel 316L is insufficient in corrosion resistance in high chloride ion environments, and pore defects are easily generated during the smelting process, affecting surface quality and processing performance.
By adjusting chemical composition and process flow, austenitic stainless steel cold rolled steel plates are prepared, including C, Si, Mn, Cr, Ni, Cu, Mo, N and other elements, to meet the specific MY, MT, and PREN value ranges and perform all Massification heat treatment, pickling, cold rolling and recrystallization heat treatment ensures yield strength, tensile strength and corrosion resistance.
Achieved high corrosion resistance, high strength and low cost of austenitic stainless steel cold-rolled steel plates, avoiding porous surface defects, yield strength between 340MPa and 480MPa, tensile strength is not less than 650MPa, and elongation is not less than 40%. , the pitting potential shall not be less than 630mV.
Smart Images

Figure CN119061331A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to an austenitic stainless steel cold-rolled steel plate product and a manufacturing method thereof, in particular to a stainless steel cold-rolled steel plate product with low cost, high strength, high corrosion resistance and high processing performance and a manufacturing method thereof. Background Art
[0002] Austenitic stainless steel 316L is widely used in the chemical industry due to its excellent corrosion resistance. The excellent corrosion resistance of 316L steel mainly comes from the addition of 2-3% Mo element. Due to the expensive price of Mo raw materials, its cost is much higher than that of conventional 18-8 series stainless steel.
[0003] The dynamic point method is used to measure the pitting potential of stainless steel in a neutral 3.5% NaCl solution at 30°C. It is a commonly used method to evaluate the chloride ion corrosion resistance of stainless steel. The corresponding current density on the measured anodic polarization curve is 100μA / cm 2 The maximum potential value is recorded as the pitting potential E' of stainless steel. b100 The higher the pitting potential value, the better the corrosion resistance. Pitting potential E' of austenitic stainless steel 316L b100 At around 400mV, it can be used in a normal temperature environment with a chloride ion content below 1000ppm, but it cannot be used in a more severe environment with a chloride ion content above 1000ppm.
[0004] The yield strength of austenitic stainless steel cold-rolled steel sheets is generally between 240 and 300 MPa. Improving the strength of stainless steel can enable the use of thinner and less steel plate raw materials in product design, thereby saving costs. Therefore, high-strength stainless steel is very popular in many applications. Adding nitrogen to the composition and using the solid solution strengthening effect of nitrogen to improve the strength of stainless steel is one of the methods for manufacturing high-strength steel. However, high-nitrogen stainless steel is prone to obvious pore defects during smelting, especially pores on the surface or near the surface of the ingot due to internal oxidation. In subsequent processing, the pores cannot be rolled together, which will leave obvious defects on the surface, affecting the surface quality. Severe pores will also cause the risk of strip breakage during rolling. Summary of the invention
[0005] The first object of the present invention is to provide an austenitic stainless steel cold-rolled steel sheet with low cost, high corrosion resistance, high strength and no obvious pore-like surface defects.
[0006] To achieve the above object, the present invention adopts the following technical scheme: an austenitic stainless steel cold-rolled steel plate, the chemical composition of the austenitic stainless steel cold-rolled steel plate comprises, by weight percentage: C: 0.008-0.030%, Si: 0.3-0.8%, Mn: 0.5-1.0%, Cr: 19.5-22.0%, Ni: 8.5-10.0%, Cu: 0.5-1.5%, Mo: 0.5-1.0%, N: 0.17-0.25%, the rest is Fe and other inevitable impurities, and the chemical composition satisfies the following relationship: 70≤MY≤120; and MT≥170; and PREN≥27; among which: MY=400×(C+2×N)+3.8×Ni+7.7×Mo-5.8×Cr; MT=320×(C+2×N) +2.2×Ni+8.6×Mo+1.1×Cr-2.1×Cu; PREN = Cr+3.3×Mo+30×N-Mn; The yield strength of the austenitic stainless steel cold-rolled steel plate is 340MPa to 480MPa; The tensile strength of the austenitic stainless steel cold-rolled steel plate is not less than 650 MPa; The elongation of the austenitic stainless steel cold-rolled steel sheet is not less than 40%; The pitting potential of the austenitic stainless steel cold-rolled steel sheet is not less than 630 mV.
[0007] Furthermore, in the aforementioned austenitic stainless steel cold-rolled steel sheet, the Cr content is 21.0-22.0%.
[0008] The second object of the present invention is to provide a method for manufacturing austenitic stainless steel cold-rolled steel sheet with low cost, high corrosion resistance, high strength and no obvious pore-like surface defects.
[0009] To achieve the above object, the present invention adopts the following technical solution: a method for manufacturing austenitic stainless steel cold-rolled steel sheet, comprising the following steps: S1: Casting the molten steel after roughing and refining into a slab, the chemical composition of the slab comprises, by weight percentage: C: 0.008-0.030%, Si: 0.3-0.8%, Mn: 0.5-1.0%, Cr: 19.5-22.0%, Ni: 8.5-10.0%, Cu: 0.5-1.5%, Mo: 0.5-1.0%, N: 0.17-0.25%, the rest is Fe and other inevitable impurities, and the chemical composition satisfies the following relationship: 70≤MY≤120; and MT≥170; and PREN≥27; among which: MY=400×(C+2×N)+3.8×Ni+7.7×Mo-5.8×Cr; MT=320×(C+2×N) +2.2×Ni+8.6×Mo+1.1×Cr-2.1×Cu; PREN = Cr+3.3×Mo+30×N-Mn; S2: subjecting the slab to homogenization heat treatment, wherein the homogenization heat treatment is carried out in a heating furnace, the slab is heated in the heating furnace for at least 120 minutes, the furnace temperature of the heating furnace is not less than 1220°C and is not higher than the Td temperature value represented by formula (1); wherein, Formula (1): Td = 1986 + 695 × C - 41.8 × Si + 4.5 × Mn - 61.4 × Cr + 44.2 × Ni - 4.0 × Mo + 20.9 × Cu + 860 × N; S3: hot rolling the slab after homogenization heat treatment to form a hot-rolled steel plate, and removing the oxide scale on the surface of the hot-rolled steel plate by pickling; S4: cold rolling the hot-rolled steel sheet at a reduction rate of not less than 55%, and then performing a recrystallization heat treatment to obtain an austenitic stainless steel cold-rolled steel sheet; The yield strength of the austenitic stainless steel cold-rolled steel plate is 340MPa to 480MPa; The tensile strength of the austenitic stainless steel cold-rolled steel plate is not less than 650 MPa; The elongation of the austenitic stainless steel cold-rolled steel sheet is not less than 40%; The pitting potential of the austenitic stainless steel cold-rolled steel sheet is not less than 630 mV.
[0010] Furthermore, in the aforementioned method for manufacturing austenitic stainless steel cold-rolled steel sheet, in which: in S3, when hot rolling the slab, the first pass reduction ratio of hot rolling rough rolling is not greater than 18%.
[0011] Furthermore, in the aforementioned method for manufacturing austenitic stainless steel cold-rolled steel sheet, in which: in S4, the recrystallization heat treatment is carried out in an annealing furnace, the annealing furnace temperature is between 1050°C and 1200°C, and after annealing, it is cooled to below 200°C at a cooling rate of not less than 15°C / S.
[0012] Furthermore, the aforementioned method for manufacturing an austenitic stainless steel cold-rolled steel sheet, wherein: in S4, the recrystallization heat treatment can be carried out in an aerobic environment or in an anaerobic environment; when the recrystallization heat treatment is carried out in an aerobic environment, it is also necessary to undergo pickling after cooling to remove the surface oxide scale to obtain an austenitic stainless steel cold-rolled steel sheet with a bright surface; and when the recrystallization heat treatment is carried out in an anaerobic environment, an austenitic stainless steel cold-rolled steel sheet with a bright surface is obtained.
[0013] Through the implementation of the above technical scheme, the beneficial effects of the present invention are: (1) the austenitic stainless steel cold-rolled steel sheet of the present invention has the excellent properties of high corrosion resistance, high strength, low cost, and no obvious pore-like surface defects; (2) the manufacturing method of the present invention is easy to implement and low cost, and can manufacture austenitic stainless steel cold-rolled steel sheets with high corrosion resistance, high strength, and no obvious pore-like surface defects. The yield strength of the manufactured austenitic stainless steel cold-rolled steel sheets is between 340MPa and 480MPa; the tensile strength is not less than 650MPa; the elongation is not less than 40%; and the pitting potential is not less than 630mV. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 This is a comparison diagram of the anodic polarization curves for measuring the pitting potential of Example 1 and Comparative Example 10.
[0015] Figure 2 It is a comparison diagram of the engineering stress-strain curves of Example 1 and Comparative Example 10. DETAILED DESCRIPTION
[0016] An austenitic stainless steel cold-rolled steel sheet, the chemical composition of the austenitic stainless steel cold-rolled steel sheet comprises, by weight percentage: C: 0.008-0.030%, Si: 0.3-0.8%, Mn: 0.5-1.0%, Cr: 19.5-22.0%, Ni: 8.5-10.0%, Cu: 0.5-1.5%, Mo: 0.5-1.0%, N: 0.17-0.25%, the rest is Fe and other inevitable impurities, and the chemical composition satisfies the following relationship: 70≤MY≤120; and MT≥170; and PREN≥27; among which: MY=400×(C+2×N)+3.8×Ni+7.7×Mo-5.8×Cr; MT=320×(C+2×N) +2.2×Ni+8.6×Mo+1.1×Cr-2.1×Cu; PREN = Cr+3.3×Mo+30×N-Mn; The yield strength of the austenitic stainless steel cold-rolled steel plate is 340MPa to 480MPa; The tensile strength of the austenitic stainless steel cold-rolled steel plate is not less than 650 MPa; The elongation of the austenitic stainless steel cold-rolled steel sheet is not less than 40%; The pitting potential of the austenitic stainless steel cold-rolled steel sheet is not less than 630 mV; preferably, the Cr content is 21.0-22.0%.
[0017] A method for manufacturing an austenitic stainless steel cold-rolled steel plate comprises the following steps: S1: Casting the molten steel after roughing and refining into a slab, the chemical composition of the slab comprises, by weight percentage: C: 0.008-0.030%, Si: 0.3-0.8%, Mn: 0.5-1.0%, Cr: 19.5-22.0%, Ni: 8.5-10.0%, Cu: 0.5-1.5%, Mo: 0.5-1.0%, N: 0.17-0.25%, the rest is Fe and other inevitable impurities, and the chemical composition satisfies the following relationship: 70≤MY≤120; and MT≥170; and PREN≥27; among which: MY=400×(C+2×N)+3.8×Ni+7.7×Mo-5.8×Cr; MT=320×(C+2×N) +2.2×Ni+8.6×Mo+1.1×Cr-2.1×Cu; PREN = Cr+3.3×Mo+30×N-Mn; S2: subjecting the slab to homogenization heat treatment, wherein the homogenization heat treatment is carried out in a heating furnace, the slab is heated in the heating furnace for at least 120 minutes, the furnace temperature of the heating furnace is not less than 1220°C and is not higher than the Td temperature value represented by formula (1); wherein, Formula (1): Td = 1986 + 695 × C - 41.8 × Si + 4.5 × Mn - 61.4 × Cr + 44.2 × Ni - 4.0 × Mo + 20.9 × Cu + 860 × N; S3: hot rolling the slab after homogenization heat treatment to form a hot-rolled steel plate, and removing the oxide scale on the surface of the hot-rolled steel plate by pickling; wherein, when the slab is hot-rolled, the first pass reduction rate of hot rolling rough rolling is not more than 18%; S4: cold rolling the hot-rolled steel sheet at a reduction rate of not less than 55%, and then performing recrystallization heat treatment to obtain an austenitic stainless steel cold-rolled steel sheet; wherein the recrystallization heat treatment is performed in an annealing furnace, the annealing furnace temperature is between 1050°C and 1200°C, and after annealing, the steel sheet is cooled to below 200°C at a cooling rate of not less than 15°C / S; and in S4, the recrystallization heat treatment can be performed in an aerobic environment or in an anaerobic environment; when the recrystallization heat treatment is performed in an aerobic environment, the steel sheet is further pickled after cooling to remove the surface oxide scale, so as to obtain an austenitic stainless steel cold-rolled steel sheet with a bright surface; the recrystallization heat treatment is performed in an anaerobic environment, so as to obtain an austenitic stainless steel cold-rolled steel sheet with a bright surface; The yield strength of the austenitic stainless steel cold-rolled steel plate is 340MPa to 480MPa; The tensile strength of the austenitic stainless steel cold-rolled steel plate is not less than 650 MPa; The elongation of the austenitic stainless steel cold-rolled steel sheet is not less than 40%; The pitting potential of the austenitic stainless steel cold-rolled steel sheet is not less than 630 mV.
[0018] The reasons for limiting the composition of the cold-rolled steel sheet are described in detail below: The content of C (carbon) is 0.008~0.030%wt. Carbon is a strong austenite-forming element. The appropriate carbon content will increase the strength of the product, but during heat treatment, carbon easily reacts with chromium to produce chromium carbide, which reduces corrosion resistance. Therefore, the C content is controlled below 0.030%; however, too low a carbon content will reduce the strength of the product, and is not conducive to the stability of the austenite phase during processing, while increasing the cost of smelting and decarburization.
[0019] The content of Si (silicon) is 0.3~0.8%wt. Silicon is a deoxidizer in the stainless steel smelting process. Too low silicon content will result in poor deoxidation effect, so the silicon content is controlled above 0.3%; silicon has a high affinity with oxygen, and too high silicon content is easy to form spinel oxide scale, which makes it difficult to remove the oxide scale after aerobic annealing. At the same time, too high silicon content will also cause smelting segregation and ductility reduction, making it difficult to produce steel strips, so the upper limit of silicon content is set at 0.8%.
[0020] The content of Mn (manganese) is 0.5~1.0%wt. Manganese is also an element that stabilizes the austenite phase. If the manganese content is too low, it will be detrimental to the dissolution and stability of the N element, so the lower limit of the manganese content is designed to be 0.5%. However, when the manganese content is too high, the pitting corrosion performance will decrease. In order to further improve the corrosion resistance, the upper limit of the manganese content is set at 1.0%.
[0021] The content of Cr (chromium) is 19.5~22.0%wt. Chromium is an essential element for improving the corrosion resistance of stainless steel. The higher the chromium content, the better the corrosion resistance. Based on this, the lower limit of chromium is set at 19.5%. At the same time, Cr is a ferrite-forming element. When the Cr content is too high, the stable austenite phase equilibrium will be broken, and higher austenite stabilizing elements are required to maintain the phase equilibrium. If the Cr content is too high, it will also cause segregation, and banded structures are likely to remain in the plate, and the solubility of N is reduced. Therefore, the present invention designs an upper limit of chromium of 22%. Preferably, in order to significantly improve the corrosion resistance, the lower limit of the Cr content is designed to be 21.0%.
[0022] The content of Ni (nickel) is 8.5~10.0%wt. Nickel is a typical austenite stabilizing element and is beneficial to improving the ductility of the material compared with other austenitizing elements. Due to the high Cr content, in order to ensure the stability of the austenite phase, the lower limit of Ni is designed to be 8.5%. When the nickel content is greater than 10.0%, the load during hot rolling is large and the raw material cost is too high, so the upper limit of Ni is set to 10.0%.
[0023] The Cu (copper) content is 0.5~1.5%wt. Adding more than 0.5% copper can significantly improve the processing and forming properties of stainless steel. However, when the copper content is too high, the tensile strength and hardness of the material will drop significantly, which does not meet the development purpose of high-strength steel. Therefore, the upper limit of Cu is designed to be 1.5%.
[0024] The content of Mo (molybdenum) is 0.5~1.0%wt. Mo is a strong and effective element to improve the corrosion resistance of steel, but when there is a high content of chromium, it is easy to form harmful intermetallic phases, which will reduce the hot working performance and forming processing performance of the material, and the cost of Mo raw materials is relatively high. Considering comprehensively, the content of Mo is controlled at 0.5~1.0%.
[0025] The content of N (nitrogen) is 0.17~0.25%wt. Nitrogen is an element that stabilizes austenite and is also an element that can improve the corrosion resistance of steel. It is also an important element for improving the strength of materials. Nitrogen alloying can reduce the usage of precious metals Ni and Cu, thereby reducing costs. Therefore, the lower limit of N in the present invention is set to 0.17%; however, too high a nitrogen content will increase the risk of nitride precipitation and easily form pores during the smelting process. The pores exposed on the surface during hot rolling are easily oxidized to cause crack-like defects on the coil surface; in addition, too high a nitrogen content will also cause the high-temperature strength of the steel to be too high, making rolling difficult, so the upper limit of nitrogen is set to 0.25%.
[0026] The rest of the steel is Fe (iron) and some inevitable impurities.
[0027] The content and function of the individual elements in the above components are not the key points of the design of the present invention, but are played by the overall coordinated combination of the contents of multiple elements. According to the embodiments, in addition to meeting the above ranges, the chemical composition of these components also needs to meet the following relationship: 70<MY<120;and MT>170;and PREN>27;among which: MY=400×(C+2×N)+3.8×Ni+7.7×Mo-5.8×Cr; MT=320×(C+2×N) +2.2×Ni+8.6×Mo+1.1×Cr-2.1×Cu; PREN = Cr+3.3×Mo+30×N-Mn; Different elements have different effects on the strength of stainless steel and interact with each other. The present invention controls the required MY value between 70 and 120 to ensure that the hot rolling and cold rolling have sufficient reduction rate, and the yield strength of the product in the conventional annealing state can be maintained between 340MPa and 480MPa. At the same time, the MT value is controlled above 170 to ensure that the material has a sufficiently high tensile strength and a sufficiently high elongation in the annealing state. If MT is below 170, the ratio of the material's yield strength to the tensile strength will be too high, and there will be problems such as insufficient product elongation and decreased forming performance. At the same time, necking defects will appear prematurely during the bulging process due to insufficient strength.
[0028] The components of the present invention also need to satisfy a PREN value of more than 27 to ensure sufficient chloride ion corrosion resistance of the product. The present invention controls the PREN value to more than 27 by combining high Cr, N, low Mo, and Mn components, thereby obtaining the characteristics of lower cost and higher chloride ion corrosion resistance than ASTM 316L stainless steel.
[0029] After the slab is cast, it is necessary to heat treat the slab for homogenization. The homogenization heat treatment is carried out in a heating furnace, and the slab is heated in the heating furnace for at least 120 minutes to fully eliminate the inevitable component segregation during casting. The furnace temperature of the heating furnace should not be lower than 1220°C, because the composition of the present invention contains a high content of N and alloy elements. If the temperature of the heating furnace is too low, the rolling force required for rolling is large, the rolling difficulty is high, and defects such as rolling cracks are prone to occur; at the same time, the temperature of the heating furnace is not higher than the Td temperature value represented by formula (1). If it is higher than the Td temperature value, although the slab is well homogenized and has low deformation resistance, due to the high Cr content in the composition, the binding force between Cr and O is strong, and the high temperature of the heating furnace will form an oxide scale that is difficult to remove, affecting the surface quality of subsequent products. On the other hand, some high-temperature ferrite will be newly generated in the slab, and the ferrite will reduce the solubility of N. The supersaturated N near the surface will escape from the surface of the slab, resulting in surface cracks in the slab during rolling.
[0030] Formula (1): Td = 1986 + 695 × C - 41.8 × Si + 4.5 × Mn - 61.4 × Cr + 44.2 × Ni - 4.0 × Mo + 20.9 × Cu + 860 × N; The slab after homogenization heat treatment is hot rolled to form a hot-rolled steel strip, and the oxide scale on the surface of the hot-rolled steel strip is removed by pickling. Preferably, the first pass reduction rate of hot rolling rough rolling is not more than 18%. During the first pass of hot rolling, the slab temperature is high and the deformation resistance is small. It is advisable to select a larger reduction rate to reduce the total number of reduction passes. However, if the first pass reduction rate is too high, due to the violent friction between the slab surface and the roller surface, the pores or internal cracks that may exist in a small amount near the surface of the high-N steel will be exposed and oxidized after being subjected to the positive compressive stress and tangential friction of the roller before rolling. In the subsequent rolling, it is impossible to roll together, resulting in surface defects and affecting the corrosion resistance. Therefore, the first pass reduction rate is controlled at 18% or below to reduce the risk caused by pores in the high-N steel slab.
[0031] The hot-rolled slab is annealed and pickled to obtain a hot-rolled steel plate, and then the hot-rolled steel plate is cold-rolled at a reduction rate of more than 55% to fully fragment the grains and provide sufficient power for recrystallization annealing. Then the recrystallization heat treatment is carried out. The temperature of the heat treatment furnace is 1050℃~1200℃ to ensure that C and N are fully dissolved and the grains are completely recrystallized. After annealing, it is cooled to below 200℃ at a cooling rate of not less than 15℃ / S to prevent the precipitation of carbonitrides and high-chromium intermetallic phases during the cooling process, which reduces the elongation and corrosion resistance.
[0032] The above recrystallization heat treatment can be carried out in an aerobic environment or in an anaerobic environment. If it is carried out in an aerobic environment, a necessary pickling step is also required to obtain an austenitic stainless steel cold-rolled steel sheet with a bright surface and no obvious oxide scale residue.
[0033] The yield strength of the cold-rolled steel sheet of the present invention processed through the above steps is not less than 340MPa and not more than 480MPa, that is, the yield strength is between 340MPa and 480MPa, the tensile strength is not less than 650MPa, and the elongation is not less than 40%.
[0034] The dynamic point method is used to measure the pitting potential of stainless steel in a neutral 3.5% NaCl solution at 30°C. It is a commonly used method to evaluate the chloride ion corrosion resistance of stainless steel. The corresponding current density on the measured anodic polarization curve is 100μA / cm 2 The maximum potential value is recorded as the pitting potential E' of stainless steel. b100 The higher the pitting potential value, the better the corrosion resistance. The pitting potential of the stainless steel of the present invention in a 30°C, 3.5% NaCl solution is above 630 mV. Compared with conventional 316L (Comparative Example 10), the pitting potential value of the stainless steel of the present invention in a 30°C, 3.5% NaCl solution is increased by more than 50%.
[0035] The present invention is further described in detail below through specific examples and comparative examples. In the following examples and comparative examples, when specifically calculating MY, MT, PREN and Td, according to industry rules, the values of the components in the formulas of MY, MT, PREN and Td are directly used in the percentage content, and the values are not converted without the percentage sign. For example, when the component C is 0.025%, the value 0.025 is directly used in the formula; and the calculated values of MY, MT, PREN and Td are rounded off and accurate to the unit place; Example 1
[0036] A method for manufacturing an austenitic stainless steel cold-rolled steel plate comprises the following steps: S1: Casting the molten steel after roughing and refining into a slab, the chemical composition of the slab comprises, by weight percentage, C: 0.025%, Si: 0.4%, Mn: 0.72%, Cr: 21.6%, Ni: 9.3%, Cu: 0.7%, Mo: 0.55%, N: 0.21%, the rest is Fe and other inevitable impurities, and the MY value is 92, the MT value is 190, and the PREN value is 29; S2: subjecting the slab to homogenization heat treatment, wherein the homogenization heat treatment is carried out in a heating furnace, the slab is heated in the heating furnace for 220 minutes, the furnace temperature of the heating furnace is controlled at 1255°C, and the furnace temperature of the heating furnace is not lower than 1220°C and not higher than the Td temperature value of 1268°C; S3: hot rolling the slab after homogenization heat treatment to form a hot-rolled steel plate, and removing the oxide scale on the surface of the hot-rolled steel plate by pickling; wherein, when the slab is hot-rolled, the first pass reduction rate of hot rolling rough rolling is 18%; S4: The hot-rolled steel sheet is cold rolled at a reduction rate of 78%, and then recrystallized in an oxygen environment. After cooling, it is pickled to remove the surface oxide scale to obtain an austenitic stainless steel cold-rolled steel sheet with a bright surface; wherein the recrystallization heat treatment is carried out in an annealing furnace at a temperature of 1150°C, and after annealing, it is cooled to below 200°C at a cooling rate of 28°C / S; The yield strength of the austenitic stainless steel cold-rolled steel plate is 402MPa; The tensile strength of the austenitic stainless steel cold-rolled steel plate is 712MPa; The elongation of the austenitic stainless steel cold-rolled steel sheet is 46%; The pitting potential of the austenitic stainless steel cold-rolled steel sheet is 1128 mV. Example 2
[0037] A method for manufacturing an austenitic stainless steel cold-rolled steel plate comprises the following steps: S1: Casting the molten steel after roughing and refining into a slab, the chemical composition of the slab comprises, by weight percentage, C: 0.023%, Si: 0.31%, Mn: 0.61%, Cr: 21.9%, Ni: 9.5%, Cu: 0.6%, Mo: 0.60%, N: 0.217%, the rest is Fe and other inevitable impurities, and the MY value is 97, the MT value is 195, and the PREN value is 29.8; S2: subjecting the slab to homogenization heat treatment, wherein the homogenization heat treatment is carried out in a heating furnace, the slab is heated in the heating furnace for 230 minutes, the furnace temperature of the heating furnace is controlled at 1250° C., and the furnace temperature of the heating furnace is not lower than 1220° C. and not higher than the Td temperature value of 1263° C.; S3: hot rolling the slab after homogenization heat treatment to form a hot-rolled steel plate, and removing the oxide scale on the surface of the hot-rolled steel plate by pickling; wherein, when the slab is hot rolled, the first pass reduction rate of hot rolling rough rolling is 14%; S4: cold rolling the hot-rolled steel sheet at a reduction rate of 75%, and then performing recrystallization heat treatment in an oxygen-free environment to obtain an austenitic stainless steel cold-rolled steel sheet with a bright surface; wherein the recrystallization heat treatment is performed in an annealing furnace at a temperature of 1150°C, and after annealing, the steel sheet is cooled to below 200°C at a cooling rate of 28°C / S; The yield strength of the austenitic stainless steel cold-rolled steel plate is 412 MPa; The tensile strength of the austenitic stainless steel cold-rolled steel plate is 722MPa; The elongation of the austenitic stainless steel cold-rolled steel sheet is 47%; The pitting potential of the austenitic stainless steel cold-rolled steel sheet is 1235 mV. Example 3
[0038] A method for manufacturing an austenitic stainless steel cold-rolled steel plate comprises the following steps: S1: Casting the molten steel after roughing and refining into a slab, the chemical composition of the slab comprises, by weight percentage, C: 0.013%, Si: 0.45%, Mn: 0.98%, Cr: 21.1%, Ni: 8.5%, Cu: 1.1%, Mo: 0.8%, N: 0.197%, the rest is Fe and other inevitable impurities, and the MY value is 79, the MT value is 177, and the PREN value is 28.7; S2: subjecting the slab to homogenization heat treatment, wherein the homogenization heat treatment is carried out in a heating furnace, the slab is heated in the heating furnace for 240 minutes, the furnace temperature of the heating furnace is controlled at 1220° C., and the furnace temperature of the heating furnace is not higher than the Td temperature value of 1250° C.; S3: hot rolling the slab after homogenization heat treatment to form a hot-rolled steel plate, and removing the oxide scale on the surface of the hot-rolled steel plate by pickling; wherein, when the slab is hot rolled, the first pass reduction rate of hot rolling rough rolling is 17%; S4: cold rolling the hot-rolled steel sheet at a reduction rate of 80%, and then performing recrystallization heat treatment in an oxygen-free environment to obtain an austenitic stainless steel cold-rolled steel sheet with a bright surface; wherein the recrystallization heat treatment is performed in an annealing furnace at a temperature of 1200°C, and after annealing, the steel sheet is cooled to below 200°C at a cooling rate of 25°C / S; The yield strength of the austenitic stainless steel cold-rolled steel plate is 342 MPa; The tensile strength of the austenitic stainless steel cold-rolled steel plate is 698 MPa; The elongation of the austenitic stainless steel cold-rolled steel sheet is 54%; The pitting potential of the austenitic stainless steel cold-rolled steel sheet is 987 mV. Example 4
[0039] A method for manufacturing an austenitic stainless steel cold-rolled steel plate comprises the following steps: S1: Casting the molten steel after roughing and refining into a slab, the chemical composition of the slab comprises, by weight percentage, C: 0.029%, Si: 0.80%, Mn: 0.59%, Cr: 21.1%, Ni: 9.8%, Cu: 0.5%, Mo: 0.98%, N: 0.170%, the rest is Fe and other inevitable impurities, and the MY value is 70, the MT value is 170, and the PREN value is 28.8; S2: subjecting the slab to homogenization heat treatment, wherein the homogenization heat treatment is carried out in a heating furnace, the slab is heated in the heating furnace for 220 minutes, the furnace temperature of the heating furnace is controlled at 1250° C., and the furnace temperature of the heating furnace is not lower than 1220° C. and not higher than the Td temperature value of 1266° C.; S3: hot rolling the slab after homogenization heat treatment to form a hot-rolled steel plate, and removing the oxide scale on the surface of the hot-rolled steel plate by pickling; wherein, when the slab is hot rolled, the first pass reduction rate of hot rolling rough rolling is 17%; S4: cold rolling the hot-rolled steel sheet at a reduction rate of more than 73%, followed by recrystallization heat treatment in an aerobic environment, and then pickling to remove surface oxide scale after cooling to obtain an austenitic stainless steel cold-rolled steel sheet with a bright surface; wherein the recrystallization heat treatment is carried out in an annealing furnace at a temperature of 1180°C, and after annealing, the steel sheet is cooled to below 200°C at a cooling rate of 25°C / S; The yield strength of the austenitic stainless steel cold-rolled steel plate is 340 MPa; The tensile strength of the austenitic stainless steel cold-rolled steel plate is 685 MPa; The elongation of the austenitic stainless steel cold-rolled steel sheet is 52%; The pitting potential of the austenitic stainless steel cold-rolled steel sheet is 1078 mV. Example 5
[0040] A method for manufacturing an austenitic stainless steel cold-rolled steel plate comprises the following steps: S1: Casting the molten steel after roughing and refining into a slab, the chemical composition of the slab comprises, by weight percentage, C: 0.030%, Si: 0.58%, Mn: 0.97%, Cr: 19.8%, Ni: 8.6%, Cu: 0.6%, Mo: 0.90%, N: 0.193%, the rest is Fe and other inevitable impurities, and the MY value is 91, the MT value is 180, and the PREN value is 27.6; S2: subjecting the slab to homogenization heat treatment, wherein the homogenization heat treatment is carried out in a heating furnace, the slab is heated in the heating furnace for 180 minutes, the furnace temperature of the heating furnace is controlled at 1260° C., the furnace temperature of the heating furnace is not lower than 1220° C. and not higher than the Td temperature value of 1329° C.; S3: hot rolling the slab after homogenization heat treatment to form a hot-rolled steel plate, and removing the oxide scale on the surface of the hot-rolled steel plate by pickling; wherein, when the slab is hot-rolled, the first pass reduction rate of hot rolling rough rolling is 16%; S4: The hot-rolled steel sheet is cold rolled at a reduction rate of 55%, and then recrystallized in an oxygen environment. After cooling, it is pickled to remove the surface oxide scale to obtain an austenitic stainless steel cold-rolled steel sheet with a bright surface; wherein the recrystallization heat treatment is carried out in an annealing furnace at a temperature of 1120°C, and after annealing, it is cooled to below 200°C at a cooling rate of 30°C / S; The yield strength of the austenitic stainless steel cold-rolled steel plate is 398 MPa; The tensile strength of the austenitic stainless steel cold-rolled steel plate is 725 MPa; The elongation of the austenitic stainless steel cold-rolled steel sheet is 45%; The pitting potential of the austenitic stainless steel cold-rolled steel sheet is 692 mV. Example 6
[0041] A method for manufacturing an austenitic stainless steel cold-rolled steel plate comprises the following steps: S1: Casting the molten steel after roughing and refining into a slab, the chemical composition of the slab comprises, by weight percentage, C: 0.029%, Si: 0.77%, Mn: 0.60%, Cr: 21.8%, Ni: 9.9%, Cu: 0.5%, Mo: 0.95%, N: 0.226%, the rest is Fe and other inevitable impurities, and the MY value is 111, the MT value is 207, and the PREN value is 31.1; S2: subjecting the slab to homogenization heat treatment, wherein the homogenization heat treatment is carried out in a heating furnace, the slab is heated in the heating furnace for 120 minutes, the furnace temperature of the heating furnace is controlled at 1270°C, and the furnace temperature of the heating furnace is not lower than 1220°C and not higher than the Td temperature value of 1277°C; S3: hot rolling the slab after homogenization heat treatment to form a hot-rolled steel plate, and removing the oxide scale on the surface of the hot-rolled steel plate by pickling; wherein, when the slab is hot-rolled, the first pass reduction rate of hot rolling rough rolling is 16%; S4: cold rolling the hot-rolled steel sheet at a reduction rate of 63%, and then performing recrystallization heat treatment in an oxygen-free environment to obtain an austenitic stainless steel cold-rolled steel sheet with a bright surface; wherein the recrystallization heat treatment is performed in an annealing furnace at a temperature of 1120°C, and after annealing, the steel sheet is cooled to below 200°C at a cooling rate of 28°C / S; The yield strength of the austenitic stainless steel cold-rolled steel plate is 465 MPa; The tensile strength of the austenitic stainless steel cold-rolled steel plate is 782MPa; The elongation of the austenitic stainless steel cold-rolled steel sheet is 43%; The pitting potential of the austenitic stainless steel cold-rolled steel sheet is 1186 mV. Example 7
[0042] A method for manufacturing an austenitic stainless steel cold-rolled steel plate comprises the following steps: S1: Casting the molten steel after roughing and refining into a slab, the chemical composition of the slab comprises, by weight percentage: C: 0.008%, Si: 0.55%, Mn: 0.95%, Cr: 21.0%, Ni: 8.5%, Cu: 1.5%, Mo: 0.99%, N: 0.248%, the rest is Fe and other inevitable impurities, and the MY value is 120, the MT value is 208, and the PREN value is 30.8; S2: subjecting the slab to homogenization heat treatment, wherein the homogenization heat treatment is carried out in a heating furnace, the slab is heated in the heating furnace for 230 minutes, the furnace temperature of the heating furnace is controlled at 1245°C, the furnace temperature of the heating furnace is not lower than 1220°C and not higher than the Td temperature value of 1300°C; S3: hot rolling the slab after homogenization heat treatment to form a hot-rolled steel plate, and removing the oxide scale on the surface of the hot-rolled steel plate by pickling; wherein, when the slab is hot rolled, the first pass reduction rate of hot rolling rough rolling is 13%; S4: The hot-rolled steel sheet is cold rolled at a reduction rate of 73%, and then recrystallized in an oxygen environment. After cooling, the steel sheet is pickled to remove the surface oxide scale, thereby obtaining an austenitic stainless steel cold-rolled steel sheet with a bright surface. The recrystallization heat treatment is carried out in an annealing furnace at a temperature of 1150°C. After annealing, the steel sheet is cooled to below 200°C at a cooling rate of 20°C / S. The yield strength of the austenitic stainless steel cold-rolled steel plate is 480 MPa; The tensile strength of the austenitic stainless steel cold-rolled steel plate is 794 MPa; The elongation of the austenitic stainless steel cold-rolled steel sheet is 40%; The pitting potential of the austenitic stainless steel cold-rolled steel sheet is 1085 mV. Example 8
[0043] A method for manufacturing an austenitic stainless steel cold-rolled steel plate comprises the following steps: S1: Casting the molten steel after roughing and refining into a slab, the chemical composition of the slab comprises, by weight percentage, C: 0.011%, Si: 0.65%, Mn: 0.99%, Cr: 20.4%, Ni: 8.8%, Cu: 0.8%, Mo: 0.50%, N: 0.205%, the rest is Fe and other inevitable impurities, and the MY value is 87, the MT value is 179, and the PREN value is 27; S2: subjecting the slab to homogenization heat treatment, wherein the homogenization heat treatment is carried out in a heating furnace, the slab is heated in the heating furnace for 220 minutes, the furnace temperature of the heating furnace is controlled at 1240°C, and the furnace temperature of the heating furnace is not lower than 1220°C and not higher than the Td temperature value of 1298°C; S3: hot rolling the slab after homogenization heat treatment to form a hot-rolled steel plate, and removing the oxide scale on the surface of the hot-rolled steel plate by pickling; wherein, when the slab is hot rolled, the first pass reduction rate of hot rolling rough rolling is 14%; S4: The hot-rolled steel sheet is cold rolled at a reduction rate of 75%, and then recrystallized in an oxygen environment. After cooling, it is pickled to remove the surface oxide scale to obtain an austenitic stainless steel cold-rolled steel sheet with a bright surface; wherein the recrystallization heat treatment is carried out in an annealing furnace at a temperature of 1110°C, and after annealing, it is cooled to below 200°C at a cooling rate of 15°C / S; The yield strength of the austenitic stainless steel cold-rolled steel plate is 392 MPa; The tensile strength of the austenitic stainless steel cold-rolled steel plate is 708MPa; The elongation of the austenitic stainless steel cold-rolled steel sheet is 54%; The pitting potential of the austenitic stainless steel cold-rolled steel sheet is 725 mV. Example 9
[0044] A method for manufacturing an austenitic stainless steel cold-rolled steel plate comprises the following steps: S1: Casting the molten steel after roughing and refining into a slab, the chemical composition of the slab comprises, by weight percentage, C: 0.012%, Si: 0.65%, Mn: 0.85%, Cr: 20.6%, Ni: 9.1%, Cu: 0.5%, Mo: 0.72%, N: 0.195%, the rest is Fe and other inevitable impurities, and the MY value is 81, the MT value is 176, and the PREN value is 28.0; S2: subjecting the slab to homogenization heat treatment, wherein the homogenization heat treatment is carried out in a heating furnace, the slab is heated in the heating furnace for 230 minutes, the furnace temperature of the heating furnace is controlled at 1235°C, and the furnace temperature of the heating furnace is not lower than 1220°C and not higher than the Td temperature value of 1286°C; S3: hot rolling the slab after homogenization heat treatment to form a hot-rolled steel plate, and removing the oxide scale on the surface of the hot-rolled steel plate by pickling; wherein, when the slab is hot rolled, the first pass reduction rate of hot rolling rough rolling is 14%; S4: cold rolling the hot-rolled steel sheet at a reduction rate of 66%, and then performing recrystallization heat treatment in an oxygen-free environment to obtain an austenitic stainless steel cold-rolled steel sheet with a bright surface; wherein the recrystallization heat treatment is performed in an annealing furnace at a temperature of 1080°C, and after annealing, the steel sheet is cooled to below 200°C at a cooling rate of 28°C / S; The yield strength of the austenitic stainless steel cold-rolled steel plate is 379 MPa; The tensile strength of the austenitic stainless steel cold-rolled steel plate is 650MPa; The elongation of the austenitic stainless steel cold-rolled steel sheet is 44%; The pitting potential of the austenitic stainless steel cold-rolled steel sheet is 796 mV. Example 10
[0045] A method for manufacturing an austenitic stainless steel cold-rolled steel plate comprises the following steps: S1: Casting the molten steel after roughing and refining into a slab, the chemical composition of the slab comprises, by weight percentage, C: 0.030%, Si: 0.35%, Mn: 0.50%, Cr: 21.2%, Ni: 10.0%, Cu: 0.7%, Mo: 0.51%, N: 0.180%, the rest is Fe and other inevitable impurities, and the MY value is 75, the MT value is 173, and the PREN value is 27.8; S2: subjecting the slab to homogenization heat treatment, wherein the homogenization heat treatment is carried out in a heating furnace, the slab is heated in the heating furnace for 220 minutes, the furnace temperature of the heating furnace is controlled at 1240°C, and the furnace temperature of the heating furnace is not lower than 1220°C and not higher than the Td temperature value of 1302°C; S3: hot rolling the slab after homogenization heat treatment to form a hot-rolled steel plate, and removing the oxide scale on the surface of the hot-rolled steel plate by pickling; wherein, when the slab is hot rolled, the first pass reduction rate of hot rolling rough rolling is 15%; S4: The hot-rolled steel sheet is cold rolled at a reduction rate of 71%, and then recrystallized in an oxygen environment. After cooling, it is pickled to remove the surface oxide scale to obtain an austenitic stainless steel cold-rolled steel sheet with a bright surface; wherein the recrystallization heat treatment is carried out in an annealing furnace at a temperature of 1050°C, and after annealing, it is cooled to below 200°C at a cooling rate of 25°C / S; The yield strength of the austenitic stainless steel cold-rolled steel plate is 342 MPa; The tensile strength of the austenitic stainless steel cold-rolled steel plate is 665MPa; The elongation of the austenitic stainless steel cold-rolled steel sheet is 48%; The pitting potential of the austenitic stainless steel cold-rolled steel sheet is 861 mV. Embodiment 11
[0046] A method for manufacturing an austenitic stainless steel cold-rolled steel plate comprises the following steps: S1: Casting the molten steel after roughing and refining into a slab, the chemical composition of the slab comprises, by weight percentage, C: 0.019%, Si: 0.30%, Mn: 0.51%, Cr: 22.0%, Ni: 9.9%, Cu: 0.7%, Mo: 1.00%, N: 0.202%, the rest is Fe and other inevitable impurities, and the MY value is 87, the MT value is 188, and the PREN value is 30.9; S2: subjecting the slab to homogenization heat treatment, wherein the homogenization heat treatment is carried out in a heating furnace, the slab is heated in the heating furnace for 180 minutes, the furnace temperature of the heating furnace is controlled at 1260° C., and the furnace temperature of the heating furnace is not lower than 1220° C. and not higher than Td temperature value 1260° C.; S3: hot rolling the slab after homogenization heat treatment to form a hot-rolled steel plate, and removing the oxide scale on the surface of the hot-rolled steel plate by pickling; wherein, when the slab is hot-rolled, the first pass reduction rate of hot rolling rough rolling is 16%; S4: The hot-rolled steel sheet is cold rolled at a reduction rate of 73%, and then recrystallized in an oxygen environment. After cooling, the steel sheet is pickled to remove the surface oxide scale, thereby obtaining an austenitic stainless steel cold-rolled steel sheet with a bright surface. The recrystallization heat treatment is carried out in an annealing furnace at a temperature of 1180°C. After annealing, the steel sheet is cooled to below 200°C at a cooling rate of 20°C / S. The yield strength of the austenitic stainless steel cold-rolled steel plate is 372 MPa; The tensile strength of the austenitic stainless steel cold-rolled steel plate is 739 MPa; The elongation of the austenitic stainless steel cold-rolled steel sheet is 48%; The pitting potential of the austenitic stainless steel cold-rolled steel sheet is 1245 mV. Example 12
[0047] A method for manufacturing an austenitic stainless steel cold-rolled steel plate comprises the following steps: S1: Casting the molten steel after roughing and refining into a slab, the chemical composition of the slab comprises, by weight percentage, C: 0.017%, Si: 0.80%, Mn: 0.98%, Cr: 19.5%, Ni: 8.5%, Cu: 0.5%, Mo: 0.98%, N: 0.188%, the rest is Fe and other inevitable impurities, and the MY value is 84, the MT value is 173, and the PREN value is 27.4; S2: subjecting the slab to homogenization heat treatment, wherein the homogenization heat treatment is carried out in a heating furnace, the slab is heated in the heating furnace for 150 minutes, the furnace temperature of the heating furnace is controlled at 1265°C, and the furnace temperature of the heating furnace is not lower than 1220°C and not higher than the Td temperature value of 1317°C; S3: hot rolling the slab after homogenization heat treatment to form a hot-rolled steel plate, and removing the oxide scale on the surface of the hot-rolled steel plate by pickling; wherein, when the slab is hot rolled, the first pass reduction rate of hot rolling rough rolling is 17%; S4: cold rolling the hot-rolled steel sheet at a reduction rate of 75%, and then performing recrystallization heat treatment in an oxygen-free environment to obtain an austenitic stainless steel cold-rolled steel sheet with a bright surface; wherein the recrystallization heat treatment is performed in an annealing furnace at a temperature of 1150°C, and after annealing, the steel sheet is cooled to below 200°C at a cooling rate of 25°C / S; The yield strength of the austenitic stainless steel cold-rolled steel plate is 370 MPa; The tensile strength of the austenitic stainless steel cold-rolled steel plate is 725 MPa; The elongation of the austenitic stainless steel cold-rolled steel sheet is 50%; The pitting potential of the austenitic stainless steel cold-rolled steel sheet is 630 mV.
[0048] Comparative Example 1 A method for manufacturing an austenitic stainless steel cold-rolled steel plate comprises the following steps: S1: Casting the molten steel after roughing and refining into a slab, the chemical composition of the slab comprises, by weight percentage, C: 0.015%, Si: 0.32%, Mn: 0.52%, Cr: 21.3%, Ni: 9.1%, Cu: 0.6%, Mo: 0.52%, N: 0.174%, the rest is Fe and other inevitable impurities, and the MY value is 60, the MT value is 163, and the PREN value is 27.7; S2: subjecting the slab to homogenization heat treatment, wherein the homogenization heat treatment is carried out in a heating furnace, the slab is heated in the heating furnace for 180 minutes, the furnace temperature of the heating furnace is controlled at 1255°C, the furnace temperature of the heating furnace is not lower than 1220°C and higher than the Td temperature value of 1240°C; S3: hot rolling the slab after homogenization heat treatment to form a hot-rolled steel plate, and removing the oxide scale on the surface of the hot-rolled steel plate by pickling; wherein, when the slab is hot rolled, the first pass reduction rate of hot rolling rough rolling is 15%; S4: cold rolling the hot-rolled steel sheet at a reduction rate of 80%, and then performing recrystallization heat treatment in an oxygen-free environment to obtain an austenitic stainless steel cold-rolled steel sheet with a bright surface; wherein the recrystallization heat treatment is performed in an annealing furnace at a temperature of 1120°C, and after annealing, the steel sheet is cooled to below 200°C at a cooling rate of 25°C / S; The yield strength of the austenitic stainless steel cold-rolled steel plate is 298 MPa; The tensile strength of the austenitic stainless steel cold-rolled steel plate is 642MPa; The elongation of the austenitic stainless steel cold-rolled steel sheet is 57%; The pitting potential of the austenitic stainless steel cold-rolled steel sheet is 718 mV.
[0049] Comparative Example 2 A method for manufacturing an austenitic stainless steel cold-rolled steel plate comprises the following steps: S1: Casting the molten steel after roughing and refining into a slab, the chemical composition of the slab comprises, by weight percentage, C: 0.030%, Si: 0.80%, Mn: 0.53%, Cr: 19.5%, Ni: 10.0%, Cu: 1.0%, Mo: 1.00%, N: 0.250%, the rest is Fe and other inevitable impurities, and the MY value is 145, the MT value is 220, and the PREN value is 29.8; S2: subjecting the slab to homogenization heat treatment, wherein the homogenization heat treatment is carried out in a heating furnace, the slab is heated in the heating furnace for 180 minutes, the furnace temperature of the heating furnace is controlled at 1260° C., and the furnace temperature of the heating furnace is not lower than 1220° C. and not higher than the Td temperature value of 1452° C.; S3: hot rolling the slab after homogenization heat treatment to form a hot-rolled steel plate, and removing the oxide scale on the surface of the hot-rolled steel plate by pickling; wherein, when the slab is hot-rolled, the first pass reduction rate of hot rolling rough rolling is 18%; S4: The hot-rolled steel sheet is cold rolled at a reduction rate of 77%, and then recrystallized in an oxygen environment. After cooling, the steel sheet is pickled to remove the surface oxide scale, thereby obtaining an austenitic stainless steel cold-rolled steel sheet with a bright surface. The recrystallization heat treatment is carried out in an annealing furnace at a temperature of 1150°C. After annealing, the steel sheet is cooled to below 200°C at a cooling rate of 25°C / S. The yield strength of the austenitic stainless steel cold-rolled steel plate is 544 MPa; The tensile strength of the austenitic stainless steel cold-rolled steel plate is 805MPa; The elongation of the austenitic stainless steel cold-rolled steel sheet is 38%; The pitting potential of the austenitic stainless steel cold-rolled steel sheet is 924 mV.
[0050] Comparative Example 3 A method for manufacturing an austenitic stainless steel cold-rolled steel plate comprises the following steps: S1: Casting the molten steel after roughing and refining into a slab, the chemical composition of the slab comprises, by weight percentage, C: 0.018%, Si: 0.92%, Mn: 0.88%, Cr: 20.6%, Ni: 9.1%, Cu: 0.9%, Mo: 0.62%, N: 0.150%, the rest is Fe and other inevitable impurities, and the MY value is 47, the MT value is 148, and the PREN value is 26.3; S2: subjecting the slab to homogenization heat treatment, wherein the homogenization heat treatment is carried out in a heating furnace, the slab is heated in the heating furnace for 220 minutes, the furnace temperature of the heating furnace is controlled at 1240° C., and the furnace temperature of the heating furnace is not lower than 1220° C. and not higher than the Td temperature value of 1247° C.; S3: hot rolling the slab after homogenization heat treatment to form a hot-rolled steel plate, and removing the oxide scale on the surface of the hot-rolled steel plate by pickling; wherein, when the slab is hot rolled, the first pass reduction rate of hot rolling rough rolling is 17%; S4: The hot-rolled steel sheet is cold rolled at a reduction rate of 77%, and then recrystallized in an oxygen environment. After cooling, the steel sheet is pickled to remove the surface oxide scale, thereby obtaining an austenitic stainless steel cold-rolled steel sheet with a bright surface. The recrystallization heat treatment is carried out in an annealing furnace at a temperature of 1180°C. After annealing, the steel sheet is cooled to below 200°C at a cooling rate of 30°C / S. The yield strength of the austenitic stainless steel cold-rolled steel plate is 292 MPa; The tensile strength of the austenitic stainless steel cold-rolled steel plate is 588MPa; The elongation of the austenitic stainless steel cold-rolled steel sheet is 62%; The pitting potential of the austenitic stainless steel cold-rolled steel sheet is 545 mV.
[0051] Comparative Example 4 A method for manufacturing an austenitic stainless steel cold-rolled steel plate comprises the following steps: S1: Casting the molten steel after roughing and refining into a slab, the chemical composition of the slab comprises, by weight percentage, C: 0.052%, Si: 0.45%, Mn: 0.82%, Cr: 19.8%, Ni: 9.3%, Cu: 1.2%, Mo: 0.80%, N: 0.240%, the rest is Fe and other inevitable impurities, and the MY value is 139, the MT value is 217, and the PREN value is 28.8; S2: subjecting the slab to homogenization heat treatment, wherein the homogenization heat treatment is carried out in a heating furnace, the slab is heated in the heating furnace for 210 minutes, the furnace temperature of the heating furnace is controlled at 1260° C., and the furnace temperature of the heating furnace is not lower than 1220° C. and not higher than the Td temperature value of 1431° C.; S3: hot rolling the slab after homogenization heat treatment to form a hot-rolled steel plate, and removing the oxide scale on the surface of the hot-rolled steel plate by pickling; wherein, when the slab is hot rolled, the first pass reduction rate of hot rolling rough rolling is 13%; S4: cold rolling the hot-rolled steel sheet at a reduction rate of 64%, and then performing recrystallization heat treatment in an oxygen-free environment to obtain an austenitic stainless steel cold-rolled steel sheet with a bright surface; wherein the recrystallization heat treatment is performed in an annealing furnace at a temperature of 1120°C, and after annealing, the steel sheet is cooled to below 200°C at a cooling rate of 28°C / S; The yield strength of the austenitic stainless steel cold-rolled steel plate is 528 MPa; The tensile strength of the austenitic stainless steel cold-rolled steel plate is 806MPa; The elongation of the austenitic stainless steel cold-rolled steel sheet is 37%; The pitting potential of the austenitic stainless steel cold-rolled steel sheet is 872 mV.
[0052] Comparative Example 5 A method for manufacturing an austenitic stainless steel cold-rolled steel plate comprises the following steps: S1: Casting the molten steel after roughing and refining into a slab, the chemical composition of the slab comprises, by weight percentage: C: 0.020%, Si: 0.50%, Mn: 1.83%, Cr: 20.2%, Ni: 9.1%, Cu: 0.9%, Mo: 0.55%, N: 0.180%, the rest is Fe and other inevitable impurities, and the MY value is 74, the MT value is 167, and the PREN value is 25.6; S2: subjecting the slab to homogenization heat treatment, wherein the homogenization heat treatment is carried out in a heating furnace, the slab is heated in the heating furnace for 115 minutes, the furnace temperature of the heating furnace is controlled at 1265°C, and the furnace temperature of the heating furnace is not lower than 1220°C and not higher than the Td temperature value of 1321°C; S3: hot rolling the slab after homogenization heat treatment to form a hot-rolled steel plate, and removing the oxide scale on the surface of the hot-rolled steel plate by pickling; wherein, when hot rolling the slab, the first pass reduction rate of hot rolling rough rolling is 21%; S4: cold rolling the hot-rolled steel sheet at a reduction rate of 55%, and then performing recrystallization heat treatment in an oxygen-free environment to obtain an austenitic stainless steel cold-rolled steel sheet with a bright surface; wherein the recrystallization heat treatment is performed in an annealing furnace at a temperature of 1150°C, and after annealing, the steel sheet is cooled to below 200°C at a cooling rate of 30°C / S; The yield strength of the austenitic stainless steel cold-rolled steel plate is 342 MPa; The tensile strength of the austenitic stainless steel cold-rolled steel plate is 684 MPa; The elongation of the austenitic stainless steel cold-rolled steel sheet is 55%; The pitting potential of the austenitic stainless steel cold-rolled steel sheet is 498 mV.
[0053] Comparative Example 6 A method for manufacturing an austenitic stainless steel cold-rolled steel plate comprises the following steps: S1: Casting the molten steel after roughing and refining into a slab, the chemical composition of the slab comprises, by weight percentage: C: 0.021%, Si: 0.44%, Mn: 1.00%, Cr: 18.8%, Ni: 8.1%, Cu: 0.7%, Mo: 0.6%, N: 0.178%, the rest is Fe and other inevitable impurities, and the MY value is 77, the MT value is 163, and the PREN value is 25.1; S2: subjecting the slab to homogenization heat treatment, wherein the homogenization heat treatment is carried out in a heating furnace, the slab is heated in the heating furnace for 230 minutes, the furnace temperature of the heating furnace is controlled at 1255°C, and the furnace temperature of the heating furnace is not lower than 1220°C and not higher than the Td temperature value of 1356°C; S3: hot rolling the slab after homogenization heat treatment to form a hot-rolled steel plate, and removing the oxide scale on the surface of the hot-rolled steel plate by pickling; wherein, when the slab is hot-rolled, the first pass reduction rate of hot rolling rough rolling is 16%; S4: The hot-rolled steel sheet is cold rolled at a reduction rate of 64%, and then recrystallized in an oxygen environment. After cooling, it is pickled to remove the surface oxide scale to obtain an austenitic stainless steel cold-rolled steel sheet with a bright surface; wherein the recrystallization heat treatment is carried out in an annealing furnace at a temperature of 1070°C, and after annealing, it is cooled to below 200°C at a cooling rate of 15°C / S; The yield strength of the austenitic stainless steel cold-rolled steel plate is 344 MPa; The tensile strength of the austenitic stainless steel cold-rolled steel plate is 672MPa; The elongation of the austenitic stainless steel cold-rolled steel sheet is 54%; The pitting potential of the austenitic stainless steel cold-rolled steel sheet is 459 mV.
[0054] Comparative Example 7 A method for manufacturing an austenitic stainless steel cold-rolled steel plate comprises the following steps: S1: Casting the molten steel after roughing and refining into a slab, the chemical composition of the slab comprises, by weight percentage, C: 0.023%, Si: 0.46%, Mn: 0.90%, Cr: 23.5%, Ni: 10.8%, Cu: 0.8%, Mo: 0.7%, N: 0.210%, the rest is Fe and other inevitable impurities, and the MY value is 87, the MT value is 196, and the PREN value is 31.2; S2: subjecting the slab to homogenization heat treatment, wherein the homogenization heat treatment is carried out in a heating furnace, the slab is heated in the heating furnace for 250 minutes, the furnace temperature of the heating furnace is controlled at 1240°C, the furnace temperature of the heating furnace is not lower than 1220°C and higher than the Td temperature value of 1216°C; S3: hot rolling the slab after homogenization heat treatment to form a hot-rolled steel plate, and removing the oxide scale on the surface of the hot-rolled steel plate by pickling; wherein, when the slab is hot-rolled, the first pass reduction rate of hot rolling rough rolling is 16%; S4: cold rolling the hot-rolled steel sheet at a reduction rate of 77%, and then performing recrystallization heat treatment in an oxygen-free environment to obtain an austenitic stainless steel cold-rolled steel sheet with a bright surface; wherein the recrystallization heat treatment is performed in an annealing furnace at a temperature of 1080°C, and after annealing, the steel sheet is cooled to below 200°C at a cooling rate of 28°C / S; The yield strength of the austenitic stainless steel cold-rolled steel plate is 378 MPa; The tensile strength of the austenitic stainless steel cold-rolled steel plate is 739 MPa; The elongation of the austenitic stainless steel cold-rolled steel sheet is 52%; The pitting potential of the austenitic stainless steel cold-rolled steel sheet is 1132 mV.
[0055] Comparative Example 8 A method for manufacturing an austenitic stainless steel cold-rolled steel plate comprises the following steps: S1: Casting the molten steel after roughing and refining into a slab, the chemical composition of the slab comprises, by weight percentage, C: 0.018%, Si: 0.44%, Mn: 0.95%, Cr: 20.1%, Ni: 9.4%, Cu: 0.6%, Mo: 0.13%, N: 0.172%, the rest is Fe and other inevitable impurities, and the MY value is 65, the MT value is 158, and the PREN value is 24.7; S2: subjecting the slab to homogenization heat treatment, wherein the homogenization heat treatment is carried out in a heating furnace, the slab is heated in the heating furnace for 200 minutes, the furnace temperature of the heating furnace is controlled at 1250°C, and the furnace temperature of the heating furnace is not lower than 1220°C and not higher than the Td temperature value of 1326°C; S3: hot rolling the slab after homogenization heat treatment to form a hot-rolled steel plate, and removing the oxide scale on the surface of the hot-rolled steel plate by pickling; wherein, when the slab is hot rolled, the first pass reduction rate of hot rolling rough rolling is 15%; S4: The hot-rolled steel sheet is cold rolled at a reduction rate of 75%, and then recrystallized in an aerobic environment. After cooling, the steel sheet is pickled to remove the surface oxide scale, thereby obtaining an austenitic stainless steel cold-rolled steel sheet with a bright surface. The recrystallization heat treatment is carried out in an annealing furnace at a temperature of 1100°C. After annealing, the steel sheet is cooled to below 200°C at a cooling rate of 25°C / S. The yield strength of the austenitic stainless steel cold-rolled steel plate is 323 MPa; The tensile strength of the austenitic stainless steel cold-rolled steel plate is 658 MPa; The elongation of the austenitic stainless steel cold-rolled steel sheet is 61%; The pitting potential of the austenitic stainless steel cold-rolled steel sheet is 423 mV.
[0056] Comparative Example 9 A method for manufacturing an austenitic stainless steel cold-rolled steel plate comprises the following steps: S1: Casting the molten steel after roughing and refining into a slab, the chemical composition of the slab comprises, by weight percentage, C: 0.015%, Si: 0.52%, Mn: 0.30%, Cr: 20.0%, Ni: 9.0%, Cu: 2.2%, Mo: 0.6%, N: 0.180%, the rest is Fe and other inevitable impurities, and the MY value is 73, the MT value is 162, and the PREN value is 27.1; S2: subjecting the slab to homogenization heat treatment, wherein the homogenization heat treatment is carried out in a heating furnace, the slab is heated in the heating furnace for 150 minutes, the furnace temperature of the heating furnace is controlled at 1250° C., and the furnace temperature of the heating furnace is not lower than 1220° C. and not higher than the Td temperature value of 1344° C.; S3: hot rolling the slab after homogenization heat treatment to form a hot-rolled steel plate, and removing the oxide scale on the surface of the hot-rolled steel plate by pickling; wherein, when the slab is hot rolled, the first pass reduction rate of hot rolling rough rolling is 15%; S4: cold rolling the hot-rolled steel sheet at a reduction rate of 73%, and then performing recrystallization heat treatment in an oxygen-free environment to obtain an austenitic stainless steel cold-rolled steel sheet with a bright surface; wherein the recrystallization heat treatment is performed in an annealing furnace at a temperature of 1120°C, and after annealing, the steel sheet is cooled to below 200°C at a cooling rate of 20°C / S; The yield strength of the austenitic stainless steel cold-rolled steel plate is 345 MPa; The tensile strength of the austenitic stainless steel cold-rolled steel plate is 562MPa; The elongation of the austenitic stainless steel cold-rolled steel sheet is 48%; The pitting potential of the austenitic stainless steel cold-rolled steel sheet is 652 mV.
[0057] Comparative Example 10 A method for manufacturing an austenitic stainless steel cold-rolled steel plate comprises the following steps: S1: Casting the molten steel after roughing and refining into a slab, the chemical composition of the slab comprises, by weight percentage, C: 0.021%, Si: 0.49%, Mn: 1.12%, Cr: 17.1%, Ni: 10.1%, Cu: 0.2%, Mo: 2.1%, N: 0.051%, the rest is Fe and other inevitable impurities, and the MY value is 5, the MT value is 98, and the PREN value is 24.4; S2: subjecting the slab to homogenization heat treatment, wherein the homogenization heat treatment is carried out in a heating furnace, the slab is heated in the heating furnace for 180 minutes, the furnace temperature of the heating furnace is controlled at 1250° C., and the furnace temperature of the heating furnace is not lower than 1220° C. and not higher than the Td temperature value of 1421° C.; S3: hot rolling the slab after homogenization heat treatment to form a hot-rolled steel plate, and removing the oxide scale on the surface of the hot-rolled steel plate by pickling; wherein, when the slab is hot-rolled, the first pass reduction rate of hot rolling rough rolling is 16%; S4: The hot-rolled steel sheet is cold rolled at a reduction rate of 66%, and then recrystallized in an oxygen environment. After cooling, it is pickled to remove the surface oxide scale to obtain an austenitic stainless steel cold-rolled steel sheet with a bright surface; wherein the recrystallization heat treatment is carried out in an annealing furnace at a temperature of 1150°C, and after annealing, it is cooled to below 200°C at a cooling rate of 25°C / S; The yield strength of the austenitic stainless steel cold-rolled steel plate is 265 MPa; The tensile strength of the austenitic stainless steel cold-rolled steel plate is 592MPa; The elongation of the austenitic stainless steel cold-rolled steel sheet is 62%; The pitting potential of the austenitic stainless steel cold-rolled steel sheet is 412 mV.
[0058] Comparative Example 11 A method for manufacturing an austenitic stainless steel cold-rolled steel plate comprises the following steps: S1: Casting the molten steel after roughing and refining into a slab, the chemical composition of the slab comprises, by weight percentage, C: 0.112%, Si: 0.43%, Mn: 1.27%, Cr: 16.8%, Ni: 6.8%, Cu: 0.18%, Mo: 0.15%, N: 0.062%, the rest is Fe and other inevitable impurities, and the MY value is 24, the MT value is 110, and the PREN value is 17.9; S2: subjecting the slab to homogenization heat treatment, wherein the homogenization heat treatment is carried out in a heating furnace, the slab is heated in the heating furnace for 210 minutes, the furnace temperature of the heating furnace is controlled at 1255°C, and the furnace temperature of the heating furnace is not lower than 1220°C and not higher than the Td temperature value of 1377°C; S3: hot rolling the slab after homogenization heat treatment to form a hot-rolled steel plate, and removing the oxide scale on the surface of the hot-rolled steel plate by pickling; wherein, when the slab is hot-rolled, the first pass reduction rate of hot rolling rough rolling is 16%; S4: cold rolling the hot-rolled steel sheet at a reduction rate of 75%, and then performing recrystallization heat treatment in an oxygen-free environment to obtain an austenitic stainless steel cold-rolled steel sheet with a bright surface; wherein the recrystallization heat treatment is performed in an annealing furnace at a temperature of 1150°C, and after annealing, the steel sheet is cooled to below 200°C at a cooling rate of 25°C / S; The yield strength of the austenitic stainless steel cold-rolled steel plate is 277 MPa; The tensile strength of the austenitic stainless steel cold-rolled steel plate is 695 MPa; The elongation of the austenitic stainless steel cold-rolled steel sheet is 58%; The pitting potential of the austenitic stainless steel cold-rolled steel sheet is 280 mV.
[0059] Comparative Example 12 A method for manufacturing an austenitic stainless steel cold-rolled steel plate comprises the following steps: S1: Casting the molten steel after roughing and refining into a slab, the chemical composition of the slab comprises, by weight percentage, C: 0.017%, Si: 0.80%, Mn: 0.98%, Cr: 19.5%, Ni: 8.5%, Cu: 0.5%, Mo: 0.98%, N: 0.188%, the rest is Fe and other inevitable impurities, and the MY value is 84, the MT value is 173, and the PREN value is 27.4; S2: subjecting the slab to homogenization heat treatment, wherein the homogenization heat treatment is carried out in a heating furnace, the slab is heated in the heating furnace for 150 minutes, the furnace temperature of the heating furnace is controlled at 1265°C, and the furnace temperature of the heating furnace is not lower than 1220°C and not higher than the Td temperature value of 1317°C; S3: hot rolling the slab after homogenization heat treatment to form a hot-rolled steel plate, and removing the oxide scale on the surface of the hot-rolled steel plate by pickling; wherein, when the slab is hot rolled, the first pass reduction rate of hot rolling rough rolling is 17%; S4: cold rolling the hot-rolled steel sheet at a reduction rate of 75%, and then performing recrystallization heat treatment in an oxygen-free environment to obtain an austenitic stainless steel cold-rolled steel sheet with a bright surface; wherein the recrystallization heat treatment is performed in an annealing furnace at a temperature of 1150°C, and after annealing, the steel sheet is cooled to below 200°C at a cooling rate of 8°C / S; The yield strength of the austenitic stainless steel cold-rolled steel plate is 370 MPa; The tensile strength of the austenitic stainless steel cold-rolled steel plate is 725 MPa; The elongation of the austenitic stainless steel cold-rolled steel sheet is 50%; The pitting potential of the austenitic stainless steel cold-rolled steel sheet is 630 mV.
[0060] In order to more intuitively understand the data changes of each embodiment and comparative example in the present invention, the data of each embodiment and comparative example are explained below in the form of tables. Table 1 lists the chemical composition of the slabs of the embodiments and comparative examples of the present invention; Table 2 lists the processing parameters and performance of the embodiments and comparative examples of the present invention.
[0061]
[0062]
[0063] It can be seen from Table 1 and Table 2 that in Examples 1 to 12, the MY values are all between 70 and 120, the MT values are all above 170, the PREN values are all not less than 27, the yield strength is between 340 and 480 MPa, the tensile strength is not less than 650 MPa, the elongation is not less than 40%, and the pitting potential is not less than 630 mV.
[0064] The calculated values MY of the chemical composition related to Examples 1, 3, 8, 10, and 11 are less than 70, and the yield strength of the products does not meet the design requirements; the calculated values MY of the chemical composition related to Examples 2 and 4 are greater than 120, the yield strength of the products is too high, and the elongation is low; the tensile strength of Examples 3 and 9 is low, which is not conducive to expansion forming; the PREN values of Examples 5, 6, 8, 10, and 11 are low, and the pitting potential is lower than 630mV. Example 7 is hot rolled after being heated in a heating furnace at a temperature above Td. A large number of spindle-shaped cracks appear on the surface after annealing and pickling, which cannot be eliminated after cold rolling; Example 5 has a short heating time and a large reduction rate in the first rolling pass. The first rolling pass is changed to a 13% reduction rate for the first rolling pass due to the large rolling resistance and the equipment overload shutdown; the cooling rate of Example 12 during the recrystallization heat treatment after cold rolling is slow, and the pitting potential is lower than 630mV.
[0065] The advantages of the present invention are: (1) the austenitic stainless steel cold-rolled steel sheet of the present invention has excellent properties of high corrosion resistance, high strength, low cost, and no obvious pore-like surface defects; (2) the manufacturing method of the present invention is easy to implement and low cost, and can manufacture austenitic stainless steel cold-rolled steel sheets with high corrosion resistance, high strength, and no obvious pore-like surface defects. The yield strength of the manufactured austenitic stainless steel cold-rolled steel sheets is between 340 MPa and 480 MPa; the tensile strength is not less than 650 MPa; the elongation is not less than 40%; and the pitting potential is not less than 630 mV.
[0066] The invention is not limited to the embodiments presented above but may vary within the scope of the presented claims.
Claims
1. An austenitic stainless steel cold-rolled steel sheet, characterized in that: The chemical composition of austenitic stainless steel cold-rolled steel sheet includes by weight percentage: C: 0.008-0.030%, Si: 0.3-0.8%, Mn: 0.5-1.0%, Cr: 19.5-22.0%, Ni: 8.5-10.0%, Cu: 0.5-1.5%, Mo: 0.5-1.0%, N: 0.17-0.25%, the rest is Fe and other inevitable impurities, and the chemical composition satisfies the following relationship: 70≤MY≤120; and MT≥170; and PREN≥27; among which: MY=400×(C+2×N)+3.8×Ni+7.7×Mo-5.8×Cr; MT=320×(C+2×N)+2.2×Ni+8.6×Mo+1.1×Cr-2.1×Cu; PREN = Cr+3.3×Mo+30×N-Mn; The yield strength of the austenitic stainless steel cold-rolled steel plate is 340MPa to 480MPa; The tensile strength of the austenitic stainless steel cold-rolled steel plate is not less than 650 MPa; The elongation of the austenitic stainless steel cold-rolled steel sheet is not less than 40%; The pitting potential of the austenitic stainless steel cold-rolled steel sheet is not less than 630 mV.
2. The austenitic stainless steel cold-rolled steel sheet according to claim 1, characterized in that: The Cr content is: 21.0~22.0%.
3. A method for manufacturing austenitic stainless steel cold-rolled steel sheet, characterized in that: The following steps are involved: S1: Casting the molten steel after roughing and refining into a slab, the chemical composition of the slab comprises, by weight percentage: C: 0.008-0.030%, Si: 0.3-0.8%, Mn: 0.5-1.0%, Cr: 19.5-22.0%, Ni: 8.5-10.0%, Cu: 0.5-1.5%, Mo: 0.5-1.0%, N: 0.17-0.25%, the rest is Fe and other inevitable impurities, and the chemical composition satisfies the following relationship: 70≤MY≤120; and MT≥170; and PREN≥27; among which: MY=400×(C+2×N)+3.8×Ni+7.7×Mo-5.8×Cr; MT=320×(C+2×N) +2.2×Ni+8.6×Mo+1.1×Cr-2.1×Cu; PREN = Cr+3.3×Mo+30×N-Mn; S2: subjecting the slab to homogenization heat treatment, wherein the homogenization heat treatment is carried out in a heating furnace, the slab is heated in the heating furnace for at least 120 minutes, the furnace temperature of the heating furnace is not less than 1220°C and is not higher than the Td temperature value represented by formula (1); wherein, Formula (1): Td = 1986 + 695 × C - 41.8 × Si + 4.5 × Mn - 61.4 × Cr + 44.2 × Ni - 4.0 × Mo + 20.9 × Cu + 860 × N; S3: hot rolling the slab after homogenization heat treatment to form a hot-rolled steel plate, and removing the oxide scale on the surface of the hot-rolled steel plate by pickling; S4: cold rolling the hot-rolled steel sheet at a reduction rate of not less than 55%, and then performing a recrystallization heat treatment to obtain an austenitic stainless steel cold-rolled steel sheet; The yield strength of the austenitic stainless steel cold-rolled steel plate is 340MPa to 480MPa; The tensile strength of the austenitic stainless steel cold-rolled steel plate is not less than 650 MPa; The elongation of the austenitic stainless steel cold-rolled steel sheet is not less than 40%; The pitting potential of the austenitic stainless steel cold-rolled steel sheet is not less than 630 mV.
4. The method for manufacturing austenitic stainless steel cold-rolled steel sheet according to claim 3, characterized in that: In S3, when the slab is hot rolled, the first pass reduction ratio of the hot rolling rough rolling is not more than 18%.
5. The method for manufacturing austenitic stainless steel cold-rolled steel sheet according to claim 3 or 4, characterized in that: In S4, the recrystallization heat treatment is carried out in an annealing furnace with a temperature of 1050°C to 1200°C. After annealing, the steel is cooled to below 200°C at a cooling rate of not less than 15°C / S.
6. The method for manufacturing austenitic stainless steel cold-rolled steel sheet according to claim 3, characterized in that: In S4, the recrystallization heat treatment can be carried out in an aerobic environment or in an anaerobic environment; when the recrystallization heat treatment is carried out in an aerobic environment, it is also necessary to undergo pickling after cooling to remove the surface oxide scale to obtain an austenitic stainless steel cold-rolled steel plate with a bright surface; when the recrystallization heat treatment is carried out in an anaerobic environment, an austenitic stainless steel cold-rolled steel plate with a bright surface is obtained.
Citation Information
Patent Citations
Austenitic antibiotic stainless steel and method for manufacturing same
CN101230438A
Nonmagnetic austenitic stainless steel and manufacturing method therefor
CN113015817A
Austenitic stainless steel plate strip and manufacturing method thereof
CN118326282A
Cited By
Ultralow-carbon-nitrogen high-copper austenitic stainless steel and cold-rolled steel strip and manufacturing method thereof
CN120330598A