Ultralow-loss annealing method for precious metal alloy material

By using high-purity hydrogen and strictly controlled vacuum and temperature conditions during the annealing of precious metal alloy materials, the problem of oxide scale of precious metal alloy materials is solved, and a low-loss annealing method is achieved, reducing production costs.

CN119061337APending Publication Date: 2024-12-03GEMCH MATERIAL TECH SUZHOU
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411103880.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Precious metal alloy materials are prone to oxidation and peeling during the annealing process, resulting in high losses and high purification costs.

Method used

An annealing method including preparing precious metal alloy materials, locking and sealing in a metal chamber, evacuating vacuum, passing high-purity hydrogen, heating and insulation, and cooling is adopted. The specific steps include a vacuum degree less than 0.01Pa and a hydrogen purity greater than 99.999 %, the heating rate is greater than 500℃/H, the insulation time is 30 to 200 minutes, and the cooling rate is greater than 100℃/H.

Benefits of technology

Effectively reduce or eliminate the scale of precious metal alloy materials and reduce production costs.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses an ultralow-loss annealing method for a precious metal alloy material, relates to the field of film plating, and aims to solve the problem of high loss during annealing of the precious metal alloy material.The ultralow-loss annealing method for the precious metal alloy material is characterized by comprising the following steps that S1, the precious metal alloy material is prepared; s2, the precious metal alloy material in the S1 is placed in a metal cavity, and locking and sealing are conducted; s3, the cavity in the S2 is subjected to vacuum pumping; s4, high-purity hydrogen is introduced into the cavity in the S3; s5, the cavity in the S4 is subjected to temperature rise heating and heat preservation; s6, the cavity in the S5 is cooled; and S7, the cavity in the step S6 is disassembled, and the precious metal alloy material is taken out. The ultralow-loss annealing method for the precious metal alloy material is low in loss and meets the grain requirement.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of film coating, and more particularly to an ultra-low loss annealing method for a noble metal alloy material. Background Art

[0002] There are many kinds of precious metal targets, the most common ones are gold, silver, platinum, palladium and rhodium, and their thin film properties are usually relatively simple.

[0003] In pursuit of excellent comprehensive performance of thin films, precious metal alloy targets came into being. In addition to controlling quality specifications, the difficulty in making precious metal targets is also the control of low loss. Grain size is a core indicator of the target material. When coating, small and uniform grains can often obtain good thin films. The commonly used method to control grains is deformation and annealing process. Because precious metal alloy targets do not have the strong antioxidant ability of single precious metals, oxidation and even peeling will occur during the annealing process. These oxide scales are difficult to collect and the purification cost is high.

[0004] Therefore, a new solution needs to be proposed to solve this problem. Summary of the invention

[0005] In view of the shortcomings of the prior art, the purpose of the present invention is to provide an ultra-low loss annealing method for precious metal alloy materials, which can effectively solve the loss problem and meet the grain requirements at the same time.

[0006] The above technical objectives of the present invention are achieved through the following technical solutions: A method for ultra-low loss annealing of precious metal alloy materials, comprising the following steps:

[0007] S1: prepare precious metal alloy materials;

[0008] S2: placing the precious metal alloy material described in S1 in the metal chamber and locking and sealing it;

[0009] S3: evacuating the chamber described in S2;

[0010] S4: introducing high-purity hydrogen into the chamber described in S3;

[0011] S5: heating the chamber described in S4 and keeping it warm;

[0012] S6: Cooling down the chamber described in S5;

[0013] S7: Disassemble the chamber described in S6 and take out the precious metal alloy material.

[0014] The present invention is further configured as follows: the noble metal alloy material includes a main component noble metal, and the noble metal includes gold, silver, platinum, palladium, and rhodium.

[0015] The present invention is further configured as follows: the noble metal alloy material also includes a main component of non-noble metals, and the non-noble metals include copper, aluminum, nickel, iron, and zirconium.

[0016] The present invention is further configured as follows: in S3, the vacuum degree of the evacuation is <0.01Pa.

[0017] The present invention is further configured such that: in S4, the purity of hydrogen is >99.999%.

[0018] The present invention is further configured as follows: in S5, the heating rate is >500°C / H.

[0019] The present invention is further configured as follows: in S5, the heat preservation time is 30 to 200 minutes.

[0020] The present invention is further configured as follows: in S6, the cooling rate is >100°C / H.

[0021] In summary, the present invention has the following beneficial effects: reducing or even eliminating the oxide scale that may appear on the precious metal alloy material during the annealing process, thereby reducing the production cost of the precious metal alloy material. DETAILED DESCRIPTION

[0022] The present invention is described in detail below in conjunction with embodiments.

[0023] The present invention provides an ultra-low loss annealing method for a precious metal alloy material, comprising the following steps:

[0024] S1: Prepare precious metal alloy materials, the main precious metal components include gold, silver, platinum, palladium, rhodium, etc., but are not limited to these, and the main non-precious metal components include Cu, Al, Ni, Fe, Zr, etc., but are not limited to these.

[0025] S2: Place the precious metal alloy material described in S1 into the metal chamber and lock and seal it.

[0026] S3: Evacuate the chamber described in S2 to a vacuum degree of <0.01Pa.

[0027] S4: High-purity hydrogen is introduced into the chamber described in S3, and the purity of the hydrogen is >99.999%.

[0028] S5: The chamber described in S4 is heated and kept warm, with a heating rate of >500°C / H and a keeping time of 30 to 200 minutes.

[0029] S6: Cooling the chamber described in S5, with a cooling rate of >100°C / H.

[0030] S7: Disassemble the S6 chamber and take out the precious metal alloy material.

[0031] The following is a specific plan:

[0032] Embodiment 1:

[0033] S1: Prepare a precious metal alloy material, the alloy composition is AuCu80wt%, and the purity is 99.99%.

[0034] S2: Place the precious metal alloy material described in S1 in the metal chamber and lock and seal it.

[0035] S3: Evacuate the chamber described in S2 to a vacuum degree of 0.005 Pa.

[0036] S4: High-purity hydrogen is introduced into the chamber described in S3, and the purity of the hydrogen is >99.999%.

[0037] S5: The chamber described in S4 is heated and kept warm, with a heating rate of 800°C / H and a holding time of 90 minutes.

[0038] S6: Cool down the chamber in S5 at a cooling rate of 400°C / H.

[0039] S7: Disassemble the S6 chamber and take out the precious metal alloy material.

[0040] Embodiment 2:

[0041] S1: Prepare a precious metal alloy material, the alloy composition is AuAgCu50wt%, and the purity is 99.99%.

[0042] S2: Place the precious metal alloy material described in S1 in the metal chamber and lock and seal it.

[0043] S3: Evacuate the chamber described in S2 to a vacuum degree of 0.001 Pa.

[0044] S4: High-purity hydrogen is introduced into the chamber described in S3, and the purity of the hydrogen is >99.999%.

[0045] S5: The chamber described in S4 is heated and kept warm, with a heating rate of 600°C / H and a holding time of 60 minutes.

[0046] S6: Cool down the chamber in S5 at a cooling rate of 300°C / H.

[0047] S7: Disassemble the S6 chamber and take out the precious metal alloy material.

[0048] The precious metal alloy materials obtained in the above-mentioned Examples 1 and 2 were observed to see whether they had oxide scales, and the results were shown in Table 1 below:

[0049] Table 1:

[0050] Case Oxide scale condition Example 1 none Example 2 none

[0051] It can be concluded that the annealing method of the present invention can reduce or even eliminate the oxide scale that may appear on the precious metal alloy material during the annealing process, thereby reducing the production cost of the precious metal alloy material.

[0052] The above is only a preferred embodiment of the present invention, and the protection scope of the present invention is not limited to the above embodiments. All technical solutions under the concept of the present invention belong to the protection scope of the present invention. It should be pointed out that for ordinary technicians in this technical field, some improvements and modifications without departing from the principle of the present invention should also be regarded as the protection scope of the present invention.

Claims

1. An ultra-low loss annealing method for precious metal alloy materials, characterized in that: The following steps are involved: S1: prepare precious metal alloy materials; S2: placing the precious metal alloy material described in S1 in the metal chamber and locking and sealing it; S3: evacuating the chamber described in S2; S4: introducing high-purity hydrogen into the chamber described in S3; S5: heating the chamber described in S4 and keeping it warm; S6: Cooling down the chamber described in S5; S7: Disassemble the chamber described in S6 and take out the precious metal alloy material.

2. The ultra-low loss annealing method of a precious metal alloy material according to claim 1, characterized in that: The noble metal alloy material includes a main component noble metal, and the noble metal includes gold, silver, platinum, palladium, and rhodium.

3. The ultra-low loss annealing method of a precious metal alloy material according to claim 1 or 2, characterized in that: The noble metal alloy material also includes a main component of non-noble metals, and the non-noble metals include copper, aluminum, nickel, iron, and zirconium.

4. The ultra-low loss annealing method of a precious metal alloy material according to claim 1, characterized in that: In S3, the vacuum degree of evacuation is <0.01Pa.

5. The ultra-low loss annealing method of a precious metal alloy material according to claim 1, characterized in that: In S4, the hydrogen purity is >99.999%.

6. The ultra-low loss annealing method of a precious metal alloy material according to claim 1, characterized in that: In S5, the heating rate is >500°C / H.

7. The ultra-low loss annealing method of a precious metal alloy material according to claim 1 or 6, characterized in that: In S5, the heat preservation time is 30 to 200 minutes.

8. The ultra-low loss annealing method of a precious metal alloy material according to claim 1, characterized in that: In S6, the cooling rate is >100°C / H.