Production method of corrosion-resistant hot-dip coating steel strip and substrate for CX-grade extreme environment corrosion-resistant pre-coated steel strip

By cleaning and heat treatment of the steel strip, Al-Zn-Mg alloy coating is used to solve the problems of coating adhesion and impurities, significantly improve the corrosion resistance, extend the service life of the steel strip and reduce production costs.

CN119061338APending Publication Date: 2024-12-03浙江华普新材股份有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411202290.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The prior art is difficult to manufacture corrosion-resistant hot-dip plated steel strips in CX-level extreme corrosion environments, resulting in insufficient service life of the steel strips. The main reasons are poor adhesion between the plating and steel substrates, thick coating structure and high internal impurities content, resulting in electricity. Occasional corrosion problems.

Method used

By performing surface cleaning, heating and reducing treatment on the steel strip, the purification and protection of the plating bath melt is controlled, and the grain size and oxide film thickness of the plating layer are controlled to reduce the impurity content inside the plating layer. Form a hot-dip coating with good adhesion.

Benefits of technology

It significantly improves the corrosion resistance of the coating, extends the service life of the steel strip, can be used in CX-class extreme environments for more than 25 years, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005018125460000061
    Figure BDA0005018125460000061
  • Figure BDA0005018125460000071
    Figure BDA0005018125460000071
  • Figure BDA0005018125460000091
    Figure BDA0005018125460000091
Patent Text Reader

Abstract

The invention relates to the technical field of continuous coating of steel strips, and particularly discloses a production method of a corrosion-resistant hot-dip coating steel strip and a substrate for a CX-grade extreme environment corrosion-resistant pre-coated steel strip. According to the method, good conditions are provided for formation of the hot-dip coating by controlling parameters such as the oil stain content and the iron powder content on the surface of the steel strip, and then the forming effect of the coating is improved by optimizing the dust content and the iron content of the plating bath melt, the thickness of an oxidation film below an air knife and the type of the plating bath melt. After being treated by the method disclosed by the invention, the obtained hot-dip coating steel strip has better resistance to electrochemical corrosion, is suitable for working for a long time in a CX-grade extreme environment, and overcomes the defects in related technologies.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of continuous coating of steel strips, and more specifically, to a method for producing corrosion-resistant hot-dip coated steel strips and a substrate for pre-coated steel strips resistant to CX-level extreme environmental corrosion. Background Art

[0002] Pre-coated hot-dip coated steel strip, also known as color-coated steel strip, is an advanced steel material that is further pre-coated after hot-dip coating on the steel strip substrate. This material can significantly extend the service life of the steel strip due to its excellent corrosion resistance. In some cases, it can increase the service life of the steel strip from 3 to 5 years to 25 to 30 years. Therefore, it is widely used in scenes with environmental levels 5 and below. With the intensification of environmental pollution, the demand for steel strips that can be used in CX-level extreme corrosion environments in many fields such as coastal construction, animal husbandry, prefabricated buildings and 5G base stations is increasing, but the current technical level has not yet fully met this demand.

[0003] In the related art, there is a corrosion-resistant treatment process for steel, which includes the following steps: (1) annealing the steel substrate in a reducing atmosphere at 720°C, and then cooling the steel substrate to 560°C; (2) immersing the 560°C steel substrate in a plating solution, spraying it with an air knife after immersion, and then cooling it to room temperature to obtain a steel strip with a coating, and further coating the coated steel strip as a substrate to obtain a pre-coated hot-dip coated steel strip.

[0004] Both theory and practice show that the method of improving the corrosion resistance of the coating by simply improving the coating composition and coating adhesion cannot fully meet the needs of producing CX-level extreme environment resistant pre-coated film substrates under current conditions, and the production cost is very high. The fundamental reason for the above situation is that the adhesion between the coating and the steel is poor, and microcracks will appear in the subsequent processing process. The corrosive medium in the environment can enter the microcracks and cause galvanic corrosion between the steel substrate and the coating; second, due to the coarse coating structure, there is relatively serious galvanic corrosion between different structures inside the coating; third, due to the high impurity content inside the coating, there is relatively serious galvanic corrosion between the coating structure and the impurities. It is precisely because of the above three reasons that the corrosion resistance of the entire coating and coating is affected.

[0005] Regarding the above-mentioned related technologies, the inventors believe that although the treatment in the related technologies has improved the corrosion resistance of steel to a certain extent, in the CX-level extreme corrosion environment, the steel strips treated with anti-corrosion according to this process still face the problem of insufficient service life. Summary of the invention

[0006] In the related art, the steel strips that have undergone anti-corrosion treatment still face the problem of insufficient service life in CX-level extreme corrosion environments. In order to improve this defect, the present application provides a method for producing corrosion-resistant hot-dip coated steel strips and a substrate for pre-coated steel strips resistant to CX-level extreme environmental corrosion. The basic principles are: first, to maximize the bonding strength between the coating and the steel substrate so that the steel substrate will not produce microcracks during processing and use; second, to prevent the coarsening of the primary aluminum-rich phase and the segregation of the magnesium component, and to reduce the galvanic corrosion between different phases of the coating structure; third, to reduce the impurity content inside the coating, and to reduce the galvanic corrosion between the coating structure and the impurities.

[0007] In a first aspect, the present application provides a method for producing a corrosion-resistant hot-dip coated steel strip, which adopts the following technical solution: A method for producing a corrosion-resistant hot-dip coated steel strip comprises the following steps: (1) The raw material steel strip for hot dip galvanizing is subjected to surface cleaning treatment to obtain a surface oil content of 0.5-5 mg / m 2 The cleaning method in the surface cleaning process includes pickling or alkali cleaning; (2) The clean steel strip is heated and reduced, and the surface is purged with nitrogen to obtain a surface dust content of 0.5-3 mg / m 2 Dust removal steel belt; (3) The gas in the furnace nose before the steel strip enters the coating bath is purified to ensure that the dust content on the surface of the coating bath melt within the furnace nose opening is 0.5-3 mg / m 2 , the thickness of the oxide film is 0.001-0.01μm; the plating bath melt is purified and iron is removed, so that the iron content of the plating bath melt is 0.01-0.03wt%; the entire plating bath surface is protected by nitrogen, so that the thickness of the oxide film at the steel strip exiting the plating bath, that is, below the air knife, is 0.01-0.03μm; the plating bath melt is an Al-Zn-Mg alloy melt; (4) immersing the steel strip in a plating bath melt for hot dip plating, so that the surface of the steel strip is plated with liquid Al-Zn-Mg alloy; (5) Use nitrogen to blow away excess liquid Al-Zn-Mg alloy on the surface of the steel strip, leaving the required amount of liquid coating; (6) Atomized water is used to cool and solidify the liquid coating on the surface of the steel strip to obtain a continuously hot-dip coated steel strip.

[0008] By adopting the above technical scheme, first, the present application performs a special cleaning treatment on the surface of the raw material steel strip in step (1) to control the oil content on the surface of the steel strip. Then, the present application further removes the dust attached to the surface by heating and reducing treatment and nitrogen purging in step (2), and provides a clean and uniform base surface through oil removal and dust removal, thereby laying a good foundation for forming a hot-dip coating with good adhesion. Afterwards, the present application controls the dust content on the surface of the Al-Zn-Mg melt plating bath and the thickness of the magnesium and aluminum oxide films under the air knife. By controlling the above parameters, the prepared alloy coating has smaller grains, so it is not easy to have a coarse primary aluminum-rich phase and magnesium component segregation, which helps to reduce the galvanic corrosion between the coating structures and maximize the corrosion resistance of the Al-Zn-Mg alloy coating. At the same time, the control of the above conditions also reduces the content of impurities such as iron in the coating, weakening the galvanic corrosion between the coating structure and the impurities. After being treated by the method of the present application, the obtained hot-dip coated steel strip has good resistance to electrochemical corrosion, and is suitable as a hot-dip coated steel strip substrate for pre-coated films working for a long time in CX-level extreme environments, overcoming the defects in related technologies.

[0009] Preferably, in step (1) of the method, the raw material steel strip used is a hot-rolled steel strip or a cold-rolled hardened steel strip.

[0010] By adopting the above technical solution, when hot-rolled steel strip or cold-rolled hardened steel strip is selected, the hot-dip coated steel strip obtained after being processed by the above method can produce products of different thicknesses to meet different uses.

[0011] Preferably, in step (1) of the method, when the raw material steel strip is a hot-rolled steel strip, the cleaning method in the surface cleaning process is pickling, followed by flattening treatment; when the raw material steel strip is a cold-rolled steel strip, the cleaning method in the surface cleaning process is electrolytic degreasing, followed by ultrasonic alkaline washing.

[0012] By adopting the above-mentioned technical scheme, the present application selects appropriate surface cleaning methods according to the different characteristics of hot-rolled steel strip and cold-rolled hardened steel strip, so that the surface of the steel strip is cleaner, which provides better conditions for improving the adhesion of the coating and helps to improve the corrosion resistance of the hot-dip coated steel strip.

[0013] Preferably, in step (1) of the method, when the raw material steel strip is a hot-rolled steel strip, the surface roughness Ra of the clean steel strip obtained after flattening treatment is 0.1-1.0 μm.

[0014] By adopting the above technical scheme, the present application limits the roughness range of the steel strip before hot-dip plating, ensures the flatness of the steel strip, makes the surface of the steel strip smoother, is conducive to forming a uniform and dense coating, reduces galvanic corrosion between different structures of the coating, and improves the corrosion resistance of the coated plate.

[0015] Preferably, in step (1) of the method, the iron powder content on the surface of the clean steel strip obtained is 0.5-3 mg / m 2 .

[0016] By adopting the above technical scheme, the present application controls the iron powder content on the surface of the steel strip before hot-dip plating, reduces impurities generated inside the coating due to iron powder, is beneficial to reducing galvanic corrosion between the coating and impurities, and improves the corrosion resistance of the coated plate.

[0017] Preferably, in step (2) of the method, when the raw material steel strip is a hot-rolled steel strip, heat treatment of material properties is not performed, but only heating to the temperature required for hot-dip plating is performed for reduction treatment; when the raw material steel strip is a cold-rolled hardened steel strip, heat treatment of material properties is performed, that is, after heating to the austenite zone, the strip is kept warm for a period of time, and then cooled to the temperature required for hot-dip plating, and reduction treatment is performed at the same time.

[0018] By adopting the above technical scheme, the present application designs different heat treatment strategies according to the characteristics of hot-rolled steel strip and cold-rolled hardened steel strip, which helps to improve the processing performance of the material, reduce the uneven deformation of the coated plate during the processing, and improve the corrosion resistance of the coated plate.

[0019] Preferably, in step (2) of the method, the iron powder content on the surface of the dust-removing steel belt is 0.5-2 mg / m 2 , the oxide film thickness is 0.0005-0.001μm.

[0020] By adopting the above-mentioned technical scheme, the present application limits the iron powder content and the thickness of the oxide film on the surface of the dust-removed steel strip. On the one hand, it reduces the impurities generated by the iron powder remaining on the surface of the steel strip and reduces the galvanic corrosion between the coating and the impurities. On the other hand, it improves the adhesion between the coating and the steel substrate after hot-dip plating and improves the corrosion resistance of the coated plate.

[0021] Preferably, in step (4) of the method, the temperature difference between the steel strip and the coating bath melt is controlled to be 0.1-0.5°C.

[0022] By adopting the above technical solution, the present application limits the temperature difference between the steel strip and the plating bath molten liquid, helps to form a uniform and dense coating, reduces galvanic corrosion between different structures of the coating, and improves the corrosion resistance of the steel strip.

[0023] Preferably, in step (5) of the method, the thickness of the oxide film on the surface of the coating is controlled to be 0.01-0.05 μm.

[0024] By adopting the above-mentioned technical scheme, since the scheme of the present application can give full play to the corrosion resistance of the Al-Zn-Mg alloy coating, a relatively dense oxide film can be obtained on the surface of the coating. When the thickness of the oxide film on the surface of the coating is within the above-mentioned range, the oxidation segregation of magnesium can be reduced, the uniformity of the coating structure can be improved, the galvanic corrosion between different structures of the coating can be reduced, and good corrosion resistance can be achieved.

[0025] In a second aspect, the present application provides a substrate for a pre-coated steel strip that is resistant to CX-level extreme environmental corrosion, and adopts the following technical solution.

[0026] A substrate for a pre-coated steel strip resistant to CX-level extreme environmental corrosion, wherein the hot-dip coated steel strip is processed by any of the above methods.

[0027] By adopting the above technical scheme, the present application fully improves the corrosion resistance of the hot-dip coated steel strip, can control the grain size in the coating to 0.2 mm or less, is not prone to falling off or cracking when using a 36J absorption energy impact specimen to test the adhesion of the coating, can also fully reduce the impurity content in the coating, and can control the thickness of the oxide film on the surface of the coating to 0.05 μm or less.

[0028] In summary, this application has the following beneficial effects: 1. First, the present application controls the oil content on the surface of the steel strip, and provides a clean and uniform base surface through oil removal and dust removal, which can form a hot-dip coating with excellent adhesion. When the coating adhesion is tested using a 36J absorption energy impact test specimen, the coated steel strip prepared in the present application is not prone to falling off or cracking.

[0029] 2. The present application reduces the impurity content inside the coating, weakens the galvanic corrosion between the coating structure and the impurities, can also fully reduce the impurity content in the coating, and can control the thickness of the oxide film on the coating surface to 0.05 μm or less.

[0030] 3. The present application controls the dust content on the surface of the Al-Zn-Mg melt plating bath, the impurities and iron content of the plating bath melt, and the thickness of the magnesium and aluminum oxide films under the air knife, so that the prepared alloy coating has smaller grains. The grain size in the coating can be controlled to 0.2 mm or less, and the primary aluminum-rich phase is not prone to coarseness and magnesium component segregation. This helps to reduce galvanic corrosion between the coating structures and maximize the corrosion resistance of the Al-Zn-Mg alloy coating.

[0031] In summary, the coated steel sheets produced by taking the above measures have overcome the defects in the relevant technologies, and the obtained hot-dip coated steel strips have good resistance to electrochemical corrosion. According to the requirements of "GB / T 10125-2012 Artificial Atmosphere Corrosion Test Salt Spray Test", the coated steel strips were subjected to copper accelerated acetate spray test, and the time for red rust to appear (referred to as corrosion time) was greater than 800 hours. Correspondingly, after further coating treatment using this coated steel strip as the substrate, the theoretical service life can reach more than 25 years in the CX level extreme environment. DETAILED DESCRIPTION

[0032] The present application is further described in detail below in conjunction with examples and comparative examples. The raw materials involved in the present application can all be obtained commercially. Example

[0033] The following description is given by taking Example 1 as an example.

[0034] Example 1 This embodiment provides a method for producing a corrosion-resistant hot-dip coated steel strip, comprising the following steps: (1) Select Q235 hot-rolled steel strip as the raw material steel strip, and clean the surface of the raw material steel strip to obtain a surface oil content of 5 mg / m 2 , iron powder content is 3mg / m 2 , a clean steel strip with a surface roughness of 1.0 μm; in this step, the specific method of surface cleaning treatment is: first use 1wt% hydrochloric acid to pickle the raw material steel strip, and then use a working roll with a surface roughness of 0.5 μm to level it under a pressure of 1000 tons; (2) When the oxygen content is 4.5PPM and the PM2.5 content is 1.8μg / m 3 The clean steel strip was reduced in a furnace and the surface of the steel strip was purged with high pressure nitrogen with a dew point of -60°C to obtain a surface dust content of 3 mg / m 2 , iron powder content 2mg / m 2 , dust removal steel belt with oxide film thickness of 0.001μm; (3) Prepare the plating bath melt, cool the gas in the furnace nose before the steel strip enters the plating bath, reduce the gas temperature to 350°C, and use micron-level filtration to purify the gas, so that the dust content on the surface of the plating bath melt in the furnace nose is 3 mg / m 2 ; Control the amount of iron dissolved so that the iron content of the plating bath melt is 0.03wt%; The entire plating bath surface is protected by nitrogen with a dew point of -60°C so that the thickness of the oxide film below the air knife is 0.03μm; In this step, the plating bath melt is an Al-Zn-Mg melt, and the specific composition is 55wt%Al+2.0wt%Mg+Zn; (4) immersing the steel strip in a plating bath melt for hot dip plating, and during the hot dip plating, the temperature difference between the steel strip and the plating bath melt is controlled to be 0.5°C; (5) Use nitrogen with a dew point of -60°C to blow away excess plating bath melt on the surface of the steel strip, so that the thickness of the oxide film on the surface of the coating is 0.05 μm; (6) Atomized desalted water is used to cool and solidify the coating on the surface of the steel strip at a cooling rate of 100°C / s to obtain a corrosion-resistant hot-dip coated steel strip.

[0035] This embodiment also provides a substrate for a pre-coated steel strip that is resistant to CX-level extreme environmental corrosion, which is prepared according to the above method.

[0036] The difference between Examples 1-3 is that some process parameters in the production method are different, see Table 1.

[0037] Example 4 This embodiment provides a method for producing a corrosion-resistant hot-dip coated steel strip, comprising the following steps: (1) Select Q235 cold-rolled hardened steel strip as the raw material steel strip, and clean the surface of the raw material steel strip to obtain a surface oil content of 5 mg / m 2 , iron powder content is 3mg / m 2 , a clean steel strip with a surface roughness of 1.0 μm; in this step, the specific method of surface cleaning is: first, at 40A / dm 2 Electrolytic degreasing for 12 seconds under the conditions of , and then ultrasonic alkaline cleaning for 8 seconds, the ultrasonic power is 500W, and the alkaline solution is 1wt% sodium hydroxide solution; (2) When the oxygen content is 4.5PPM and the PM2.5 content is 1.8μg / m 3 The clean steel strip is heated, kept warm, cooled and reduced in a furnace, and the surface of the steel strip is purged with high-pressure nitrogen at a pressure of 1.5 MPa at a speed of 100 m / s to obtain a surface dust content of 3 mg / m 2 , iron powder content 2mg / m 2 , dust removal steel belt with oxide film thickness of 0.001μm; (3) Prepare the plating bath melt, cool the gas in the furnace nose before the steel strip enters the plating bath, reduce the gas temperature to 350°C, and use micron-level filtration to purify the gas, so that the dust content on the surface of the plating bath melt in the furnace nose is 3 mg / m 2 ; Control the amount of iron dissolved so that the iron content of the plating bath melt is 0.03wt%; The entire plating bath surface is protected by nitrogen with a dew point of -60°C so that the thickness of the oxide film below the air knife is 0.03μm; In this step, the plating bath melt is an Al-Zn-Mg melt, and the specific composition is 55wt%Al+2.0wt%Mg+Zn; (4) immersing the steel strip in a plating bath melt for hot dip plating, and during the hot dip plating, the temperature difference between the steel strip and the plating bath melt is controlled to be 0.5°C; (5) Use nitrogen with a dew point of -60°C to blow away excess plating bath melt on the surface of the steel strip, so that the thickness of the oxide film on the surface of the coating is 0.05 μm; (6) Atomized desalted water is used to cool the coating on the surface of the steel strip at a cooling rate of 50°C / s to obtain a corrosion-resistant hot-dip coated steel strip.

[0038] This embodiment also provides a substrate for a pre-coated steel strip that is resistant to CX-level extreme environmental corrosion, which is prepared according to the above method.

[0039] The difference between Examples 4-6 is that some process parameters in the production method are different, see Table 1.

[0040] Table 1 Some process parameters in the production method Example 7 The difference between this embodiment and embodiment 1 is that in step (1) of the method for producing a corrosion-resistant hot-dip coated steel strip, the iron powder content on the surface of the cleaned steel strip is 4 mg / m 2 .

[0041] Example 8 The difference between this embodiment and embodiment 1 is that in step (1) of the method for producing a corrosion-resistant hot-dip coated steel strip, the roughness of the surface of the cleaned steel strip is 1.5 μm.

[0042] Example 9 The difference between this embodiment and embodiment 1 is that in step (2) of the method for producing a corrosion-resistant hot-dip coated steel strip, the iron powder content on the surface of the steel strip is 4 mg / m 2 .

[0043] Example 10 The difference between this embodiment and embodiment 1 is that in step (2) of the method for producing a corrosion-resistant hot-dip coated steel strip, the thickness of the oxide film on the surface of the steel strip is 0.002 μm.

[0044] Embodiment 11 The difference between this embodiment and embodiment 1 is that in step (4) of the method for producing a corrosion-resistant hot-dip coated steel strip, the temperature difference between the steel strip and the coating bath melt is 1°C.

[0045] Example 12 The difference between this embodiment and embodiment 1 is that in step (5) of the method for producing a corrosion-resistant hot-dip coated steel strip, the thickness of the oxide film on the coating surface is 0.1 μm.

[0046] Comparative Example Comparative Example 1 A steel processing process comprises the following steps: (1) A raw material steel strip (Q235 hot-rolled steel strip) with a surface roughness of 1.0 μm was annealed in a reducing atmosphere (85% N2+15% H2) at 720°C, and then the steel was cooled to 560°C; (2) The raw material steel strip at 560°C is immersed in a plating solution with a composition of 5.5wt% Al+2.5wt% Mg+Zn, and after immersion, it is sprayed with an air knife and then cooled to room temperature to obtain a hot-dip coated steel strip with an alloy coating.

[0047] Comparative Example 2 The difference between this comparative example and Example 1 is that in step (1) of the production method of corrosion-resistant hot-dip coated steel strip, the oil content on the surface of the steel strip is 8 mg / m 2 .

[0048] Comparative Example 3 The difference between this comparative example and Example 1 is that in step (2) of the production method of corrosion-resistant hot-dip coated steel strip, the dust content on the surface of the steel strip is 5 mg / m 2 .

[0049] Comparative Example 4 The difference between this comparative example and Example 1 is that in step (3) of the method for producing a corrosion-resistant hot-dip coated steel strip, the dust content on the surface of the coating bath melt is 3.5 mg / m 2 .

[0050] Comparative Example 5 The difference between this comparative example and Example 1 is that in step (3) of the method for producing a corrosion-resistant hot-dip coated steel strip, the thickness of the oxide film on the surface of the coating bath melt is 0.02 μm.

[0051] Comparative Example 6 This comparative example is different from Example 1 in that, in step (3) of the method for producing a corrosion-resistant hot-dip coated steel strip, the iron content of the coating bath melt is 0.5 wt%.

[0052] Comparative Example 7 The difference between this comparative example and Example 1 is that in step (3) of the method for producing a corrosion-resistant hot-dip coated steel strip, the thickness of the oxide film below the air knife is 0.08 μm.

[0053] Performance testing methods 1. Coating adhesion The weighing method is used to detect the coating adhesion on the surface of the hot-dip coated steel strip. The steps are as follows: (1) After hot-dip coating, take a sample and use an electronic balance to measure and record the total weight of the hot-dip coated steel strip substrate and coating; (2) The surface coating is removed by pickling to leave the steel substrate, and the substrate is measured using a balance to measure the weight of the substrate.

[0054] (3) The coating adhesion amount was calculated based on the difference between the two measurement results and the substrate area. The results are shown in Table 2.

[0055] 2. Corrosion resistance Referring to the requirements of GB / T 10125-2012 Artificial atmosphere corrosion test salt spray test, the hot-dip coated steel strip was subjected to a copper accelerated acetate salt spray test, and the time for the appearance of red rust in each group of tests (referred to as corrosion time) was recorded. The results are shown in Table 2.

[0056] Table 2 Combining Examples 1-12 and Comparative Examples 1-7 with Table 2, it can be seen that the coating adhesion of each group of hot-dip coated steel strips in Table 2 is distributed in the range of 500-550 g / m 2 The temperature of each group of hot-dip coated steel strips is within the range of 0.0447 W / m, while the time for red rust to appear in the copper salt accelerated acetic acid spray test is quite different.

[0057] There are three main reasons why comparative examples 1-7 have severe corrosion. First, the adhesion between the coating and the steel is poor, and there are microcracks. The corrosive medium in the test can enter the microcracks and cause galvanic corrosion between the steel substrate and the coating; second, due to the coarse coating structure, there is severe galvanic corrosion between different structures inside the coating; third, due to the high impurity content inside the coating, there is severe galvanic corrosion between the coating structure and the impurities.

[0058] In contrast, the improvements of Examples 1-12 are mainly reflected in three aspects. First, a clean and uniform base surface is provided by degreasing and dust removal, which can form a hot-dip coating with excellent adhesion and not easy to crack, so that the corrosive medium is not easy to invade through the cracks, reducing the occurrence of galvanic corrosion. Second, the dust content on the surface of the Al-Zn-Mg melt bath in the hot-dip furnace nose, the impurities and iron content of the bath melt, and the thickness of the magnesium and aluminum oxide films under the air knife are controlled, so that the prepared alloy coating has smaller grains, and the grain size can be controlled at 0.2 mm or less in the coating. It is not easy to have coarse primary aluminum-rich phases and segregation of magnesium components, which helps to reduce galvanic corrosion between coating structures and maximize the corrosion resistance of the Al-Zn-Mg alloy coating. Third, the impurity content inside the coating is reduced, weakening the galvanic corrosion between the coating structure and the impurities.

[0059] Therefore, the coated steel sheets of Examples 1-12 overcome the defects in the related art, and the obtained hot-dip coated steel strips have a good resistance to electrochemical corrosion. According to the requirements of "GB / T 10125-2012 Artificial Atmosphere Corrosion Test Salt Spray Test", the coated steel strips were subjected to a copper accelerated acetate spray test, and the time for the appearance of red rust (referred to as corrosion time) was greater than 800 hours. Correspondingly, after further coating treatment using the coated steel strip as a substrate, the theoretical service life can reach more than 25 years in a CX-level extreme environment.

[0060] Combining Examples 1-6 and Comparative Example 1 and Table 2, it can be seen that the corrosion time measured in Examples 1-6 is greater than that in Comparative Example 1, indicating that the coated steel strip of the present application is not prone to coarse primary aluminum-rich phases and segregation of magnesium components, which helps to reduce galvanic corrosion between coating structures and maximizes the corrosion resistance of the Al-Zn-Mg alloy coating. At the same time, since the impurity content inside the coating is reduced, the galvanic corrosion between the coating structure and the impurities is also weakened. After being treated by the method of the present application, the obtained hot-dip coated steel strip has a good resistance to electrochemical corrosion, is suitable for long-term work in CX-level extreme environments, and overcomes the defects in the relevant technology.

[0061] Combining Examples 1-6 and Comparative Examples 2-4 and Table 2, it can be seen that the corrosion time measured in Examples 1-6 is greater than that in Comparative Examples 2-4, indicating that in the method of the present application, controlling the dust content and oil content on the surface of the steel strip lays a good foundation for forming a uniform and dense hot-dip coating. The advantage is that the prepared alloy coating has smaller grains, so it is not easy to have coarse primary aluminum-rich phases and segregation of magnesium components, which helps to reduce galvanic corrosion between coating structures and maximize the corrosion resistance of the Al-Zn-Mg alloy coating.

[0062] Combining Examples 1-6 and Comparative Example 5 and Table 2, it can be seen that the corrosion times measured in Examples 1-6 are all greater than those in Comparative Example 5, indicating that in the method of the present application, controlling the thickness of the oxide film on the surface of the coating bath melt helps to improve the corrosion resistance of the hot-dip coated steel strip.

[0063] Combining Examples 1-6 and Comparative Example 6 and Table 2, it can be seen that the corrosion times measured in Examples 1-6 are all greater than those in Comparative Example 6, indicating that in the method of the present application, controlling the iron content of the plating bath melt helps to improve the corrosion resistance of the hot-dip coated steel strip.

[0064] Combining Examples 1-6 and Comparative Example 7 and Table 2, it can be seen that the corrosion times measured in Examples 1-6 are all greater than those in Comparative Example 7, indicating that in the method of the present application, controlling the thickness of the oxide film under the air knife helps to improve the corrosion resistance of the hot-dip coated steel strip.

[0065] It can be seen from Example 1 and Examples 7-10 and Table 2 that in step (1) and step (2), controlling the iron powder content, roughness and oxide film thickness on the surface of the steel strip helps to fully improve the corrosion resistance of the hot-dip coated steel strip. By controlling the oxide film thickness on the surface of the steel strip before hot-dip coating, on the one hand, the impurities generated by the iron powder remaining on the surface of the steel strip are reduced, and the galvanic corrosion between the coating and the impurities is reduced. On the other hand, the adhesion between the coating and the steel substrate after hot-dip coating is improved, and the corrosion resistance of the coated plate is improved. By controlling the iron powder content on the surface of the steel strip, the impurities generated inside the coating due to the iron powder are reduced, which is conducive to reducing the galvanic corrosion between the coating and the impurities and improving the corrosion resistance of the coated plate. By limiting the roughness range of the steel strip before hot-dip coating, the flatness of the steel strip is ensured, which is conducive to forming a uniform and dense coating, reducing the galvanic corrosion between different structures of the coating, and improving the corrosion resistance of the coated plate.

[0066] It can be seen from Example 1 and Example 11 and Table 2 that by controlling the temperature difference between the steel strip and the plating bath melt within a smaller range, it is helpful to form a uniform and dense coating, reduce galvanic corrosion between different structures of the coating, and improve the corrosion resistance of the steel strip.

[0067] It can be seen from Example 1 and Example 12 and Table 2 that since the scheme of the present application can give full play to the corrosion resistance of the Al-Zn-Mg alloy coating, a relatively dense oxide film can be obtained on the surface of the coating. When the thickness of the oxide film on the surface of the coating is in the range of 0.01-0.05 μm, the segregation of magnesium can be reduced, the uniformity of the coating structure is improved, the galvanic corrosion between different structures of the coating is reduced, and good corrosion resistance is achieved.

[0068] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A method for producing a corrosion-resistant hot-dip coated steel strip, It is characterized in that The following steps are involved: (1) The raw material steel strip for hot dip galvanizing is cleaned and the surface oil content is 0.5-5 mg / m 2 The cleaning method in the surface cleaning process includes pickling or alkali cleaning; (2) The clean steel strip is heated and reduced, and the surface is purged with nitrogen to obtain a surface dust content of 0.5-3 mg / m 2 Dust removal steel belt; (3) Prepare the plating bath melt and purify the gas in the furnace nose before the steel strip enters the plating bath, so that the dust content on the surface of the plating bath melt within the furnace nose mouth is 0.5-3 mg / m 2 , the thickness of the oxide film is 0.001-0.01μm; the plating bath melt is purified and iron is removed, so that the iron content of the plating bath melt is 0.01-0.03wt%; the entire plating bath surface is protected by nitrogen, so that the thickness of the oxide film at the steel strip exiting the plating bath, that is, below the air knife, is 0.01-0.03μm; the plating bath melt is an Al-Zn-Mg alloy melt; (4) immersing the steel strip in a plating bath melt for hot dip plating, so that the surface of the steel strip is coated with liquid Al-Zn-Mg alloy; (5) Use nitrogen to blow away excess liquid Al-Zn-Mg alloy on the surface of the steel strip, leaving the required amount of liquid coating; (6) Atomized water is used to cool and solidify the liquid coating on the surface of the steel strip to obtain a continuously hot-dip coated steel strip.

2. The method for producing a corrosion-resistant hot-dip coated steel strip according to claim 1, It is characterized in that In step (1) of the method, the raw material steel strip used is a hot-rolled steel strip or a cold-rolled hardened steel strip.

3. The method for producing a corrosion-resistant hot-dip coated steel strip according to claim 2, It is characterized in that In step (1) of the method, when the raw material steel strip is a hot-rolled steel strip, the cleaning method in the surface cleaning process is pickling, followed by flattening treatment; when the raw material steel strip is a cold-rolled steel strip, the cleaning method in the surface cleaning process is electrolytic degreasing, followed by ultrasonic alkaline cleaning.

4. The method for producing a corrosion-resistant hot-dip coated steel strip according to claim 3, It is characterized in that In step (1) of the method, when the raw material steel strip is a hot-rolled steel strip, the surface roughness Ra of the clean steel strip obtained after flattening treatment is 0.1-1.0 μm.

5. The method for producing a corrosion-resistant hot-dip coated steel strip according to claim 3, It is characterized in that In step (1) of the method, the iron powder content on the surface of the clean steel strip obtained is 0.5-3 mg / m 2 .

6. The method for producing a corrosion-resistant hot-dip coated steel strip according to claim 2, It is characterized in that In step (2) of the method, when the raw material steel strip is a hot-rolled steel strip, no heat treatment of the material properties is performed, but only the steel strip is heated to the temperature required for hot-dip plating and then subjected to reduction treatment; when the raw material steel strip is a cold-rolled hardened steel strip, a heat treatment of the material properties is performed, that is, after being heated to the austenite zone, the steel strip is kept warm for a period of time, and then cooled to the temperature required for hot-dip plating, and a reduction treatment is performed at the same time.

7. The method for producing a corrosion-resistant hot-dip coated steel strip according to claim 6, It is characterized in that In step (2) of the method, the iron powder content on the surface of the dust-removing steel belt is 0.5-2 mg / m 2 , the oxide film thickness is 0.0005-0.001μm.

8. The method for producing a corrosion-resistant hot-dip coated steel strip according to claim 1, It is characterized in that In step (4) of the method, the temperature difference between the steel strip and the coating bath melt is controlled to be 0.1-0.5°C.

9. The method for producing a corrosion-resistant hot-dip coated steel strip according to claim 1, It is characterized in that In step (5) of the method, the thickness of the oxide film on the surface of the coating is controlled to be 0.01-0.05 μm.

10. A substrate for pre-coated steel strip resistant to CX-level extreme environmental corrosion, It is characterized in that The method is processed by any one of claims 1 to 9.