Method for preparing composite wear-resistant coating with core-shell structure through laser cladding assisted by ultrasonic vibration
Through ultrasonic vibration-assisted laser cladding technology, the melting point difference between ceramics and metals and ultrasonic vibrations are used to form a core-shell structure composite coating, which solves the problems of uneven distribution and decomposition of ceramic particles and improves the wear resistance and toughness of the coating.
Patent Information
- Application Number
- CN202411262817.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-10
- Publication Date
- 2024-12-03
AI Technical Summary
Existing laser cladding technology is difficult to effectively control the distribution uniformity of ceramic particles and inhibit their decomposition, resulting in coating defects and cracks.
Ultrasonic vibration-assisted laser cladding technology is adopted to ball mill ceramic powder and metal powder through mechanical ball milling method, laser cladding is performed using the difference in melting points between ceramic and metal, and the ceramic particles are evenly distributed through ultrasonic vibration to form ceramic particles as cores and metals. A composite coating of core-shell structure with a phase shell.
The uniform distribution of ceramic particles and the formation of high-performance coatings are achieved, the wear resistance and toughness of the composite wear-resistant coatings are improved, and the internal stress and crack risks are reduced.
Smart Images

Figure CN119061396A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of laser cladding wear-resistant coatings, and in particular relates to a method for preparing a core-shell structure composite wear-resistant coating by ultrasonic vibration-assisted laser cladding. Background Art
[0002] Wear is one of the main reasons for the failure of materials and workpieces, and is also a major component of energy consumption. It is urgent to seek new wear-resistant materials, so new wear-resistant materials will gradually replace traditional wear-resistant materials in various fields.
[0003] Laser cladding technology offers inherent advantages such as fast melting speed, low cost, high efficiency, good metallurgical bonding with the substrate, and selective local surface treatment (or micro-area processing) of parts. Therefore, the use of laser cladding technology to prepare metal-based composite coatings containing high-melting-point ceramic phases has attracted widespread attention in the field of material surface strengthening. Ceramic particle-reinforced metal-based composites combine many of the excellent properties of the metal matrix and ceramic phase. They possess the high hardness and high strength of ceramics and the good plasticity and toughness of metal materials, making them a hot topic of research among scholars. Although laser cladding technology has successfully produced surface composite materials with excellent wear resistance, laser cladding still faces problems such as the difficulty in controlling the distribution of the ceramic reinforcement phase, the generation of cracks, and the melting of ceramic particles. Although some methods have been explored (including matching process parameters, adjusting the weight percentage of the ceramic phase, preheating the substrate, and adding rare earth elements) to reduce the defect sensitivity of metal-ceramic composite coatings prepared by laser cladding, they do not fundamentally solve the problem.
[0004] During the cladding process, all ceramic particles remain in the liquid melt pool for the duration of the laser beam exposure. Ceramic powders generally have high laser energy absorption and low thermal conductivity. Therefore, during laser irradiation, the edges of the ceramic particles may partially decompose or even completely melt. Upon cooling, these particles may reprecipitate from the alloy liquid or form other ceramic phases, causing internal thermal stress and cracking in the coating. Furthermore, the high surface area of ceramic particles makes them prone to agglomeration, making uniform distribution difficult to achieve during cladding.
[0005] Therefore, it is necessary to develop a laser cladding method that can inhibit the decomposition of ceramic particles during the cladding process and make them uniformly distributed. Summary of the Invention
[0006] The technical problem to be solved by the present invention is to address the deficiencies of the above-mentioned prior art and provide a method for preparing a core-shell composite wear-resistant coating by ultrasonic vibration-assisted laser cladding. This method uses ultrasonic vibration-assisted laser cladding to achieve the fusion of dissimilar materials, inhibit the formation of intermetallic compounds, and uniformly distribute ceramic particles, thereby obtaining a core-shell composite wear-resistant coating with dispersed ceramic particles as the core and a metal phase as the shell. This improves the performance of the composite wear-resistant coating, allowing the coating to combine the high wear resistance of the ceramic phase with the toughness of the metal phase, and solves the problem of ceramic particles being easily decomposed and difficult to evenly distribute in the existing cladding process.
[0007] To solve the above technical problems, the technical solution adopted by the present invention is: a method for preparing a core-shell structure composite wear-resistant coating by ultrasonic vibration-assisted laser cladding, characterized in that the method comprises the following steps:
[0008] Step 1: Screening the ceramic powder;
[0009] Step 2: Place the ceramic powder and metal powder processed by the screen in step 1 into a ball mill, place a diamond ball mill, seal the jar, and ball mill for more than 2 hours, then take out and place in a drying oven for drying to obtain a mixture; the drying temperature is 80° C. and the time is 1 hour to 2 hours;
[0010] Step 3: Clean the surface of the material to be clad and install and position it, and load the mixture obtained in step 2 into the powder feeder of the laser cladding equipment as cladding powder;
[0011] Step 4: Set the laser cladding process parameters including laser power, defocus, scanning speed, powder feeding rate, set the ultrasonic vibration power and frequency, then turn on the laser cladding equipment and ultrasonic vibration device, complete the laser cladding with the assistance of ultrasonic vibration, and form a core-shell structure composite wear-resistant coating on the surface of the material to be clad.
[0012] The present invention first adopts a mechanical ball milling method to ball mill a high-melting-point ceramic powder and a low-melting-point metal powder, and then adopts ultrasonic vibration-assisted laser cladding to prepare a wear-resistant coating on the surface of the material to be clad. In this preparation process, on the one hand, the large difference in melting points between ceramic powder and metal powder is utilized, and a laser cladding process is adopted to make the low-melting-point metal powder melt first to form a molten pool to wrap the unmelted high-melting-point ceramic particles, thereby avoiding the melting of the ceramic particles, and realizing the fusion of dissimilar materials to form a coating through capillary action, thereby maximally suppressing the formation of intermetallic compounds, and avoiding the wear-resistant coating from having a large brittleness and easy cracking tendency; on the other hand, the cavitation effect of ultrasonic vibration is utilized to make the cavitation bubbles in the molten metal generate high-temperature, high-pressure, high-speed microjets in the process of formation and disintegration to stir the molten pool, thereby evenly distributing the ceramic particle reinforcement phase in the wear-resistant coating, ensuring the acquisition of a high-performance composite wear-resistant coating.
[0013] The above-mentioned method for preparing a core-shell structure composite wear-resistant coating by ultrasonic vibration-assisted laser cladding is characterized in that the screen treatment in step 1 uses a -325 mesh screen.
[0014] The above-mentioned method of preparing a core-shell structure composite wear-resistant coating by ultrasonic vibration-assisted laser cladding is characterized in that the ceramic powder in step one is a high-melting-point superhard spherical particle, which is tungsten carbide, titanium carbide, diamond or cubic boron nitride powder with a particle size not exceeding 45 μm.
[0015] The above-mentioned method for preparing a core-shell structure composite wear-resistant coating by ultrasonic vibration-assisted laser cladding is characterized in that the metal powder in step 2 is iron, nickel, cobalt or titanium metal powder with a particle size of more than 100 μm.
[0016] The metal powder used in the present invention has a large particle size and a high absorption rate for laser. Under conditions of laser power lower than that of conventional laser cladding, the large-sized, low-melting-point metal powder melts earlier than the small-sized, high-melting-point ceramic powder, and wraps the ceramic powder to form a shell, while the small-sized ceramic particles are dispersed as nuclei. On the one hand, it can effectively inhibit the melting of ceramic particles, prevent the formation of intermetallic compounds, reduce the internal stress generated during the coating formation process, and avoid excessive internal stress causing cracks in the coating. On the other hand, the metal shell consolidates the ceramic particles as the wear-resistant phase, and transmits and bears the load, retaining the circular structure of the ceramic particles to the maximum extent, so that the composite wear-resistant coating has a certain plasticity and increases the toughness of the composite wear-resistant coating.
[0017] The aforementioned method for preparing a core-shell composite wear-resistant coating by ultrasonic vibration-assisted laser cladding is characterized in that the melting points of the ceramic powder in step one and the metal powder in step two differ by at least 1000°C. By controlling the melting point difference between the ceramic powder and the metal powder, the metal powder is ensured to melt and encapsulate the ceramic powder, thereby producing the core-shell composite wear-resistant coating. Generally, the greater the melting point difference between the two, the easier it is to obtain a core-shell composite wear-resistant coating.
[0018] The above-mentioned method for preparing a core-shell composite wear-resistant coating by ultrasonic vibration-assisted laser cladding is characterized in that the volume ratio of ceramic powder to metal powder in the mixture described in step 2 is 1:8 to 1:10, and the ceramic powder is tungsten carbide, diamond, or cubic boron nitride powder, and the metal powder is iron, nickel, cobalt, or titanium metal powder. By limiting the volume ratio of ceramic powder to metal powder and controlling the proportion of ceramic powder, the uniformity of the distribution of ceramic particles serving as the core of the composite wear-resistant coating is ensured, while the probability of melting and decomposition of ceramic particles is reduced, thereby avoiding the formation of intermetallic compounds that may cause defects in the composite wear-resistant coating.
[0019] The above-mentioned method for preparing a core-shell structure composite wear-resistant coating by ultrasonic vibration-assisted laser cladding is characterized in that the laser cladding in step 4 adopts a synchronous powder feeding method, and the laser power of the laser cladding is 500W to 800W, the positive defocus is 5mm to 10mm, the powder feeding rate is 5g / min to 10g / min, the scanning speed is 150mm / min to 200mm / min, and the overlap rate is above 60%. Laser cladding has the characteristics of heat concentration, fast heating, fast cooling, and small heat-affected zone. The present invention adopts a lower laser power and controls other process parameters so that the low-melting-point metal powder melts first, while the high-melting-point ceramic powder does not melt due to the insufficient molten pool temperature and the short holding time at high temperature, so that the ceramic powder particle reinforcement phase fails to melt and is completely retained. At the same time, since the contact time between the metal droplet and the ceramic particle reinforcement phase is extremely short, the interfacial reaction can be effectively prevented. That is, through appropriate process optimization, an ideal core-shell structure composite wear-resistant coating is obtained.
[0020] The aforementioned method for preparing a core-shell composite wear-resistant coating by ultrasonic vibration-assisted laser cladding is characterized in that the ultrasonic-assisted vibration in step 4 has a power of 500W to 600W and a frequency of 10kHz to 30kHz. The nonlinear acoustic streaming and transient cavitation generated by ultrasonic-assisted vibration at this power and frequency significantly help promote uniform dispersion of the ceramic particle reinforcement phase, smooth thermal temperature gradients, reduce cracks, refine grains, and improve mechanical properties.
[0021] Compared with the prior art, the present invention has the following advantages:
[0022] 1. The present invention adopts an ultrasonic vibration-assisted laser cladding method, in which low-melting-point metal powder is first melted by laser cladding and then wrapped around ceramic particles. The dissimilar materials are fused through capillary action, thereby suppressing the formation of intermetallic compounds to the maximum extent, avoiding the coating having a large brittleness and a tendency to easily cause cracks. At the same time, the cavitation effect of ultrasonic vibration is used to increase the fluidity and density distribution uniformity of ceramic particles, so that the ceramic particles are evenly distributed and defects such as pores and cracks are reduced, forming a core-shell structure composite wear-resistant coating with dispersed ceramic particles as the core and the metal phase as the shell, thereby improving the performance of the composite wear-resistant coating and making the coating have both the high wear resistance of the ceramic phase and the toughness of the metal phase.
[0023] 2. The method of preparing core-shell structure composite wear-resistant coating by ultrasonic vibration-assisted laser cladding of the present invention combines the advantages of surface coating technology and composite material technology. According to the needs of different parts of the product, a high wear-resistant and toughened coating with ceramic particles as the reinforcing phase can be prepared on its surface at a lower cost, thereby improving product performance.
[0024] 3. The present invention achieves precise control of heat input by controlling the process parameters of laser cladding to regulate its rapid solidification process, thereby controlling the composition, thickness and dilution rate of the composite wear-resistant coating. The preparation process is simple to operate, has high processing efficiency, and is easy to implement.
[0025] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is a schematic structural diagram of the core-shell structure composite wear-resistant coating prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0027] Example 1
[0028] This embodiment includes the following steps:
[0029] Step 1: sieve the CrN ceramic powder through a -325 mesh screen;
[0030] Step 2: Place the spherical CrN ceramic powder with a particle size of 40 μm to 45 μm and the Cr metal powder with a particle size of 150 μm after being screened in Step 1 into a ball mill, place a diamond ball mill, seal the mill, and perform ball milling for 4 hours. Then, take it out and place it in a drying oven at 80° C. for 1 hour to obtain a mixture, wherein the volume ratio of CrN ceramic powder to Cr metal powder in the mixture is 1:8;
[0031] Step 3: Clean the 316H stainless steel surface and install and position it, and load the mixture obtained in step 2 into the powder feeder of the laser cladding equipment as cladding powder;
[0032] Step 4. Set the laser cladding process parameters including laser power, defocus, scanning speed, powder feeding rate, set the ultrasonic vibration power and frequency, then start the laser cladding equipment and ultrasonic vibration device, and complete the laser cladding with the assistance of ultrasonic vibration. The laser cladding adopts a synchronous powder feeding method, and the laser power of the laser cladding is 600W, the positive defocus is 10mm, the powder feeding rate is 5g / min, the scanning speed is 180mm / min, the overlap rate is 70%, the power of the ultrasonic assisted vibration is 500W, and the frequency is 25kHz. A core-shell structure composite wear-resistant coating with dispersed CrN ceramic particles as the core, Cr metal phase as the shell and wrapped around the core is formed on the surface of 316H stainless steel.
[0033] Figure 1 This is a schematic diagram of the structure of the core-shell composite wear-resistant coating prepared in this embodiment. Figure 1 It can be seen that under lower laser power conditions, large-sized, low-melting-point metal powder melts earlier than small-sized, high-melting-point ceramic powder, and wraps the ceramic powder to form a shell, while small-sized ceramic particles are dispersed as cores to form a core-shell structure composite wear-resistant coating.
[0034] The ceramic powder in this embodiment may also be replaced by diamond or cubic boron nitride powder, and the metal powder may also be replaced by iron or nickel metal powder.
[0035] Example 2
[0036] This embodiment includes the following steps:
[0037] Step 1: Process the TiC ceramic powder through a -325 mesh sieve;
[0038] Step 2: Place the spherical TiC ceramic powder with a particle size of 20 μm to 25 μm and the Ti metal powder with a particle size of 180 μm after being screened in step 1 into a ball mill, place a diamond ball mill, seal the mill, and perform ball milling for 4 hours. Then, take it out and place it in a drying oven at 80° C. for 2 hours to obtain a mixture, wherein the volume ratio of TiC ceramic powder to Ti metal powder in the mixture is 1:10;
[0039] Step 3: Clean the surface of TC4 titanium alloy and install and position it, and load the mixture obtained in step 2 into the powder feeder of the laser cladding equipment as cladding powder;
[0040] Step 4. Set the laser cladding process parameters including laser power, defocus, scanning speed, powder feeding rate, set the ultrasonic vibration power and frequency, then start the laser cladding equipment and ultrasonic vibration device, and complete the laser cladding with the assistance of ultrasonic vibration. The laser cladding adopts a synchronous powder feeding method, and the laser power of the laser cladding is 800W, the positive defocus is 5mm, the powder feeding rate is 10g / min, the scanning speed is 200mm / min, the overlap rate is 60%, the power of the ultrasonic assisted vibration is 600W, and the frequency is 10kHz. A core-shell structure composite wear-resistant coating with dispersed TiC ceramic particles as the core, Ti metal phase as the shell and wrapped around the core is formed on the surface of the TC4 titanium alloy.
[0041] The ceramic powder in this embodiment may also be replaced by diamond or cubic boron nitride powder, and the metal powder may also be replaced by iron or nickel metal powder.
[0042] Example 3
[0043] This embodiment includes the following steps:
[0044] Step 1: Process the WC ceramic powder through a -325 mesh sieve;
[0045] Step 2: Place the spherical WC ceramic powder with a particle size of 40 μm to 45 μm and the Co metal powder with a particle size of 120 μm after being screened in Step 1 into a ball mill, place a diamond ball mill, seal the mill, and perform ball milling for 4 hours. Then, take it out and place it in a drying oven at 80° C. for 1 hour to obtain a mixture, wherein the volume ratio of the WC ceramic powder to the Co metal powder in the mixture is 1:9;
[0046] Step 3: Clean the 304 stainless steel surface and install and position it, and then load the mixture obtained in step 2 into the powder feeder of the laser cladding equipment as cladding powder;
[0047] Step 4. Set the laser cladding process parameters including laser power, defocus, scanning speed, powder feeding rate, set the ultrasonic vibration power and frequency, then start the laser cladding equipment and ultrasonic vibration device, and complete the laser cladding with the assistance of ultrasonic vibration. The laser cladding adopts a synchronous powder feeding method, and the laser power of the laser cladding is 700W, the positive defocus is 8mm, the powder feeding rate is 7g / min, the scanning speed is 150mm / min, the overlap rate is 80%, the power of the ultrasonic assisted vibration is 500W, and the frequency is 30kHz. A core-shell structure composite wear-resistant coating with dispersed WC ceramic particles as the core, Co metal phase as the shell and wrapped around the core is formed on the surface of 304 stainless steel.
[0048] The ceramic powder in this embodiment may also be replaced by diamond or cubic boron nitride powder, and the metal powder may also be replaced by iron or nickel metal powder.
[0049] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent variation made to the above embodiment based on the essence of the invention technology shall still fall within the scope of protection of the technical solution of the present invention.
Claims
1. A method for preparing a core-shell structure composite wear-resistant coating by ultrasonic vibration-assisted laser cladding. It is characterized in that The method comprises the following steps: Step 1: Screen the ceramic powder; Step 2: Put the ceramic powder and metal powder processed by the screen in step 1 into a ball mill, put in a diamond ball mill, seal the mill and perform ball milling for more than 2 hours, then take out and place in a drying oven for drying to obtain a mixture; the drying temperature is 80° C. and the time is 1 hour to 2 hours; Step 3: clean the surface of the material to be clad and install and position it, and load the mixture obtained in step 2 into the powder feeder of the laser cladding equipment as cladding powder; Step 4: Set the laser cladding process parameters including laser power, defocus, scanning speed, powder feeding rate, set the ultrasonic vibration power and frequency, and then start the laser cladding equipment and ultrasonic vibration device to complete the laser cladding with the assistance of ultrasonic vibration to form a core-shell structure composite wear-resistant coating on the surface of the material to be clad.
2. The method for preparing a core-shell structure composite wear-resistant coating by ultrasonic vibration-assisted laser cladding according to claim 1, It is characterized in that The sieve treatment described in step 1 uses a -325 mesh sieve.
3. The method for preparing a core-shell structure composite wear-resistant coating by ultrasonic vibration-assisted laser cladding according to claim 1, It is characterized in that The ceramic powder in step 1 is a high melting point superhard spherical particle, which is tungsten carbide, titanium carbide, diamond or cubic boron nitride powder with a particle size not exceeding 45 μm.
4. The method for preparing a core-shell structure composite wear-resistant coating by ultrasonic vibration-assisted laser cladding according to claim 1, It is characterized in that The metal powder in step 2 is iron, nickel, cobalt or titanium metal powder with a particle size of more than 100 μm.
5. The method for preparing a core-shell structure composite wear-resistant coating by ultrasonic vibration-assisted laser cladding according to claim 1, It is characterized in that The melting point difference between the ceramic powder in step 1 and the metal powder in step 2 is more than 1000°C.
6. The method for preparing a core-shell structure composite wear-resistant coating by ultrasonic vibration-assisted laser cladding according to claim 1, It is characterized in that The volume ratio of the ceramic powder to the metal powder in the mixture in step 2 is 1:8-1:10, and the ceramic powder is tungsten carbide, diamond or cubic boron nitride powder, and the metal powder is iron, nickel, cobalt or titanium metal powder.
7. The method for preparing a core-shell structure composite wear-resistant coating by ultrasonic vibration-assisted laser cladding according to claim 1, It is characterized in that The laser cladding in step 4 adopts a synchronous powder feeding method, and the laser power of the laser cladding is 500W to 800W, the positive defocus is 5mm to 10mm, the powder feeding rate is 5g / min to 10g / min, the scanning speed is 150mm / min to 200mm / min, and the overlap rate is above 60%.
8. The method for preparing a core-shell structure composite wear-resistant coating by ultrasonic vibration-assisted laser cladding according to claim 1, It is characterized in that The power of the ultrasonic-assisted vibration in step 4 is 500W to 600W, and the frequency is 10kHz to 30kHz.