Compositions for depositing monolayers of alkanethiol on metal surfaces and related methods

By using compositions of alkylthiols, water-soluble emulsifiers and additional layer remover on metal surfaces, the rapid formation of alkanethiol monolayers is solved, and the problem of gloss loss on the surface of silver and gold is achieved by using ultrasonic baths or polishing processes. Anti-dark and lubricating effects for commercial applications.

CN119061398APending Publication Date: 2024-12-03NANO MINT TECHNOLOGIES LLC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410009803.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-05-30
Filing Date
2024-01-03
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The prior art is difficult to quickly and effectively form a uniform monolayer of alkanethiol on the silver and gold surfaces, resulting in the loss of gloss on the silver surface and the red spots on the gold surface, affecting the maintenance and commercial application of metal products.

Method used

Using an anti-dark composition containing alkanethiol, a water-soluble emulsifier and an additional layer of remover, a very ordered monolayer of alkanethiol is formed in 1-10 minutes by ultrasonic bath or polishing process to remove the additional layer of alkanethiol. layer, ensuring tight packing and low thickness of the single layer.

Benefits of technology

It realizes the rapid and effective formation of a uniform alkylthiol monolayer on the metal surface during commercial production time, preventing the loss of gloss on the silver and gold surfaces, reducing the mold to blacken, and improving the surface quality and lubricating performance of the coin.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119061398A_ABST
    Figure CN119061398A_ABST
Patent Text Reader

Abstract

A composition and method for depositing an alkylthiol monolayer on a metal surface is provided. The monolayer of alkanethiol is applied using an economically reliable method, such as by polishing or ultrasonic bathing. The additional layer of alkanethiol is removed, leaving a single self-assembled monolayer (SAM) that enhances the darkness of the surface and lubricates the surface.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention generally relates to a composition and method for inhibiting corrosion of metallic materials by applying a sulfur-containing organic inhibitor to the metal surface at risk of corrosion. Background Art

[0002] Tarnishing or discoloration of silver surfaces is a long-standing problem. Beautiful metal objects, such as coins, jewelry, and tableware, tend to tarnish quickly if they are exposed to normal atmospheric conditions. Even when silver and gold objects are carefully stored in a controlled environment, tarnishing can still occur over time. For example, collectible silver coins are often stored in plastic capsules to reduce tarnishing, but after a few years, the edges of the coins begin to take on a brown color. Even museum artifacts kept in a controlled environment can tarnish over the years.

[0003] Tarnish or discoloration of silver surfaces is caused by sulfidation, as silver readily reacts with H2S in the air to form silver sulfide. Very low concentrations of H2S can tarnish silver surfaces.

[0004] Tarnish on the surface of gold usually appears as small red spots. Even the purest gold retains a tiny percentage of residual silver embedded within the gold metal. Research has shown that even though gold has a purity greater than 99.99%, small amounts of silver sulfide are still present on the surface of the gold. It is this residual silver that, over time, turns into visible red spots of silver tarnish on the surface of the gold and causes buyers to question the purity of the material.

[0005] To address the associated issues of tarnishing on copper-nickel coins, for more than a decade the minting industry has treated copper alloy coins with benzotriazole (BTA) compositions to form an anti-tarnish film on the copper-nickel surface. The applied copper-nickel anti-tarnish film not only has anti-tarnishing properties, but also acts as a lubricant. The use of this film saves millions of dollars each year. While the anti-tarnishing problem of copper-nickel alloys is addressed by applying a BTA film, BTA does not react with silver or gold. Therefore, tarnishing of silver or gold coins and other articles having a metal surface remains a problem.

[0006] Due to the unresolved problem of tarnishing on silver, many chemicals have been screened in recent years to evaluate their anti-tarnish properties and assess their binding strength on the silver surface. Alkanethiol films were found in the laboratory to form strong bonds with silver surfaces and cover the metal surface to block attack by corrosive molecules, but the discovered compositions and methods require many days to form a very ordered alkanethiol film that can tightly cover the surface, which is necessary to prevent tarnishing.

[0007] Alkanethiol (or alkylthiol) is a thiol having an R—SH structure of a hydrophobic alkyl chain (R) attached to a thiol group (SH).

[0008] The alkanethiols were identified as self-assembled monolayers (SAMs) in which the sulfhydryl (SH) groups of the alkanethiols have an affinity for silver and act as surface anchors. The alkane chain tails align with each other. The force that promotes self-assembly ordering is the hydrophobic van der Waals interactions between the carbons of the alkane chains. In the alkanethiols monolayer, this interaction causes the alkane chains to be tightly packed and tilted to about 30 degrees to maximize the interactions between the chains and reduce the overall surface energy. It is believed that in a very ordered monolayer, the hydrophobic interactions between the chains overcome the rotational freedom of the molecules.

[0009] In tests, when alkanethiol is introduced to a metal surface, an initial poorly ordered stage of a monolayer forms quickly. Far from being very ordered, it has many troublesome defects and regions in the multilayer, which are caused by van der Waals interactions between the carbons of the alkane chains. Within a few days, the initially poorly ordered alkanethiol film was found in tests to be able to self-assemble to become a very ordered SAM.

[0010] A well-ordered monolayer is advantageous because if the protective layer is not densely packed, it cannot block corrosive elements and cannot perform its anti-tarnishing function. In addition, the monolayer is required to effectively perform the lubrication function during minting to achieve longer die life, to minimize die blackening, and to maintain high coin surface quality. In addition, a completely hydrophobic outer surface is required so that the coin blank or coin will not be exposed to water and avoid the formation of water spots on its surface.

[0011] Although alkanethiol films have been used as anti-tarnish treatments for silver surfaces with some degree of success, there are two key issues that have not been resolved. These two unresolved issues have greatly limited the use of SAM technology in the commercial market. The first issue is that the time to form a SAM film is too long for commercial applications. In most research laboratories, it takes several days to produce a SAM film covering the entire surface after immersing the sample in a sulfur-containing organic inhibitor solution. The second issue is film thickness. Using traditional methods and treatment solutions, it has proven difficult to produce a true monolayer of thiol films on silver or gold surfaces, and the poorly formed defective monolayers do not meet the needs of commercial use.

[0012] Thus, there is a need for an anti-tarnishing composition that can be used to produce an aqueous solution of an alkanethiolan into which an article having a metal surface can be immersed to deposit a uniform monolayer of the alkanethiolan on the surface to provide anti-tarnishing and / or lubricity properties; and a need for methods of applying alkanethiolans, methods of producing aqueous solutions of alkanethiolans, and methods of producing treated metal articles, wherein the anti-tarnishing treatment can be quickly and efficiently applied to the metal article in accordance with commercial manufacturing times for producing metal objects, and wherein the anti-tarnishing composition forms a uniform, well-ordered monolayer that minimizes defects and areas of multilayering. Summary of the invention

[0013] The present invention relates to anti-tarnish compositions for depositing an alkanethiol monolayer on a metal surface, and also to methods for depositing alkanethiols, methods for producing aqueous alkanethiol solutions, and methods for producing metal articles treated with the anti-tarnish compositions. In the present invention, the anti-tarnish treatment is applied quickly to accommodate production times in commercial equipment, and is applied in a uniform, well-ordered monolayer while removing additional layers of alkanethiol that may have accumulated on the base alkanethiol monolayer. The self-assembled alkanethiol monolayer reduces tarnish on the surface and further acts as a lubricant between the mold and the surface.

[0014] The anti-tarnish composition comprises an alkanethiols, a water-soluble emulsifier and an extra layer remover. The extra layer remover comprises a carboxylic acid or a salt thereof, and preferably comprises tartaric acid or a salt thereof, in an amount effective to remove extra molecules of the alkanethiols beyond the tightly packed basic monomolecular layer of the alkanethiols. Although tartaric acid can also act as an emulsifier, the emulsifier preferably comprises polysorbate 80. In a preferred aspect of the present invention, an antimicrobial agent can be added to the anti-tarnish composition, which allows for longer storage and / or use time. In another aspect of the present invention, a surfactant can be additionally added to the anti-tarnish solution.

[0015] The composition is dispersed in water to form an aqueous solution of an alkanethiol. The composition of the present invention is applied by polishing or an ultrasonic bath in an aqueous solution of an alkanethiol. Due to the selected components of the anti-tarnish composition of the present invention and the method of the present invention used, a well-ordered monolayer can be applied to the metal surface in a very short time, such as within 1-10 minutes. Therefore, due to the rapid application, the rapid and efficient ordering of a uniform monolayer, and the removal of the extra layer of the alkanethiol, the solution and method of the present invention can be effectively used in commercial production.

[0016] The application of this alkane thiol solution to the surface of silver and its alloys is particularly described herein, but it can also be used on other metal surfaces. The alkane thiol composition of the present invention can be applied to gold (and other metals) to solve the problem of residual silver tarnishing and to provide lubrication for stamping or other processes that can be used to manufacture metal products. For example, a gold surface can be treated so that a small amount of residual silver on its surface will not form a visible red spot of silver tarnish. Thus, the composition and treatment of the present invention provide advantages in treating not only silver, but also gold and other metals.

[0017] Anti-tarnish treatment can be used before or after the production of metal products. For example, tests were conducted in a coin minting facility where anti-tarnish treatment was applied before coins were stamped, after coins were stamped, and both before and after stamping. Applying the treatment before stamping advantageously increased lubrication and reduced die surface blackening in addition to increasing anti-tarnish properties. Applying the treatment after stamping provides anti-tarnish properties to the surface of the newly stamped metal. Applying the treatment before and after stamping provides both benefits.

[0018] In one aspect of the invention, the alkanethiol comprises hexadecyl mercaptan.

[0019] In another aspect of the present invention, the alkanethiol comprises octadecyl mercaptan.

[0020] In one aspect of the invention, the emulsifier comprises polysorbate 80.

[0021] In another aspect of the invention, the emulsifier comprises Triton X-100.

[0022] In another aspect of the present invention, the emulsifier comprises a water-soluble nonionic surfactant.

[0023] In one aspect of the present invention, the additional layer removing agent comprises tartaric acid or a salt thereof.

[0024] In another aspect of the present invention, the additional layer removal agent comprises tartaric acid.

[0025] In another aspect of the present invention, the additional layer removal agent comprises potassium tartrate.

[0026] In one aspect of the invention, the alkanethiol solution further comprises an antimicrobial agent.

[0027] In additional aspects of the invention, the antimicrobial agent comprises didecyl dimethyl ammonium bicarbonate and / or didecyl dimethyl ammonium carbonate sold under the brand name CARBOSHIELD 1000.

[0028] In one aspect of the invention, the treatment method comprises bathing the metal object to be treated in an ultrasonic water bath.

[0029] In another aspect of the invention, a treatment method includes bathing the metal object to be treated in an ultrasonic water bath having two wave generators.

[0030] In an additional aspect of the invention, a treatment method includes bathing the metal object to be treated in an ultrasonic water bath having two wave generators operating at different frequencies.

[0031] In one aspect of the present invention, the ultrasonic bath treatment time is less than 5 minutes.

[0032] In another aspect of the invention, the ultrasonic bath time is 1 minute.

[0033] In additional aspects of the invention, the ultrasonic bath time is between 1 minute and 5 minutes.

[0034] In another aspect of the invention, the ultrasonic bath time is between 1 minute and 10 minutes.

[0035] In another aspect of the invention, the monolayer is used in a portable, home ultrasonic cleaner.

[0036] In another aspect of the invention, the monomolecular layer is applied to the surface of the metal object by a polishing process in a polishing machine using stainless steel media.

[0037] In an additional aspect of the invention, the monomolecular layer is applied to the coin blank by a polishing process using a stainless steel media.

[0038] In one aspect of the invention, the anti-tarnish composition is applied prior to the stamping of the coin.

[0039] In another aspect of the invention, the anti-tarnish composition is applied after the stamping of the coin.

[0040] In additional aspects of the invention, the anti-tarnish composition is applied both before and after the stamping of the coin.

[0041] In another aspect of the invention, the anti-tarnish composition is applied as a treatment to the surface of the metal article after the metal article has been formed or shaped.

[0042] In another aspect of the invention, a method for depositing an alkanethiol monolayer on a metal surface includes an environmental sulfurization test to evaluate anti-tarnishing performance.

[0043] In another aspect of the invention, a method for depositing an alkanethiol monolayer on a metal surface includes an accelerated sulfurization test to evaluate anti-tarnishing performance.

[0044] It is an object of the present invention to provide a composition for depositing an alkanethiol monolayer onto a metal surface for anti-tarnishing and / or lubrication, and methods associated with said composition, which have improved performance relative to the above-mentioned prior art systems and methods.

[0045] These and other objects, features and advantages of the present invention will become more apparent from the accompanying drawings and the following detailed description of the preferred embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] Preferred embodiments of the present invention will hereinafter be described with reference to the accompanying drawings, which are provided to illustrate rather than to limit the present invention, wherein like reference numerals denote like elements.

[0047] Figure 1 is a top view of the reverse side of a 1993 US Mint Walking Liberty 1 ounce silver coin prior to treatment with the anti-tarnish composition of the present invention.

[0048] Figure 2 is a schematic diagram of an ultrasonic water bath, a wave generator, and an anti-tarnishing fluid alkanethiol solution, schematically showing a 1993 United States Mint minted Liberty coin (not to scale) during deposition of an alkanethiol monolayer of the present invention on a portion of the surface of the 1993 United States Mint minted Liberty coin.

[0049] Figure 3 After accelerated vulcanization test, Figure 2 A top view of the reverse side of a 1993 United States Mint Walking Liberty coin treated as shown, showing tarnish only on the portion of the coin that was not treated with the alkanethiol monolayer film coating of the present invention.

[0050] Figure 4 is a graph showing the results of measured reflectivity testing comparing the uncoated / untreated reverse and obverse of a 1993 U.S. Mint Walking Liberty coin to the reverse and obverse of a 1993 U.S. Mint Walking Liberty coin that had been treated with the anti-tarnish composition of the present invention to form a monolayer of an alkanethiol on the coin surface.

[0051] Figure 5A is a graphic representation of a gold bar formed from a gold billet ultrasonically bathed in the anti-tarnish composition of the present invention, showing a Figure 5B The untreated gold bars have a smoother surface.

[0052] Figure 5B is a diagrammatic representation of a gold bar formed from a standard gold billet (without application of the anti-tarnishing composition of the present invention).

[0053] Figure 6 is a graph showing the measured reflectance test results for various coins exposed to the sulfurization test, including, for comparison, a Route 66 Round treated with the anti-tarnish composition of the present invention.

[0054] Fig. 7A is a schematic diagram showing the surface contact angle of a water drop on a metal surface that has been treated with the anti-tarnish composition of the present invention, which can be compared with Figure 7B Make a comparison.

[0055] Figure 7B is a schematic diagram showing the surface contact angle of a water droplet on a standard untreated metal surface of the prior art, which is shown for use with Fig. 7A Compare this to water droplets on a metal surface.

[0056] Like reference numerals refer to like parts throughout the several views of the drawings. DETAILED DESCRIPTION

[0057] As shown in the accompanying drawings, the present invention relates to an anti-tarnish composition and an alkanethiol aqueous solution 10 formed when the chemical substances of the anti-tarnish composition are mixed with water (preferably deionized water). The anti-tarnish composition and the alkanethiol aqueous solution 10 are used to deposit an alkanethiol monolayer onto a metal surface 25 of an object 20 to be treated. It further relates to methods related to producing the alkanethiol aqueous solution 10 from the anti-tarnish composition, applying the alkanethiol aqueous solution 10 to form a SAM alkanethiol film on the surface 25, making an anti-tarnishing article 20 having a metal surface 25, and methods related to testing the anti-tarnish and lubricity properties of a metal article 20 after treating the article 20 with the alkanethiol solution 10.

[0058] The alkanethiol aqueous solution 10 can be used to apply an alkanethiol monolayer to a metal surface 25 of an article 20 before, after, or both before and after the metal article is formed; or the alkanethiol monolayer can be applied to the surface of an article such as jewelry, silverware, or a museum artifact that was created months, years, or centuries ago.

[0059] The compositions and methods of the present invention are suitable for improving the tarnish resistance of any of a variety of metal articles 20, although in the exemplary discussion herein, the application of the monolayer and the associated methods are specifically discussed with respect to its application to silver and gold coins, particularly silver coins. However, other types of new or old articles 20 may also be advantageously treated by using the disclosed anti-tarnish compositions of the present invention incorporated into an aqueous solution of an alkanethiolan 10. For example, the compositions and methods of the present invention are suitable and useful for individuals with new or old silver articles that may have tarnish and would benefit from tarnish removal accompanied by the application of an anti-tarnish monolayer. In addition, the compositions and methods of the present invention disclosed herein may advantageously be used by restorers of museum artifacts having tarnished metal surfaces to remove the tarnish and apply an anti-tarnish monolayer to prevent or minimize future tarnish or discoloration.

[0060] The alkanethiols of the anti-tarnish composition of the present invention have the general formula R-SH, wherein SH is a mercapto group, and wherein R is an alkyl group having 10 to 20 carbon atoms forming a hydrophobic alkyl chain. In one embodiment of the present invention, the alkanethiols comprise octadecyl mercaptan. In another embodiment of the present invention, the alkanethiols comprise hexadecyl mercaptan.

[0061] The anti-tarnish composition of the present invention comprises an alkanethiol, an emulsifier and an additional layer remover. The components of the anti-tarnish composition are combined with water (and optionally other components) to form an alkanethiol aqueous solution 10.

[0062] In one aspect of the invention, an aqueous solution of alkanethiols 10 is used to provide a lubricating and anti-tarnishing coating to a coin blank. In this aspect, it can be placed in a polishing machine, and the coin blank can be rotated and polished with stainless steel media.

[0063] In another aspect of the invention, an alkanethiol aqueous solution 10 is disposed within a tank 13 of an ultrasonic water bath 12. In this aspect of the invention, one or more metal articles 20 to be treated are supported and bathed in the alkanethiol aqueous solution 10 into which the alkanethiol anti-tarnish composition has been mixed.

[0064] In both aspects, the self-assembled monolayer of alkanethiols is deposited in a time period measured in minutes, rather than the days required by conventional methods. Upon immersion in the aqueous solution of alkanethiols 10, the sulfur of the mercapto groups complexes with the silver atoms at the surface of the treated article, and the large organic portion of the alkanethiols molecules forms a shield on the metal surface to protect it from atmospheric pollutants and provide a lubricating effect. In order to quickly achieve a uniform monolayer, the extra layer remover removes molecules of the alkanethiols that are superimposed on or extend beyond the very ordered base monolayer of the alkanethiols. This effect of the extra layer remover allows the deposition of an alkanethiols monolayer having a thickness of less than 100 nanometers. In one aspect of the invention, the alkanethiols monolayer has a thickness between 20 and 100 nanometers. Preferably, the alkanethiols monolayer is deposited as a uniform monolayer having a thickness of 40 to 60 nanometers.

[0065] In addition to the alkanethiols, emulsifiers, and additional layer removers, the anti-tarnish composition may also include other components added to the composition to help remove tarnish from the surface, further aid in emulsification, increase the viscosity of the fluid in tank 13, provide a stable product, and / or further help remove additional molecules and layers of the alkanethiols. For example, in addition to the alkanethiols, emulsifiers, and additional layer removers, the composition may also include any one or more of the following: one or more antimicrobial agents, additional emulsifiers, surfactants, rheology modifiers, liquid diluents, and / or additional additional layer removers. Optionally, the anti-tarnish composition may further include a colorant and / or a flavor enhancer.

[0066] The surfactant may be a nonionic surfactant and / or a cationic surfactant, but is preferably a nonionic surfactant such as glyceryl monostearate.

[0067] The antimicrobial agent may be any standard antimicrobial compound; in a preferred aspect of the invention, didecyl dimethyl ammonium bicarbonate and / or didecyl dimethyl ammonium carbonate sold under the brand name CARBOSHIELD 1000 are preferred. The CARBOSHIELD 1000 components, in addition to their antimicrobial properties, may act as a cationic surfactant and act to inhibit corrosion. Because approximately 99% of the chemicals in the aqueous alkanethiol solution 10 may be food grade, fungi will grow in the aqueous alkanethiol solution 10 over time, which may cause the aqueous alkanethiol solution 10 to clump (like fat on the surface of soup). By using an antimicrobial agent, the aqueous alkanethiol solution 10 may be stored for considerable periods of time and may be used in the ultrasonic bath 12 for longer periods of time.

[0068] The emulsifier of the anti-tarnish composition may be a nonionic emulsifier (such as polysorbate 80, polysorbate 20, glyceryl monostearate, a polyethylene glycol derivative sold under the brand name TRITON X-10o, etc.). In a preferred aspect of the present invention, the emulsifier of the anti-tarnish composition comprises polysorbate 80 (which may also partially act as a surfactant).

[0069] In a preferred aspect of the invention, some components of the anti-tarnish composition are first mixed with a diluent before being introduced into the water of the ultrasonic bath 12. The diluent can be a liquid such as water, or a low molecular weight organic compound such as methanol, ethanol, propanol, etc. The diluent can optionally be a mixture of water and an organic compound, or can be an organic compound mixed with a rheological expansion fluid to carry the alkanethiol molecules as they move and relocate along the metal surface. In a preferred aspect of the invention, the diluent comprises 91% propanol.

[0070] In one aspect of the invention, the extra layer removal agent is a carboxylic acid or a salt thereof. In another aspect, the extra layer removal agent is tartaric acid or a salt thereof. In one aspect of the invention, the extra layer removal agent is a salt of tartaric acid, such as the potassium salt of tartaric acid, potassium tartrate. In a preferred aspect, the extra layer removal agent is tartaric acid.

[0071] Tartaric acid is preferred because it can dissolve chemicals that are weakly bound to the silver surface (such as emulsifiers and / or antimicrobial agents) into the water of the aqueous alkanethiol solution 10, and it can dissociate any additional layers of alkanethiol that are weakly bound above the base monolayer of alkanethiol. However, tartaric acid cannot dissolve strong chemical bonds, such as alkanethiol to silver bonds. Because tartaric acid is used to dissociate any non-alkanethiol chemicals that may be loosely bound to the metal surface, it allows the alkanethiol molecules in the aqueous alkanethiol solution 10 to reach the silver surface and form stronger bonds.

[0072] In one embodiment, the general formula of the anti-tarnish composition is as follows (in weight percent):

[0073] Alkanethiol = 0.1 to 5%;

[0074] Emulsifier = 0.1 to 5%;

[0075] Alcohol = 3 to 35%;

[0076] Water (preferably deionized water) = 1 to 95%; and

[0077] Additional layer remover = 1 to 20%.

[0078] In another embodiment of the present invention, the anti-tarnish composition has the following formula (by weight percentage):

[0079] Hexadecyl mercaptan and / or octadecyl mercaptan = 0.1 to 1%;

[0080] Polysorbate 80 = 0.1 to 1%;

[0081] Didecyldimethylammonium bicarbonate and / or didecyldimethylammonium carbonate (such as sold under the brand name Carboshield 1000) = 0.1% to 1%;

[0082] 91% Propanol = 4 to 12%;

[0083] Water (preferably deionized water) = 1 to 95%; and

[0084] Tartaric acid or its salts = 4 to 12%.

[0085] In another embodiment, the anti-tarnish composition is formulated as follows (in weight percent):

[0086] Hexadecyl mercaptan and / or octadecyl mercaptan = 0.3 to 0.5%;

[0087] Polysorbate 80 = 0.3 to 0.5%;

[0088] Didecyldimethylammonium bicarbonate and / or didecyldimethylammonium carbonate (such as sold under the brand name Carboshield 1000) = 0.3 to 0.7%;

[0089] 91% Propanol = 6 to 10%;

[0090] Water (preferably deionized water) = 1 to 95%; and

[0091] Tartaric acid or its salts = 6 to 10%.

[0092] In a preferred embodiment, the anti-tarnish composition has the following formula (by weight percentage):

[0093] Hexadecyl mercaptan = 0.3 to 0.5%;

[0094] Polysorbate 80 = 0.3 to 0.5%;

[0095] Didecyldimethylammonium bicarbonate and / or didecyldimethylammonium carbonate (such as sold under the brand name Carboshield 1000) = 0.3 to 0.7%;

[0096] 91% Propanol = 6 to 10%;

[0097] Water (preferably deionized water) = 75 to 90%; and

[0098] Tartaric acid = 6 to 10%.

[0099] In the solution / bath preparation method of the present invention, an aqueous alkanethiolan solution 10 is prepared from the components of the disclosed anti-tarnish composition and introduced into an ultrasonic bath 12 in preparation for receiving one or more articles to be treated.

[0100] The steps of the solution / bath preparation method include the following:

[0101] a) Start preparing an ultrasonic bath by placing water (preferably deionized water) into the tank 13 of the ultrasonic bath 12.

[0102] b) Heat the water in the ultrasonic bath 12 to 35°C to 65°C.

[0103] c) Add additional layer remover to the water.

[0104] d) Activate the ultrasonic generator 15 of the ultrasonic bath 12 to dissolve the additional layer removing agent into the water.

[0105] e) Wait until the extra layer remover is completely dissolved in the water.

[0106] f) In a separate container (such as a graduated cylinder), heat the diluent to 35°C to 65°C, such as by immersing the separate container in a cup of warm water.

[0107] g) Add the emulsifier to the diluent and stir, such as with a glass rod.

[0108] h) Add any antimicrobial agent to the diluent and stir.

[0109] i) Add the alkanethiol to the diluent and stir until all chemicals are dissolved to produce an alkanethiol / diluent mixture.

[0110] j) The ultrasonic generator 15 of the ultrasonic bath 12 is activated to start generating ultrasonic waves.

[0111] k) The alkanethiol / diluent mixture is poured into the water in tank 13 of ultrasonic bath 12. The generation of high frequency waves in the water by means of ultrasonic generator 15 causes the alkanethiol / diluent mixture to emulsify in the water in tank 13 and possibly generate some foam.

[0112] 1) The generation of ultrasonic waves is maintained while stirring until any foam disappears and the alkanethiol aqueous solution 10 formed in the tank 13 has a uniform appearance.

[0113] In a preferred embodiment of the present invention, the steps of the solution / bath preparation method include the following:

[0114] a) Start preparing an ultrasonic bath by placing water (preferably deionized water) into the tank 13 of the ultrasonic bath 12.

[0115] b) Heat the water in the ultrasonic bath 12 to 45°C to 55°C.

[0116] c) Adding tartaric acid or its salt to water as an additional layer removing agent.

[0117] d) Activate the ultrasonic generator 15 of the ultrasonic bath 12 to dissolve the additional layer removing agent into the water.

[0118] e) Wait until the extra layer remover is completely dissolved in the water.

[0119] f) In a separate container (such as a graduated cylinder), heat the alcohol to 45°C to 55°C, such as by immersing the separate container in a cup of warm water.

[0120] g) Add the emulsifier to the alcohol and stir.

[0121] h) Add the antimicrobial agent to the alcohol and stir.

[0122] i) Add the alkanethiol to the alcohol and stir until all chemicals are dissolved to produce an alkanethiol / alcohol mixture.

[0123] j) The ultrasonic generator 15 of the ultrasonic bath 12 is activated to start generating ultrasonic waves.

[0124] k) The alkanethiol / alcohol solution is poured into the water in the tank 13 of the ultrasonic bath 12. The generation of high frequency waves in the water by means of the ultrasonic generator 15 causes the alkanethiol / alcohol mixture to emulsify into the water in the tank 13 and possibly some foaming.

[0125] 1) The generation of ultrasonic waves is maintained while stirring until any foam disappears and the alkanethiol aqueous solution 10 formed in the tank 13 has a uniform appearance.

[0126] In one embodiment of the present invention, the ultrasonic bath 12 is equipped with an ultrasonic generator 15 that generates ultrasonic waves of a first frequency, which can be in the range of about 25 to 60 kHz. The ultrasonic bath 12 is typically sold as an ultrasonic cleaner with a heater and a digital timer that can be set to establish the length of time that the ultrasonic generator 15 will be activated. The ultrasonic bath 12 typically converts low-frequency AC current into high-frequency sound waves by using a piezoelectric transducer to generate a sine wave. These high-frequency ultrasonic vibrations generate tiny spherical bubbles that violently implode, creating cavitation through the formation and violent collapse of tiny vacuum bubbles in the solution. These implosions are not too violent, but energy is applied to every surface that the solution contacts.

[0127] In another embodiment of the present invention, the ultrasonic bath 12 is equipped with a swept frequency circuit. In this embodiment, the ultrasonic generator 15 generates ultrasonic waves at a first frequency that can be in the range of about 25 to 60 kHz, but additionally sweeps the output frequency to the transducer at about 2-3 kHz to eliminate inactive regions between adjacent standing waves. The sweep frequency provided produces overlapping ultrasonic waves.

[0128] In another embodiment of the present invention, the ultrasonic bath 12 is equipped with two swept frequency ultrasonic generators 15, 17 which generate ultrasonic waves at first and second output frequencies and also sweep one or both output frequencies at about 2-3 kHz.

[0129] In a preferred embodiment of the present invention, the ultrasonic bath 12 is a two-way dual-frequency bath equipped with two ultrasonic generators 15, 17 that generate ultrasonic waves of a first frequency and a second frequency, wherein both frequencies can be in the range of about 25 to 60 kHz. In one example, one ultrasonic generator 15 can be disposed at the bottom of the ultrasonic bath tank 13, and one ultrasonic generator 17 can be disposed at the side wall of the tank 13. In one aspect of the present invention, the first generator 15 is a 200-Watt 40-kHz ultrasonic generator located below the tank, and the second generator 17 is a 200-Watt 20-kHz ultrasonic generator disposed adjacent to the side wall of the tank 13.

[0130] When the two generators 15, 17 are started, it is found that due to the different frequencies provided by the two generators 15, 17, the cavitation bubbles generated are not spheres, but ellipsoids. When the ellipsoid collapses, the pressure area affected by the impact increases and the pressure is relatively uniform. The pressure spikes generated by the collapse of the cavitation bubble are blunted. This pressure adjustment is important for collectible coins, jewelry or museum artifacts. Any impact marks that may remain must be avoided. The two-way dual-frequency ultrasonic bath provides a good working environment to increase the chemical reaction rate without damaging the initial surface features. The processing time for completely applying the film to cover the solid surface is reduced from several days to one to a few minutes. In one aspect of the present invention, the ultrasonic bath time is 1-10 minutes. In another aspect, the ultrasonic bath time is less than 7 minutes. In another aspect, the ultrasonic bath time is less than 5 minutes. In another aspect, the ultrasonic bath time is less than 2 minutes. In one aspect, the ultrasonic bath time is 1 minute.

[0131] Preferably, the temperature of the aqueous alkanethiolate solution 10 in the tank is controlled between 45 and 50° C. Preferably, the coin or metal object 20 is directly immersed in the prepared solution without a pre-cleaning cycle in an ultrasonic bath. This is preferred because any cleaning process may damage the details on the object or coin.

[0132] When processing multiple coins or other articles 210 having metal surfaces, they can be processed sequentially or simultaneously. In one aspect where the coins are processed at a manufacturing plant, multiple coins can be supported in a tank 13 for simultaneous processing to accommodate manufacturing time frames. In other aspects, such as a home ultrasonic cleaner containing an aqueous solution of an alkanethiol 10 of the present invention, jewelry pieces can be processed individually or in groups.

[0133] After being immersed in the aqueous alkanethiol solution 10, the coin or article 20 is rinsed with distilled water and allowed to air dry or may be towel dried.

[0134] When applying a monolayer of alkanethiols to a metal surface or coin blank by polishing, a standard polishing process is used with the aqueous alkanethiols 10 of the present invention replacing the standard polishing water mixture. The coin blank to be treated, the aqueous alkanethiols 10 of the present invention, and stainless steel balls are placed in the bowl of the polishing machine. A rotor at the bottom of the bowl provides the mechanical agitation required to move the stainless steel balls and coin blank. As numerous balls slide over the blank, the chemicals within the aqueous alkanethiols 10 react with the metal surface 25.

[0135] When the alkanethiol monolayer is used in a home or restoration business, the user may not want to perform the steps of the solution / bath preparation method disclosed above. In this case, the alkanethiol aqueous solution 10 of the present invention can be prepared at the manufacturer and sold in containers (e.g., one gallon, two gallon, or five gallon jugs, etc.). In another aspect of the present invention, the components of the anti-tarnish composition can be sold with instructions for the user to mix with water in a home or commercial ultrasonic bath to produce the alkanethiol aqueous solution 10 of the present invention for use in a home or commercial ultrasonic bath. In another aspect of the present invention, the components of the anti-tarnish composition can be sold partially pre-mixed with additional water to be added by the user. In another aspect of the present invention, the components of the anti-tarnish composition can be sold in a set of multiple containers with preparation instructions provided to the user for mixing with water to produce the developed alkanethiol aqueous solution 10 for use in a home or commercial ultrasonic bath.

[0136] The process of applying alkanethiol to the surface of a metal object is a dynamic coating process in which the article to be treated is introduced into an aqueous alkanethiol solution 10 and a well-ordered alkanethiol SAM is formed on the surface. The method of applying the alkanethiol may vary slightly depending on the apparatus in which the article to be treated 20 is placed for treatment, as the aqueous alkanethiol solution 10 may be used in an ultrasonic bath 12, a more modestly sized home ultrasonic cleaner (such as those sold for cleaning jewelry), or a polished cylindrical container.

[0137] In this dynamic coating process, some molecules from the aqueous solution of alkanethiols 10 are continuously and simultaneously adsorbed onto the metal surface, while other molecules are desorbed from the surface. Although in some processes for applying a SAM film to a metal surface, the thickness of the molecules increases with time or with an increase in alkanethiols in the solution, when tartaric acid within the specific range disclosed herein is used, the SAM film thickness remains constant even when the concentration of alkanethiols in the solution 10 increases or when the bath time length increases.

[0138] When using the anti-tarnishing compositions and methods provided herein, the manufacturer or restorer may need to confirm, ensure or prove that the self-assembled monolayer exists and protects the metal surface 25. Although environmental testing can be performed in which H2S in the air is allowed to react with silver to form silver sulfide, it may take months or years to see results. To avoid waiting, an accelerated vulcanization system can be used in which the article 20 is exposed to a higher concentration of sulfur for a shorter period of time.

[0139] For example, in a mint or coin manufacturing facility, the production line moves rapidly, so it is not possible to use complex instrumentation to measure the deposited SAM film within the short time frame of the production line. Therefore, an accelerated sulfurization system can be used to accelerate the exposure to sulfur to provide test results. This will then allow the color and reflectivity of the coin to be used to evaluate the anti-tarnish performance of the SAM alkanethiol monolayer within a short time frame.

[0140] Tests have been conducted to ensure that the anti-tarnish composition and application method using the aqueous alkanethiol solution 10 produces a SAM alkanethiol monolayer that is deposited as a single well-ordered layer and forms a complete anti-tarnish film. Figure 1-3 One test shown was using a 1993 United States Mint Walking Liberty coin. Figure 1 A 1993 United States Mint Walking Liberty coin is shown, stored in a protected environment and relatively untarnished. Figure 2 The coin is then partially suspended in the developed alkanethiol solution 10, shown schematically (not to scale), so that only a portion (in the test shown, more than half of the coin's surface) is treated. After treatment, the coin is rinsed with distilled water and allowed to dry. No visible or measurable changes in reflectivity or color are seen on the treated portion of the surface. The coin is then placed in an accelerated vulcanization chamber for one hour, which is equivalent to several years of exposure to ambient atmosphere. The test results are shown in Figure 1. Figure 3 As shown, the treated portion of the coin remains in pristine condition and the uncoated areas on the coin react with the H2S in an accelerated vulcanization system and turn brown and dark blue, losing their luster.

[0141] exist Figure 4The results of a three-day sulfidation test are shown in a graph in FIG. 1 (in this case, the sulfidation test uses H2S released from vegetables, although other accelerated sulfidation tests may be used.) Reflectivity was measured in coated and uncoated areas of a 1993 United States Mint Walking Liberty silver coin. For the coated areas of the surface, the average reflectivity dropped from about 92% to about 89% after three days. For the uncoated surface areas, the reflectivity dropped to about 50-60%. The results demonstrate that a monolayer applied by the composition and method of the present invention can protect the unpolished surface of a coin, and demonstrate that the coin does not need to be newly minted for the alkanethiols to be applied. Thus, for collectors who prefer a slightly sulfided surface, the coin can be maintained in this favorable color, and sulfidation, which would further tarnish the coin, can be inhibited.

[0142] Figure 6 Results of another test are shown in . In this test, an alkanethiol monolayer was applied to a 2022 Sunshine Mint Route 66 silver round. The blank of the Route 66 silver round was polished with the alkanethiol solution 10 of the present invention before stamping, and was ultrasonically bathed in the solution 10 for 1.5 minutes after stamping. The treated coin was compared to seven 1 oz silver coins from around the world. Eight coins were placed in an accelerated vulcanization system to evaluate the anti-tarnish properties of the applied alkanethiol monolayer. Initially, the color and reflectivity of the coins were similar. Although some coins had a matte surface and some coins had a polished surface, the reflectivity was similar; initial reflectivity ranged from 92% to 96%.

[0143] After only one hour of vulcanization testing, all of the coins except the Route 66 silver round changed their color. The details of the process or chemical treatment of the various mints that produced the seven comparison coins are unknown, but the results of the vulcanization testing varied between the coins. The Britannia coin, made by the Royal Mint, showed the worst protection against tarnishing. The reflectivity of the Route 66 silver round did not change at all. Therefore, coin manufacturers using the anti-tarnishing compositions and methods of the present invention will maintain the original reflectivity and color, thereby reducing or eliminating customer complaints about tarnishing problems.

[0144] After the vulcanization test, small water droplets condense on the surface of the coin. The water droplets later evaporate, but some of the water droplets leave watermarks on the surface of the coin. However, due to its low surface tension properties, no watermarks are found on the Route 66 silver round.

[0145] Another test that can show the effectiveness of the anti-tarnishing alkanethiol monolayer in protecting the silver surface 25 is the test of the surface contact angle of a water droplet, such as Fig. 7A and 7BAs shown. Fig. 7A The processed Route 66 silver round is shown in Figure 7B The surface of a British coin from the Royal Mint is shown in Figure 25. The contact angle of the surface of the Route 66 coin was measured to be 90.1 degrees, which is consistent with the Figure 6 The highest contact angle was measured on the coins compared in the 2016 Coins. The lowest surface contact angle was measured on the British Royal Mint Britannia coin, which was 52.9 degrees. The contact angle values ​​also correlated with the presence of water spots on the coin surface after the vulcanization test. The Route 66 coin had no water spots.

[0146] Testing also showed that the alkanethiolan monolayer provided lubrication and reduced the coefficient of friction between the die and the blank during production. Thus, the alkanethiolan monolayer of the present invention increased die life and coin surface quality.

[0147] Gold articles and coins may also benefit from applying a monolayer of an alkanethiol to the gold surface both by reducing or eliminating red tarnish spots during stamping and by increasing the smoothness of the gold surface. Gold articles and coins may appear tarnished due to random red spots found on the surface caused by silver sulfide. While relatively long processes for etching gold surfaces with nitric acid are known to reduce gold tarnish, the inventive compositions and methods disclosed herein can be accomplished in a shorter time and with less damage to the surface.

[0148] In one test, 24 gold bars were ultrasonically bathed in the alkanethiol solution 10 disclosed above for 5 minutes. The bars were then rinsed in 50 degree deionized water and dried with a towel. The bars were then cast directly on a casting machine. Two phenomena were observed.

[0149] First, the mold surface did not turn black during stamping. The clean mold surface indicates that the alkanethiol monolayer on the billet surface is monomolecular and no additional alkanethiol molecules accumulate on the mold surface from casting again and again.

[0150] Second, the surface morphology is improved due to the low friction. While silver is a solid lubricant (so the stamped coin image looks essentially the same with or without an alkanethiol monolayer between the coin surface and the die), gold is not a solid lubricant. In the case of an alkanethiol monolayer applied to the gold surface, the friction is lower. This lower friction results in a smoother stamping surface. Figure 5A and 5B A comparison of whole gold bars with and without an alkanethiol monolayer is shown in FIG. Figure 5A The gold bars shown in . Figure 5B A control gold bar without an alkanethiol monolayer is shown in FIG. Most of the fine scratches on the surface of the treated gold bar are plastically smoothed, resulting in a Figure 5B Improved surface compared to standard gold bars.

[0151] Tarnished gold bars were also tested. Application of a monolayer of the alkanethiols of the present invention to tarnished gold bars resulted in the disappearance of the red tarnished spots. Furthermore, after accelerated sulfidation testing, the red spots did not reappear. This indicates that the anti-tarnish compositions and methods of the present invention can be used in gold product lines to replace nitric acid etching and improve surface smoothness.

[0152] The composition and treatment method proposed herein produce a thin and uniform SAM film. If the SAM film is not very thin and very uniform, some very small black spots will appear after being exposed to air for several months. The small black spots were analyzed with a scanning electron microscope, and it was observed that the sulfur concentration at the black spot position was very high. In contrast to the monolayer alkanethiols applied in the present invention, the black spots are silver sulfate formed by multilayer alkanethiols on the surface 25. Therefore, it is necessary to include an effective extra layer remover. Without wishing to be bound by theory, it is believed that the extra layer remover acts as a soap and opens the bonding between physical adsorptions, such as van der Waals forces, but it cannot open the bonding of chemical reaction products. Therefore, an extra layer remover is added to the alkanethiols aqueous solution 10 and an ultrasonic bath (or polishing method) is utilized to remove the extra physically adsorbed layer of the alkanethiols, and only the monolayer of the reaction is retained on the metal surface. In Fourier transform infrared (FTIR) spectroscopy measurements, the alkanethiols SAM film formed is proven to be a monolayer.

[0153] Anti-tarnish treatment can be used before or after the production of metal products. For example, tests were conducted in a coin minting facility where anti-tarnish treatment was applied before coins were stamped, after coins were stamped, and both before and after stamping. Applying the treatment before stamping advantageously increased lubrication and reduced die surface blackening in addition to increasing anti-tarnish properties. Applying the treatment after stamping provides anti-tarnish properties to the newly stamped metal surface. Applying the treatment before and after stamping provides two benefits.

[0154] Thus, the anti-tarnish composition of the present invention can be used to produce an aqueous solution of an alkanethiol into which an article 20 having a metal surface 25 can be immersed to deposit a uniform monolayer of the alkanethiol on the surface 25 to provide anti-tarnish and / or lubricity properties. The time frame for this application is short enough to be used in a coin manufacturing facility.

[0155] As many detailed modifications, variations and changes may be made to the preferred embodiments of the invention described, it is intended that all matters in the foregoing description and shown in the accompanying drawings be interpreted as illustrative and not in a limiting sense. Therefore, the scope of the invention should be determined by the appended claims and their legal equivalents.

Claims

1. An alkanethiolan aqueous solution, comprising: Alkanethiol for forming an alkanethiol monolayer; emulsifiers; and a carboxylic acid or a salt thereof in an amount effective to remove additional molecules of said alkanethiol beyond the base monolayer of said alkanethiol monolayer; and water.

2. The alkanethiol aqueous solution according to claim 1, wherein the alkanethiol is hexadecanethiol. The alkanethiol aqueous solution according to claim 1 , wherein the alkanethiol is octadecyl mercaptan.

4. The alkanethiol aqueous solution according to claim 1, wherein the alkanethiol aqueous solution is used to deposit a monolayer of the alkanethiol on a metal surface.

5. The alkanethiolan aqueous solution according to claim 4, wherein the metal surface comprises a silver surface. The alkanethiolan aqueous solution according to claim 1 , wherein the carboxylic acid comprises tartaric acid.

7. The alkanethiolan aqueous solution according to claim 1, wherein the carboxylic acid comprises potassium tartrate.

8. An anti-tarnish composition comprising: Alkanethiol for forming an alkanethiol monolayer; emulsifiers; and Tartaric acid or a salt thereof in an amount effective to remove additional molecules of said alkanethiol beyond the base monolayer of said alkanethiol monolayer.

9. The anti-tarnish composition according to claim 8, wherein the alkanethiol is hexadecyl mercaptan.

10. The anti-tarnish composition according to claim 8, wherein the alkanethiol is octadecyl mercaptan.

11. The anti-tarnish composition according to claim 8, wherein the anti-tarnish composition is mixed with water to form an aqueous solution of an alkanethiol.

12. The anti-tarnish composition of claim 8, wherein the anti-tarnish composition further comprises an antimicrobial agent.

13. A method for treating a metal surface of an article, include: The metal surface is treated with a solution comprising an alkanethiol and tartaric acid or a salt thereof; wherein the amount of tartaric acid or a salt thereof is effective to remove additional molecules of the alkanethiol beyond a base monolayer of the alkanethiol.

14. The method according to claim 13, further comprising: include: The metal surface was left in the solution for no longer than ten minutes.

15. The method of claim 13, wherein the metal surface is treated with a solution include: placing the solution in an ultrasonic bath with an ultrasonic generator; immersing the metal surface in the solution in the ultrasonic bath; activating the ultrasonic generator; and The metal surface remains in the ultrasonic bath for at least one minute while the ultrasonic generator is activated.

16. The method of claim 13, wherein the metal surface is treated with a solution include: placing the solution in an ultrasonic bath with two ultrasonic generators; immersing the article in the solution in the ultrasonic bath; activating both of the two ultrasonic generators; and The article remains in the ultrasonic bath for at least one minute while the two ultrasonic generators are activated.

17. The method of claim 16, wherein the two ultrasonic generators operate at different frequencies.

18. The method according to claim 16, in: One of the two ultrasonic generators is disposed at the bottom of the ultrasonic bath; and The second of the two ultrasonic generators is arranged on one side of the ultrasonic bath.

19. The method of claim 13, wherein the article comprises a coin blank and the metal surface comprises a coin blank surface; and wherein the metal surface is treated with a solution include: placing the solution in a polisher comprising a motor and a bowl containing a plurality of stainless steel balls; introducing the coin blank into the bowl; starting the motor; and The coin blanks are left in the polishing machine for at least one minute.

20. The method of claim 13, wherein the base monolayer is deposited at a thickness of 20 to 100 nanometers.

21. A method for manufacturing a metal object, include: forming a shaped article having an outer surface formed at least in part from metal; and The shaped article is surface treated with a solution comprising an alkanethiol and an amount of tartaric acid or a salt thereof effective to remove additional molecules of the alkanethiol beyond a base monolayer of the alkanethiol.

22. The method for manufacturing a metal object according to claim 21, wherein the solution further comprises an emulsifier.

23. The method for manufacturing a metal object according to claim 21, wherein the solution further comprises an antimicrobial agent.