Corrosive liquid for dendritic crystal morphology of 300M steel VAR cast ingot as well as preparation method and application of corrosive liquid
Through the corrosion liquid and corrosion method with specific ratios, the dendrite morphology of the 300M steel VAR ingot is shown, which solves the problem of inability to corrode the dendrite spacing in the prior art, and improves the quality of vacuum self-consumption smelting.
Patent Information
- Application Number
- CN202411184307.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-12-03
AI Technical Summary
The prior art cannot effectively corrode the dendrite spacing of 300M steel VAR ingots, and the dendrite morphology cannot be observed, affecting the quality of the vacuum self-consumption process.
Provide a corrosion liquid composed of alcohol, picric acid, nitric acid and surfactant. The corrosion base liquid, corrosion liquid reinforcement and surfactant are optimized through a specific volume ratio. Combined with grinding, polishing and light corrosion methods, 300M steel is shown. Dental morphology of VAR ingots.
Effectively corrode the dendrite spacing of 300M steel VAR ingots, clearly observe the dendrite morphology, and provide guiding opinions to improve the quality of vacuum self-consumption smelting.
Smart Images

Figure BDA0005013097050000031 
Figure BDA0005013097050000061 
Figure BDA0005013097050000091
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of etching liquid, and in particular to an etching liquid used for 300M steel VAR ingot dendrite morphology, a preparation method and application thereof. Background Art
[0002] 300M steel is an important medium-carbon nickel-chromium-molybdenum steel in the U.S. aviation industry. Compared with other alloy steels, this alloy has ultra-high strength, high yield strength, good plasticity and toughness, and a low proportion of alloy elements, with good plasticity and toughness. At the same time, due to the addition of certain V and Mo elements, the steel has good hardenability. Therefore, 300M steel has become the main material for key components such as modern aircraft landing gear. However, due to the unique composition system of 300M steel, its corrosion resistance is poor. The use of conventional corrosive agents can easily over-corrode the sample, resulting in blurred organization and inability to accurately observe its dendrite morphology.
[0003] The Chinese patent with publication number CN113702124A discloses a test method for obtaining the dendrite morphology of medium-low carbon steel ingots, which comprises: S1, keeping the medium-low carbon steel ingot sample at 50-100°C at austenitizing temperature Ac3 for 10-20 minutes, and then rapidly cooling to room temperature to obtain a martensitic structure; S2, grinding the sample to remove the iron oxide scale and decarburized layer, grinding and polishing to a mirror surface; S3, immersing the sample in a corrosive mixed solution, observing the surface of the sample until it turns black, and then taking it out;
[0004] S4. Use a metallographic microscope with a puzzle shooting function to take puzzle photos of the sample to obtain a complete dendrite structure photo of the sample. The method provided by the present invention overcomes the shortcomings of the prior art that the dendrite morphology test of the ingot is easy to damage the organization and has large errors. By heat treating and lightly corroding the sample, a perfect dendrite structure can be obtained. Combined with a metallographic microscope, it can provide an effective testing method for determining the dendrite structure parameters of medium and low carbon steel ingots. However, since there are still certain Si and Ni in 300M steel, its composition is different from that of ordinary carbon steel, resulting in that the corrosion method suitable for the dendrite spacing of ordinary carbon steel is not applicable to 300M steel.
[0005] The Chinese patent with publication number CN106092708A discloses a method for corrosion visualization of 300M steel grain size, which comprises the following steps: (1) pre-treating a 300M steel grain size sample, wherein the tempering temperature of the 300M steel is 470°C; (2) preparing an etchant for the 300M steel grain size sample; (3) heating the prepared etchant to 33°C and maintaining the temperature constant; (4) placing the treated 300M steel grain size sample in the etchant at a constant temperature. (5) During the corrosion process, continuously wipe the corrosion surface of the 300M steel grain size sample. After wiping for 10 to 20 minutes, take out the 300M steel grain size sample; (6) Use running cold water to wash the 300M steel grain size sample. While washing, wipe the corrosion marks on the corrosion surface of the sample; (7) After washing, drip alcohol on the corrosion surface of the 300M steel grain size sample, and then blow dry the sample; (8) Finally, observe the morphology of the 300M steel grain size sample and evaluate the grain size grade of the sample. The present invention provides a method that focuses on corrosion visualization of 300M steel grain size samples tempered at 470°C. Compared with the original method of corrosion visualization using corrosive agents, the grain boundary display effect is clear, which is helpful for accurately evaluating the grain size grade of 300M steel and provides favorable conditions for the formulation and optimization of the 300M steel production process.
[0006] The Chinese patent with publication number CN103305846A provides a 300M steel metallographic analysis etching solution and an etching method, wherein the etching solution is composed of the following components in weight ratio: 25-50 parts of etching solution component A; 43-70 parts of etching solution component B; 11 parts of corrosion rate regulator 2; 3-6 parts of 2,4,6-trinitroresorcinol; 0.1-1.5 parts of cationic surfactant; the corrosion rate regulator is an ether substance; the etching solution component A is a HNO containing 0.5-2wt% by weight 3 A saturated aqueous solution of picric acid; the etching solution component B is a saturated alcohol solution of picric acid containing 0.1 to 6 wt % of HCl; the etching solution and the etching method of the present invention can be used under not harsh conditions and ordinary materials can be used to achieve clear grain boundary corrosion of 300M steel in a very economical way.
[0007] The above two etching solutions and etching methods for 300M steel can only successfully etch out the grain boundaries and measure the grain size, but cannot be used to corrode VAR ingots, thus unable to measure the secondary dendrite spacing, and unable to provide guidance for VAR smelting. Summary of the invention
[0008] The technical problem solved by the present invention is to provide an etching solution for the dendrite morphology of 300M steel VAR ingot, which can effectively etch out the dendrite spacing of the 300M steel VAR ingot and observe the dendrite morphology.
[0009] In view of this, the present application provides a corrosive solution for 300M steel VAR ingot dendrite morphology, which is composed of the following components in volume ratio:
[0010] 35-45 parts of corrosion base liquid;
[0011] 2-3 parts of corrosion liquid enhancer;
[0012] 3-5 parts of surfactant;
[0013] The corrosion base liquid is composed of the following components in volume ratio:
[0014] 35-45 parts of alcohol;
[0015] 2-3 parts of picric acid;
[0016] Wherein, the concentration of the alcohol is 97%;
[0017] The corrosion liquid intensifier is composed of the following components in volume ratio:
[0018] 30-40 parts of alcohol;
[0019] 3-5 parts of nitric acid;
[0020] Wherein, the concentration of the alcohol is 97%, and the concentration of the nitric acid is 90%;
[0021] The surfactant is composed of the following components in volume ratio:
[0022]
[0023] Preferably, in the corrosion base liquid, the content of the alcohol is 36 to 44 parts, and the content of the picric acid is 2 to 3 parts.
[0024] Preferably, in the corrosion liquid intensifier, the content of the alcohol is 33 to 38 parts, and the content of the nitric acid is 3 to 4 parts.
[0025] Preferably, in the surfactant, the content of water is 17 to 18 parts, and the content of sodium lauryl sulfate is 3 to 4 parts.
[0026] Preferably, the content of the etching base liquid is 36 to 42 parts, and the content of the surfactant is 4 to 5 parts.
[0027] The present application also provides a method for preparing the etching solution for 300M steel VAR ingot dendrite morphology, comprising the following steps:
[0028] Mixing alcohol and picric acid according to volume ratio to obtain a corrosion base liquid;
[0029] Mixing alcohol and nitric acid according to volume ratio to obtain a corrosion liquid intensifier;
[0030] Mix water, sodium lauryl sulfate, potassium hydroxide, ethylparaben, sodium benzoate, sodium chloride, sodium sulfate and sodium hydroxide according to volume ratio to obtain a surfactant;
[0031] The etching base liquid, the etching liquid intensifier and the surfactant are mixed according to the volume ratio to obtain the etching liquid.
[0032] The present application also provides a corrosion method for a 300M steel VAR ingot, comprising the following steps:
[0033] The 300M steel VAR ingot was ground and polished to obtain an initial sample of the 300M steel VAR ingot;
[0034] Wipe the initial sample with alcohol and then blow dry;
[0035] Wipe the surface of the dried sample with the corrosive liquid and rinse the surface of the sample with running water;
[0036] The etching liquid is the etching liquid or the etching liquid prepared by the preparation method.
[0037] Preferably, the temperature of the etching solution is 15-25°C.
[0038] Preferably, the wiping time of the corrosive liquid is 5 to 10 seconds, and the wiping is performed in the same direction.
[0039] Preferably, the drying is carried out by cold air.
[0040] The present application provides a corrosive liquid for the dendritic morphology of 300M steel VAR ingots, which is composed of a corrosive base liquid, a corrosive liquid intensifier and a surfactant in a specific volume ratio. The corrosive base liquid is composed of alcohol and picric acid in a specific volume ratio to etch out the dendritic morphology. The corrosive liquid intensifier is composed of alcohol and nitric acid in a specific volume ratio to accelerate the corrosion rate and enhance the corrosion effect of the corrosive liquid. The surfactant is composed of water, sodium lauryl sulfate, potassium hydroxide, ethyl hydroxybenzoate, sodium benzoate, sodium chloride and sodium hydroxide in a specific volume ratio to achieve the removal of impurities and floating ash and ensure the cleanliness of the sample surface. Therefore, the corrosive liquid provided by the present application can effectively etch out the dendritic spacing of the 300M steel VAR ingot, observe the dendritic morphology, provide guidance for the vacuum consumable process, and improve the quality of vacuum consumable smelting of 300M steel. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 A photograph of the dendrite morphology of a 300M steel VAR ingot after being corroded by the corrosive solution and the corrosive method provided in Example 1 of the present invention (50X);
[0042] Figure 2 A photograph of the dendrite morphology of a 300M steel VAR ingot after being corroded by the corrosive solution and the corrosive method provided in Example 2 of the present invention (50X);
[0043] Figure 3 A photograph of the dendrite morphology of a 300M steel VAR ingot after being corroded by the corrosive solution and the corrosive method provided in Example 3 of the present invention (50X);
[0044] Figure 4 A photograph of the dendrite morphology of a 300M steel VAR ingot after being corroded by the corrosive solution and the corrosive method provided in Comparative Example 1 of the present invention (50X);
[0045] Figure 5 This is a dendrite morphology photograph (50X) of 300M steel VAR ingot after corrosion using the etching solution and etching method provided in Comparative Example 2 of the present invention. DETAILED DESCRIPTION
[0046] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples. However, it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the present invention.
[0047] In view of the problem that it is difficult to etch out good dendrite morphology and measure the secondary dendrite spacing of 300M steel VAR ingots in the prior art, the present invention provides a etching solution for the dendrite morphology of 300M steel VAR ingots, which can effectively etch out the dendrite spacing and observe the dendrite structure by accurately and quantitatively optimizing the components and ratios of the etching base liquid, the etching liquid intensifier and the surfactant. Specifically, the present application provides an etching solution for the dendrite morphology of 300M steel VAR ingots disclosed in an embodiment of the present invention, which is composed of the following components in volume ratio:
[0048] 35-45 parts of corrosion base liquid;
[0049] 2-3 parts of corrosion liquid enhancer;
[0050] 3-5 parts of surfactant;
[0051] The corrosion base liquid is composed of the following components in volume ratio:
[0052] 35-45 parts of alcohol;
[0053] 2-3 parts of picric acid;
[0054] Wherein, the concentration of the alcohol is 97%;
[0055] The corrosion liquid intensifier is composed of the following components in volume ratio:
[0056] 30-40 parts of alcohol;
[0057] 3-5 parts of nitric acid;
[0058] Wherein, the concentration of the alcohol is 97%, and the concentration of the nitric acid is 90%;
[0059] The surfactant is composed of the following components in volume ratio:
[0060]
[0061] In the present application, the components of the etching solution are all formulated in volume fractions.
[0062] Specifically, in the etching solution provided in the present application, the concentration of alcohol in the etching base liquid is 97%, and its content is 35-45 parts, specifically, the content of alcohol is 36-44 parts; for example, the content of alcohol in the present application is 37 parts, 38 parts, 39 parts, 40 parts, 41 parts, 42 parts or 43 parts. The content of picric acid is 2-3 parts, specifically, the content of picric acid is 2 parts or 3 parts.
[0063] The corrosion base liquid can also be called corrosive agent A, wherein picric acid can show the banded segregation and dendritic segregation of 300M steel grade, thereby showing the dendritic morphology, and alcohol is used to dilute the corrosive agent A to prevent excessive corrosion and improve the corrosion contrast.
[0064] The corrosion enhancer is used to accelerate the corrosion rate and strengthen the corrosion effect of the corrosive liquid; it is composed of alcohol and nitric acid in a specific volume ratio, the content of the alcohol is 30-40 parts, specifically, the content of the alcohol is 33-38 parts; for example, the content of the alcohol in this application is 31 parts, 32 parts, 34 parts, 35 parts, 36 parts, 37 parts or 39 parts; the content of the nitric acid is 3-5 parts, specifically, the content of the nitric acid is 3 parts, 4 parts or 5 parts. The concentration of the alcohol is 97%, and the concentration of the nitric acid is 90%.
[0065] The surfactant is composed of water, sodium lauryl sulfate, potassium hydroxide, ethylparaben, sodium benzoate, sodium chloride and sodium hydroxide in a specific volume ratio. Since 300M steel has poor corrosion resistance, impurities are easily adsorbed on the surface during the corrosion process, affecting metallographic observation. Therefore, the surfactant in a specific volume ratio can facilitate the removal of impurities and floating dust to ensure the cleanliness of the sample surface. Specifically, the content of the water is 17 to 18 parts; for example, the content of the water in this application is 16 parts and 19 parts. For example, the content of sodium lauryl sulfate in this application is 3 parts, 4 parts and 5 parts. For example, the content of potassium hydroxide is 2 parts and 3 parts. For example, the content of ethylparaben is 2 parts and 3 parts. For example, the content of sodium benzoate is 1 part and 2 parts. For example, the content of sodium chloride is 2 parts and 3 parts. For example, the content of sodium sulfate is 1 part and 2 parts. For example, the content of sodium hydroxide is 2 parts and 3 parts.
[0066] After the above-mentioned corrosion base liquid, corrosion liquid intensifier and surfactant are prepared, the above-mentioned corrosion base liquid, corrosion liquid intensifier and surfactant are mixed according to the volume ratio, wherein the content of the corrosion base liquid is 35-45 parts; for example, the content of the corrosion base liquid in the present application is 36 parts, 37 parts, 38 parts, 39 parts, 40 parts, 41 parts, 42 parts, 43 parts, 44 parts. The content of the corrosion liquid intensifier is 2-3 parts; for example, the content of the corrosion liquid intensifier in the present application is 2 parts or 3 parts. The content of the surfactant is 3-5 parts; for example, the content of the surfactant in the present application is 3 parts, 4 parts or 5 parts.
[0067] The present application also provides a method for preparing a corrosive solution for 300M steel VAR ingot dendrite morphology, comprising the following steps:
[0068] Mixing alcohol and picric acid according to volume ratio to obtain a corrosion base liquid;
[0069] Mixing alcohol and nitric acid according to volume ratio to obtain a corrosion liquid intensifier;
[0070] Mix water, sodium lauryl sulfate, potassium hydroxide, ethylparaben, sodium benzoate, sodium chloride, sodium sulfate and sodium hydroxide according to volume ratio to obtain a surfactant;
[0071] The etching base liquid, the etching liquid intensifier and the surfactant are mixed according to the volume ratio to obtain the etching liquid.
[0072] Furthermore, the present application also provides a corrosion method for a 300M steel VAR ingot, comprising the following steps:
[0073] The 300M steel VAR ingot was ground and polished to obtain an initial sample of the 300M steel VAR ingot;
[0074] Wipe the initial sample with alcohol and then blow dry;
[0075] Wipe the surface of the dried sample with the corrosive liquid and rinse the surface of the sample with running water;
[0076] The corrosive liquid is the corrosive liquid described in the above scheme.
[0077] The 300M steel VAR ingot is a VAR ingot obtained by vacuum consumable arc melting (VAR) during the preparation of the 300M steel.
[0078] In the above-mentioned corrosion process, the grinding and polishing are technical means well known to those skilled in the art, and the present application does not impose any particular limitation on the specific implementation process.
[0079] After polishing, the obtained initial sample is wiped with alcohol to remove impurities such as residual polishing liquid / paste on the surface, and then blown dry, preferably using a cold air blower perpendicular to the surface of the initial sample.
[0080] Since the corrosion resistance of 300M steel VAR ingot is poor, it is necessary to control the temperature of the etching solution to avoid excessively high temperature of the etching solution, which will cause over-corrosion of the sample and fail to obtain an ideal dendrite morphology. The temperature of the etching solution is 15-25°C, specifically, the temperature of the etching solution is 18-24°C, and more specifically, the temperature of the etching solution is 19-22°C.
[0081] In the process of corroding the sample surface with a corrosive liquid, it is preferred to use a cotton ball to dip into the corrosive liquid, wipe the sample surface while rinsing the surface with running water, and wipe it multiple times in the same direction. After about 5 to 10 seconds, the sample surface loses its metallic luster and visible dendrite structure appears on the surface. After drying with a hair dryer, take a photo of the dendrite morphology under a microscope, and then use relevant software to measure the secondary dendrite spacing.
[0082] In view of the problem that it is difficult to corrode a good dendrite morphology and measure the secondary dendrite spacing of the existing 300M steel VAR ingot, the present invention optimizes the ratio of the corrosion base liquid, the corrosion liquid intensifier and the surfactant, and accurately and quantitatively provides a corrosion liquid that can corrode the secondary dendrites of the 300M steel VAR ingot. The corrosion liquid can effectively corrode the dendrite spacing of the 300M steel VAR ingot, so as to facilitate the observation of the dendrite morphology, provide guidance for the vacuum consumable process, and improve the quality of the vacuum consumable smelting of 300M steel.
[0083] In order to further understand the present invention, the etching liquid and etching method for the dendrite morphology of 300M steel VAR ingot provided by the present invention are described in detail in combination with the embodiments below. The protection scope of the present invention is not limited by the following embodiments.
[0084] Example 1
[0085] The composition of the corrosive agent A is:
[0086] 45 parts of 97% alcohol;
[0087] 3 parts of picric acid;
[0088] The composition of the corrosion liquid enhancer B is:
[0089] 40 parts of 97% alcohol;
[0090] 3 parts of 90% nitric acid;
[0091] The composition of surfactant C is:
[0092]
[0093] The composition of the corrosive liquid is:
[0094] Etching agent A 42 parts;
[0095] 2 parts of corrosion liquid enhancer B;
[0096] Surfactant C 4 parts;
[0097] The present invention utilizes the above-mentioned corrosive liquid to corrode the metallographic specimen of 300M steel VAR ingot, and the method is as follows:
[0098] 1) Mix the above-mentioned components in the above-mentioned volume ratio in a beaker and stir slowly with a glass rod. Then grind and polish the metallographic sample of 300M steel VAR ingot according to the conventional metallographic analysis method. Use a cotton ball dipped in alcohol to gently wipe the surface of the sample to wipe off impurities such as residual polishing paste on the surface. Use a cold air blower to blow dry perpendicularly to the surface of the sample.
[0099] 2) Use a thermometer to measure the temperature of the prepared etchant, and start corrosion after the temperature drops to 24°C;
[0100] 3) Use a cotton ball to dip in the corrosive agent, wipe the surface of the sample while rinsing the surface with running water, and wipe multiple times in the same direction. After about 8 seconds, the surface of the sample loses its metallic luster, and visible dendrites appear on the surface. After drying with a hair dryer, take photos of the dendrite morphology under a microscope, and then use relevant software to measure the secondary dendrite spacing.
[0101] like Figure 1 As shown, Figure 1 This is a photo of the dendrite morphology of 300M steel VAR ingot after corrosion. Figure 1 The dendrite morphology can be clearly seen, and the secondary dendrite spacing can be measured.
[0102] Example 2
[0103] A corrosive solution for 300M steel VAR ingot dendrite morphology, which is composed of the following components in weight ratio:
[0104] The composition of the corrosive agent A is:
[0105] 44 parts of 97% alcohol;
[0106] 3 parts of picric acid;
[0107] The composition of the corrosion liquid enhancer B is:
[0108] 38 parts of 97% alcohol;
[0109] 3 parts of 90% nitric acid;
[0110] The composition of surfactant C is:
[0111]
[0112] The composition of the corrosive liquid is:
[0113] Etching agent A 40 parts;
[0114] 3 parts of corrosion liquid enhancer B;
[0115] Surfactant C 3 parts;
[0116] The present invention utilizes the above-mentioned corrosive liquid to corrode the metallographic specimen of 300M steel VAR ingot, and the method is as follows:
[0117] 1) Mix the above-mentioned components in the above-mentioned volume ratio in a beaker and stir slowly with a glass rod. Then grind and polish the metallographic sample of 300M steel VAR ingot according to the conventional metallographic analysis method. Use a cotton ball dipped in alcohol to gently wipe the surface of the sample to wipe off impurities such as residual polishing paste on the surface. Use a cold air blower to blow dry perpendicularly to the surface of the sample.
[0118] 2) Use a thermometer to measure the temperature of the prepared corrosive agent, and start corrosion after the temperature drops to 22°C;
[0119] 3) Use a cotton ball to dip in the corrosive agent, wipe the surface of the sample while rinsing the surface with running water, and wipe it multiple times in the same direction. After about 7 seconds, the surface of the sample loses its metallic luster, and visible dendrites appear on the surface. After drying with a hair dryer, take photos of the dendrite morphology under a microscope, and then use relevant software to measure the secondary dendrite spacing.
[0120] like Figure 2 As shown, Figure 2 This is a photo of the dendrite morphology of 300M steel VAR ingot after corrosion. Figure 2The dendrite morphology can be clearly seen, and the secondary dendrite spacing can be measured.
[0121] Example 3
[0122] The composition of the corrosive agent A is:
[0123] 36 parts of 97% alcohol;
[0124] 3 parts of picric acid;
[0125] The composition of the corrosion liquid enhancer B is:
[0126] 33 parts of 97% alcohol;
[0127] 3 parts of 90% nitric acid;
[0128] The composition of surfactant C is:
[0129]
[0130] The composition of the corrosive liquid is:
[0131] Etching agent A 38 parts;
[0132] 3 parts of corrosion liquid enhancer B;
[0133] Surfactant C 5 parts;
[0134] The present invention utilizes the above-mentioned corrosive liquid to corrode the metallographic specimen of 300M steel VAR ingot, and the method is as follows:
[0135] 1) Mix the above-mentioned components in the above-mentioned volume ratio in a beaker and stir slowly with a glass rod. Then grind and polish the metallographic sample of 300M steel VAR ingot according to the conventional metallographic analysis method. Use a cotton ball dipped in alcohol to gently wipe the surface of the sample to wipe off impurities such as residual polishing paste on the surface. Use a cold air blower to blow dry perpendicularly to the surface of the sample.
[0136] 2) Use a thermometer to measure the temperature of the prepared etchant, and start corrosion after the temperature drops to 18°C;
[0137] 3) Use a cotton ball to dip in the corrosive agent, wipe the surface of the sample while rinsing the surface with running water, and wipe it multiple times in the same direction. After about 10 seconds, the surface of the sample loses its metallic luster, and visible dendrites appear on the surface. After drying with a hair dryer, take a photo of the dendrite morphology under a microscope, and then use relevant software to measure the secondary dendrite spacing.
[0138] like Figure 3 As shown, Figure 3 This is a photo of the dendrite morphology of 300M steel VAR ingot after corrosion. Figure 3The dendrite morphology can be clearly seen, and the secondary dendrite spacing can be measured.
[0139] Comparative Example 1
[0140] The same as Example 1, except that: the etching solution is composed of 40 parts of etching agent A and 5 parts of surfactant C, and does not contain the etching enhancer B;
[0141] 1) Mix the above-mentioned components in the above-mentioned volume ratio in a beaker and stir slowly with a glass rod. Then grind and polish the metallographic sample of 300M steel VAR ingot according to the conventional metallographic analysis method. Use a cotton ball dipped in alcohol to gently wipe the surface of the sample to wipe off impurities such as residual polishing paste on the surface. Use a cold air blower to blow dry perpendicularly to the surface of the sample.
[0142] 2) Use a thermometer to measure the temperature of the prepared etchant, and start corrosion after the temperature drops to 30°C;
[0143] 3) Use a cotton ball to dip in the corrosive agent, wipe the surface of the sample while rinsing the surface with running water, and wipe it multiple times in the same direction. After about 8 seconds, the surface of the sample loses its metallic luster, and visible dendrites appear on the surface. However, there are large areas of uncorroded dendrites in some places, indicating that the corrosion is not thorough. Figure 4 shown.
[0144] Comparative Example 2
[0145] The same as Example 1, except that: the etching solution is composed of 42 parts of etching agent A and 3 parts of etching enhancer B, and does not contain surfactant C;
[0146] 1) Mix the above-mentioned components in the above-mentioned volume ratio in a beaker and stir slowly with a glass rod. Then grind and polish the metallographic sample of 300M steel VAR ingot according to the conventional metallographic analysis method. Use a cotton ball dipped in alcohol to gently wipe the surface of the sample to wipe off impurities such as residual polishing paste on the surface. Use a cold air blower to blow dry perpendicularly to the surface of the sample.
[0147] 2) Use a thermometer to measure the temperature of the prepared etchant, and start corrosion after the temperature drops to 24°C;
[0148] 3) Use a cotton ball to dip in the corrosive agent, wipe the surface of the sample while rinsing the surface with running water, and wipe it several times in the same direction. After about 10 seconds, the surface of the sample loses its metallic luster, and visible dendrites appear on the surface. The boundaries of the dendrites are obvious, but there are many black dot-like impurities on the surface of the sample, which affect the observation of the sample. Figure 5 shown.
[0149] The above embodiments are only used to help understand the method and core idea of the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made to the present invention without departing from the principles of the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.
[0150] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. An etching solution for the dendrite morphology of 300M steel VAR ingots, comprising the following components in volume ratio: 35-45 parts of corrosion base liquid; 2-3 parts of corrosion liquid enhancer; 3-5 parts of surfactant; The corrosion base liquid is composed of the following components in volume ratio: 35-45 parts of alcohol; 2-3 parts of picric acid; Wherein, the concentration of the alcohol is 97%; The corrosion liquid intensifier is composed of the following components in volume ratio: 30-40 parts of alcohol; 3-5 parts of nitric acid; Wherein, the concentration of the alcohol is 97%, and the concentration of the nitric acid is 90%; The surfactant is composed of the following components in volume ratio:
2. The etching solution according to claim 1, characterized in that: In the corrosion base liquid, the content of the alcohol is 36 to 44 parts, and the content of the picric acid is 2 to 3 parts.
3. The etching solution according to claim 1, characterized in that: In the etching liquid intensifier, the content of the alcohol is 33 to 38 parts, and the content of the nitric acid is 3 to 4 parts.
4. The etching solution according to claim 1, characterized in that: In the surfactant, the content of water is 17 to 18 parts, and the content of sodium lauryl sulfate is 3 to 4 parts.
5. The etching solution according to claim 1, characterized in that: The content of the corrosion base liquid is 36-42 parts, and the content of the surfactant is 4-5 parts.
6. The method for preparing the etching solution for 300M steel VAR ingot dendrite morphology according to claim 1, comprising the following steps: Mixing alcohol and picric acid according to volume ratio to obtain a corrosion base liquid; Mixing alcohol and nitric acid according to volume ratio to obtain a corrosion liquid intensifier; Mix water, sodium lauryl sulfate, potassium hydroxide, ethylparaben, sodium benzoate, sodium chloride, sodium sulfate and sodium hydroxide according to volume ratio to obtain a surfactant; The etching base liquid, the etching liquid intensifier and the surfactant are mixed according to the volume ratio to obtain the etching liquid.
7. A method for corroding a 300M steel VAR ingot, comprising the following steps: The 300M steel VAR ingot was ground and polished to obtain an initial sample of the 300M steel VAR ingot; Wipe the initial sample with alcohol and then blow dry; Wipe the surface of the dried sample with the corrosive liquid and rinse the surface of the sample with running water; The etching liquid is the etching liquid according to any one of claims 1 to 5 or the etching liquid prepared by the preparation method according to claim 6.
8. The etching method according to claim 7, characterized in that: The temperature of the etching solution is 15-25°C.
9. The etching method according to claim 7, characterized in that: The wiping time of the corrosive liquid is 5 to 10 seconds, and the wiping is carried out in the same direction.
10. The etching method according to claim 7, characterized in that: The drying is carried out by cold air.