Cleaning method of graphite piece for silicon carbide epitaxial growth and silicon carbide epitaxial growth device

By inserting alkali vapor into the silicon carbide epitaxial furnace chamber to clean graphite parts, the problem of by-product deposition during the silicon carbide epitaxial process is solved, and a convenient cleaning process is achieved, which improves process stability and reduces costs.

CN119061472APending Publication Date: 2024-12-03ZJU HANGZHOU GLOBAL SCI & TECH INNOVATION CENT
View PDF 17 Cites 0 Cited by

Patent Information

Application Number
CN202411571341.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-11-06
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

During the process of silicon carbide epitaxial, silicon carbide by-products and particulate matter deposited on the surface of graphite parts lead to fallen objects and triangular defects, affecting the quality of the film. The existing technology requires manual disassembly and polishing, and needs to be baked and cleaned, which is cumbersome and inconvenient.

Method used

The graphite parts are cleaned by injecting alkali vapor into the epitaxial furnace chamber. The alkali vapor reacts with the silicon carbide by-product to remove them, and the cleaning is achieved without dismantling the graphite parts and baking.

Benefits of technology

It realizes convenient cleaning of graphite parts, improves process stability, reduces production costs, avoids liquid wetting, and significantly improves the quality of silicon carbide epitaxial film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119061472A_ABST
    Figure CN119061472A_ABST
Patent Text Reader

Abstract

The invention relates to a cleaning method for a graphite piece for silicon carbide epitaxial growth and a silicon carbide epitaxial growth device.According to the cleaning method for the graphite piece for silicon carbide epitaxial growth, the graphite piece installed in a furnace cavity of an epitaxial furnace is cleaned, and the furnace cavity is provided with a gas inlet and a tail gas outlet; the cleaning method comprises the step of continuously introducing alkali steam into the furnace chamber of the epitaxial furnace through the air inlet. According to the cleaning method, the graphite piece does not need to be detached from the epitaxial furnace, the graphite piece can be directly cleaned in situ, the steps of detaching and installing the graphite piece are omitted, the cleaning method is very convenient, the process stability is remarkably improved, and the production cost is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of silicon carbide epitaxial film preparation, and in particular to a method for cleaning a graphite piece used for silicon carbide epitaxial growth and a silicon carbide epitaxial growth device. Background Art

[0002] As a third-generation semiconductor material, silicon carbide (4H-SiC) has good physical and electrical properties. In the epitaxial process of 4H-SiC thin films, chemical vapor deposition is mainly used. Chemical vapor deposition usually uses graphite as the substrate of silicon carbide. The commonly used heating method is hot wall heating, that is, the graphite in the entire growth chamber needs to be heated. This results in a layer of silicon carbide byproducts and particulate matter on the surface of the graphite after multiple epitaxial growth processes. These deposits will produce a large number of drops and triangular defects during the epitaxial process, which seriously affects the quality of the silicon carbide epitaxial film. At present, after the silicon carbide film is epitaxially grown to a certain thickness, the graphite part needs to be removed from the furnace chamber of the epitaxial furnace, and the graphite is manually polished to clean the silicon carbide byproducts on the surface of the graphite part before reloading the furnace. After the graphite part is reloaded into the furnace, it needs to be baked several times before it can continue to be used, which makes the cleaning of the graphite part very inconvenient. Summary of the invention

[0003] Based on this, it is necessary to provide a method for cleaning a graphite part used for epitaxial growth of silicon carbide and a silicon carbide epitaxial growth device, which can conveniently clean the graphite part used for epitaxial growth of silicon carbide.

[0004] The present application provides a method for cleaning graphite parts used for silicon carbide epitaxial growth, which is used to clean graphite parts installed in a furnace chamber of an epitaxial furnace. The furnace chamber has an air inlet and an exhaust gas outlet. The cleaning method comprises: continuously introducing alkaline vapor into the furnace chamber of the epitaxial furnace through the air inlet.

[0005] In one of the embodiments, the temperature of the alkaline vapor introduced into the furnace chamber of the epitaxial furnace is 900°C to 1400°C.

[0006] In one embodiment, when the alkali vapor is introduced, the pressure of the furnace chamber of the epitaxial furnace is 100 mbar to 800 mbar.

[0007] In one embodiment, the flow rate of the alkali vapor is 100 sccm-1000 sccm, and the time for introducing the alkali vapor is controlled to be 60 min-90 min.

[0008] In one embodiment, the air inlet is connected to a high-temperature furnace, and the high-temperature furnace and the air inlet are communicated. Before the alkali vapor is introduced into the furnace chamber of the epitaxial furnace, the solid alkali is first placed in the crucible of the high-temperature furnace, and then the high-temperature furnace is heated to 360°C~600°C to convert the solid alkali into molten alkali, and maintained for 10min~30min, and then heated to 900°C~1400°C to obtain alkali vapor.

[0009] In one embodiment, the solid base is potassium hydroxide or sodium hydroxide.

[0010] In one embodiment, after the introduction of alkali vapor is stopped and the furnace chamber of the epitaxial furnace is cooled to room temperature, an inert gas is introduced into the furnace chamber through the air inlet to purge the furnace chamber, so that the epitaxial reaction byproducts on the graphite parts are cleaned.

[0011] In one embodiment, the inert gas is argon.

[0012] The present application also provides a silicon carbide epitaxial growth device, comprising: an epitaxial furnace and a high-temperature furnace, the epitaxial furnace having a furnace chamber, the furnace chamber having an air inlet and an exhaust gas outlet, a graphite part for silicon carbide epitaxial growth installed in the furnace chamber, the high-temperature furnace being connected to the air inlet, and the high-temperature furnace being communicated with the air inlet, and the silicon carbide epitaxial growth device is used to implement the above-mentioned cleaning method.

[0013] In one of the embodiments, the air inlet and the exhaust gas outlet are respectively located at two ends of the furnace cavity.

[0014] Compared with the prior art, the cleaning method for graphite parts for silicon carbide epitaxial growth and the silicon carbide epitaxial growth device provided by the present application allow alkaline vapor to be introduced to clean the graphite parts. Since the alkaline vapor can react with the silicon carbide byproducts, the silicon carbide byproducts fall off the surface of the graphite parts, thereby achieving the cleaning of the graphite parts. The cleaning method does not require the graphite parts to be removed from the epitaxial furnace, and the graphite parts can be cleaned directly in situ, eliminating the steps of disassembling and installing the graphite parts, and eliminating the step of baking the graphite parts. It is very convenient, and significantly improves the process stability and reduces the production cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] In order to more clearly illustrate the technical solutions in the embodiments of the present application or the conventional technology, the drawings required for use in the embodiments or the conventional technology descriptions are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0016] Figure 1This is a schematic structural diagram of a silicon carbide epitaxial growth device according to an embodiment of the present application; Figure 2 This is a comparison diagram of the surface of a graphite part before and after cleaning using the cleaning method of Example 1; Figure 3 This is a comparison diagram of the surface of a graphite part before and after cleaning using the cleaning method of Example 2; Figure 4 This is a comparison diagram of the surface of a graphite part before and after cleaning using the cleaning method of Example 3; Figure 5 This is a comparison diagram of the surface of a graphite part before and after cleaning using the cleaning method of Example 4; Figure 6 This is a comparison diagram of the surface of a graphite part before and after cleaning using the cleaning method of Example 5.

[0017] Figure numerals: 1, high temperature furnace; 2, crucible; 3, epitaxial furnace; 31, furnace chamber; 32, air inlet; 33, exhaust gas outlet; 4, graphite part; 5, silicon carbide by-product. DETAILED DESCRIPTION

[0018] In order to make the above-mentioned purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are described in detail below in conjunction with the accompanying drawings. In the following description, many specific details are set forth to facilitate a full understanding of the present application. However, the present application can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present application, so the present application is not limited by the specific embodiments disclosed below.

[0019] It should be noted that when a component is referred to as being "fixed to" or "disposed on" another component, it may be directly on the other component or there may also be a central component. When a component is considered to be "connected to" another component, it may be directly connected to the other component or there may be a central component at the same time. The terms "vertical", "horizontal", "upper", "lower", "left", "right" and similar expressions used in the specification of this application are for illustrative purposes only and do not represent the only implementation method.

[0020] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In the description of this application, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.

[0021] In the present application, unless otherwise clearly specified and limited, a first feature being “above” or “below” a second feature may mean that the first feature is directly in contact with the second feature, or the first feature and the second feature are indirectly in contact through an intermediate medium. Moreover, a first feature being “above”, “above” or “above” a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being “below”, “below” or “below” a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.

[0022] Unless otherwise defined, all technical and scientific terms used in the specification of this application have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application. The term "and / or" used in the specification of this application includes any and all combinations of one or more related listed items.

[0023] Please combine Figure 1 As shown, the present application provides a cleaning method for a graphite piece for epitaxial growth of silicon carbide, wherein a graphite piece 4 installed in a furnace chamber 31 of an epitaxial furnace 3 is cleaned, and the furnace chamber 31 has an air inlet 32 ​​and an exhaust gas outlet 33, and the cleaning method comprises: continuously introducing alkali vapor into the furnace chamber 31 of the epitaxial furnace 3 through the air inlet 32. In this way, the alkali vapor can react with the silicon carbide byproduct 5, so that the silicon carbide byproduct 5 falls off from the surface of the graphite piece 4, thereby achieving the cleaning of the graphite piece 4. The cleaning method does not need to remove the graphite piece 4 from the epitaxial furnace 3, and the graphite piece 4 can be directly cleaned in situ, eliminating the steps of disassembling and installing the graphite piece 4, and eliminating the step of baking the graphite piece 4, which is very convenient, and significantly improves the process stability and reduces the production cost. In addition, since the alkali vapor is a gas rather than a liquid, the situation where the graphite piece 4 is wetted by the liquid is avoided, thereby eliminating the step of baking the graphite piece 4.

[0024] It is understood that when the silicon carbide epitaxial reaction is carried out, the silicon carbide substrate is set on the graphite part 4, and the reaction gas is introduced from the air inlet 32 ​​for reaction, and the reaction tail gas is discharged from the tail gas outlet 33. After the silicon carbide film is epitaxially grown to a certain thickness, the reaction is terminated, and then the silicon carbide substrate is removed, and then alkali vapor is introduced to clean the graphite part 4. Alkaline vapor is also introduced into the furnace chamber 31 of the epitaxial furnace 3 from the air inlet 32, and the reaction tail gas is discharged from the tail gas outlet 33. Although Figure 1Only one air inlet 32 ​​is illustrated, but the invention is not limited thereto. The number of the air inlets 32 may be one or more. When the air inlets 32 are multiple, the reaction gas of the epitaxial reaction and the alkaline vapor for cleaning may be introduced into the furnace chamber 31 of the epitaxial furnace 3 from the same air inlet 32, or may be introduced into the furnace chamber 31 of the epitaxial furnace 3 from different air inlets 32. The present application does not impose any limitation on this.

[0025] Furthermore, the temperature of the alkali vapor introduced into the furnace chamber 31 of the epitaxial furnace 3 is 900° C. to 1400° C. Thus, the temperature of the alkali vapor is greater than or equal to 900° C., ensuring that the alkali vapor is always gas and does not become liquid, thereby avoiding the situation where the graphite piece 4 is wetted by the liquid, thereby eliminating the step of baking the graphite piece 4. At the same time, the temperature of the alkali vapor is less than or equal to 1400° C., which saves energy consumption while ensuring that the alkali vapor is gas, thereby reducing the cleaning cost.

[0026] In some specific embodiments, the temperature of the alkaline vapor introduced into the furnace chamber 31 of the epitaxial furnace 3 can be 900°C, 950°C, 1000°C, 1050°C, 1100°C, 1150°C, 1200°C, 1250°C, 1300°C, 1350°C, 1400°C, or any other value within the range of 900°C to 1400°C.

[0027] Furthermore, when the alkali vapor is introduced, the pressure of the furnace chamber 31 of the epitaxial furnace 3 is 100 mbar to 800 mbar. In this way, the alkali vapor is ensured to fully react with the silicon carbide byproduct 5, thereby ensuring the cleaning effect of the graphite part 4.

[0028] In some specific implementations, when alkali vapor is introduced, the pressure of the furnace chamber 31 of the epitaxial furnace 3 is 100 mbar, 150 mbar, 200 mbar, 250 mbar, 300 mbar, 350 mbar, 400 mbar, 450 mbar, 500 mbar, 550 mbar, 600 mbar, 650 mbar, 700 mbar, 750 mbar, 800 mbar, or any other value in the range of 100 mbar to 800 mbar.

[0029] Further, the flow rate of the alkali vapor is 100sccm~1000sccm, and the time for passing the alkali vapor is controlled at 60min~90min. In this way, it is ensured that a sufficient amount of alkali vapor is passed, so as to ensure that the alkali vapor and the silicon carbide byproduct 5 are fully reacted, and then the graphite part 4 is cleaned. In some specific embodiments, the flow rate of the alkali vapor can be 100sccm, 200ccm, 300sccm, 400sccm, 500sccm, 600sccm, 700sccm, 800sccm, 900sccm, 1000sccm, or any other value within the range of 100sccm~1000sccm. In some specific embodiments, the time for passing the alkali vapor can be controlled at 60min, 65min, 70min, 75min, 80min, 85min, 90min, or any other value within the range of 60min~90min.

[0030] Further, the air inlet 32 ​​is connected to the high temperature furnace 1, and the high temperature furnace 1 is connected to the air inlet 32. Before the alkali vapor is introduced into the furnace chamber 31 of the epitaxial furnace 3, the solid alkali is first placed in the crucible 2 of the high temperature furnace 1, and then the high temperature furnace 1 is heated to 360°C~600°C so that the solid alkali becomes molten alkali, and maintained for 10min~30min, and then heated to 900°C~1400°C to obtain alkali vapor. In this way, it is very convenient to use solid alkali as a raw material. It avoids the direct use of alkali vapor as a raw material, which leads to inconvenience in transportation and storage, thereby increasing costs. When in use, first heat up to 360°C~600°C and maintain for 10min~30min, which can ensure that all solid alkalis become molten alkalis, thereby ensuring that the molten alkali can be quickly converted into alkali vapor when the temperature is raised to 900°C~1400°C, and the flow rate of alkali vapor entering the furnace chamber 31 of the epitaxial furnace 3 is ensured. It can be understood that when the high-temperature furnace 1 is heated for the first time, the temperature can be raised to 360°C, 400°C, 450°C, 500°C, 550°C, 600°C, or any other value in the range of 360°C to 600°C, and the holding time at this temperature can be 10min, 15min, 20min, 25min, 30min, or any other value in the range of 10min to 30min.

[0031] Furthermore, the solid alkali is potassium hydroxide or sodium hydroxide. Potassium hydroxide and sodium hydroxide are both common alkalis and can react well with the silicon carbide by-product 5 so that the silicon carbide by-product 5 falls off the surface of the graphite piece 4.

[0032] It is understandable that the amount of alkali vapor introduced into the furnace chamber 31 of the epitaxial furnace 3 is determined according to the amount of silicon carbide byproducts 5 attached to the graphite piece 4, as long as the alkali vapor can clean the silicon carbide byproducts 5 on the surface of the graphite piece 4. Further, the solid alkali placed in the crucible 2 of the high-temperature furnace 1 is 10g~2000g, so that sufficient alkali vapor is generated at high temperature, thereby ensuring that the silicon carbide byproducts 5 on the surface of the graphite piece 4 are cleaned. Specifically, the solid alkali placed in the crucible 2 of the high-temperature furnace 1 can be 10g, 50g, 100g, 200g, 300g, 400g, 500g, 600g, 700g, 800g, 900g, 1000g, 1100g, 1200g, 1300g, 1400g, 1500g, 1600g, 1700g, 1800g, 1900g, 2000g, or any other value within the range of 10g~2000g.

[0033] Furthermore, after the introduction of the alkali vapor is stopped, the high temperature furnace 1 is turned off to allow the high temperature furnace 1 to cool to room temperature, thereby preventing the alkali vapor from being further generated.

[0034] Furthermore, after the introduction of alkali vapor is stopped, an inert gas is introduced into the furnace chamber 31 through the air inlet 32 ​​to purge the furnace chamber 31, so that the epitaxial reaction byproducts (i.e., silicon carbide byproducts 5) on the graphite piece 4 are purged clean, so that the epitaxial furnace 3 can be directly used for the next epitaxial reaction after the inert gas purge, which is very convenient. It is worth mentioning that when the alkali vapor is introduced to clean the graphite piece 4 in the furnace chamber 31, the epitaxial furnace 3 is not heated, that is, the epitaxial furnace 3 is at room temperature. In the present application, "introducing an inert gas into the furnace chamber 31 through the air inlet 32 ​​to purge the furnace chamber 31" is performed after the step of "closing the high-temperature furnace 1 to cool the high-temperature furnace 1 to room temperature".

[0035] In one embodiment, the inert gas is argon. When the argon gas is introduced to purge the furnace chamber 31, the purging may be performed 3 to 5 times to ensure that the silicon carbide byproduct 5 is purged cleanly.

[0036] In one embodiment, the cleaning method of the graphite piece 4 for epitaxial growth of silicon carbide provided by the present application comprises: first putting 10g~2000g of solid alkali into the crucible 2 of the high temperature furnace 1. Then the high temperature furnace 1 is heated to 360℃~600℃ so that the solid alkali becomes molten alkali, and maintained for 10min~30min. Then the temperature is raised to 900℃~1400℃ to obtain alkali vapor with a temperature of 900℃~1400℃. The alkali vapor is introduced into the furnace chamber 31 of the epitaxial furnace 3 so that the pressure of the furnace chamber 31 is 100mbar~800mbar, the flow rate of the alkali vapor is 100sccm~1000sccm, and the time of introducing the alkali vapor is controlled at 60min~90min, then the introduction of the alkali vapor is stopped, the high temperature furnace 1 is closed so that the high temperature furnace 1 is cooled to room temperature, and argon gas is introduced into the furnace chamber 31 of the epitaxial furnace 3 to purge the furnace chamber 31 3 times~5 times, so that the silicon carbide byproduct 5 is purged clean.

[0037] For further information, see Figure 1 The present application also provides a silicon carbide epitaxial growth device, including: an epitaxial furnace 3 and a high-temperature furnace 1, the epitaxial furnace 3 has a furnace chamber 31, the furnace chamber 31 has an air inlet 32 ​​and an exhaust gas outlet 33, a graphite piece 4 for silicon carbide epitaxial growth is installed in the furnace chamber 31, the high-temperature furnace 1 is connected to the air inlet 32, and the high-temperature furnace 1 is connected to the air inlet 32, and the silicon carbide epitaxial growth device is used to implement the above-mentioned cleaning method. When implementing the above-mentioned cleaning method, it is not necessary to remove the graphite piece 4, and the graphite piece 4 is cleaned by directly introducing alkaline vapor into the furnace chamber 31 of the epitaxial furnace 3, which is very convenient.

[0038] In this embodiment, the gas inlet 32 ​​and the tail gas outlet 33 are respectively located at two ends of the furnace chamber 31. In this way, it is ensured that the gas can clean every corner of the furnace chamber 31 of the epitaxial furnace 3.

[0039] The following is a method for cleaning a graphite piece used for epitaxial growth of silicon carbide in combination with a specific embodiment, namely Figure 1 A method for cleaning the silicon carbide epitaxial growth apparatus is described below.

[0040] Example 1 The cleaning method of graphite parts for epitaxial growth of silicon carbide includes: firstly putting 10g of solid alkali (sodium hydroxide) into a crucible of a high temperature furnace, then heating the high temperature furnace to 360°C to convert the solid alkali into molten alkali, and maintaining it for 10 minutes, then heating it to 900°C to obtain alkali vapor at a temperature of 900°C. The alkali vapor is introduced into the furnace chamber of the epitaxial furnace, so that the pressure of the furnace chamber is 100mbar, the flow rate of the alkali vapor is 100sccm, and the time of introducing the alkali vapor is controlled to be 60min, after which the introduction of the alkali vapor is completed, the high temperature furnace is closed and cooled to room temperature, and argon gas is introduced into the furnace chamber of the epitaxial furnace to purge the furnace chamber three times, so that the silicon carbide by-products are purged cleanly.

[0041] Example 2 The cleaning method of graphite parts used for epitaxial growth of silicon carbide includes: firstly putting 300g of solid alkali (sodium hydroxide) into a crucible of a high-temperature furnace, then heating the high-temperature furnace to 400°C to convert the solid alkali into molten alkali, and maintaining it for 20 minutes, and then heating it to 1000°C to obtain alkali vapor with a temperature of 1000°C. The alkali vapor is introduced into the furnace chamber of the epitaxial furnace, so that the pressure of the furnace chamber is 300mbar, the flow rate of the alkali vapor is 300sccm, and the time for introducing the alkali vapor is controlled to be 70min, after which the introduction of the alkali vapor is completed, the high-temperature furnace is closed and cooled to room temperature, and argon gas is introduced into the furnace chamber of the epitaxial furnace to purge the furnace chamber three times, so that the silicon carbide by-products are purged cleanly.

[0042] Example 3 The cleaning method of graphite parts for epitaxial growth of silicon carbide includes: firstly putting 1000g of solid alkali (sodium hydroxide) into a crucible of a high temperature furnace, then heating the high temperature furnace to 500°C to convert the solid alkali into molten alkali, and maintaining it for 25 minutes, then heating it to 1200°C to obtain alkali vapor at a temperature of 1200°C. The alkali vapor is introduced into the furnace chamber of the epitaxial furnace, so that the pressure of the furnace chamber is 500mbar, the flow rate of the alkali vapor is 800sccm, and the time of introducing the alkali vapor is controlled to be 80min, after which the introduction of the alkali vapor is completed, the high temperature furnace is closed to cool the high temperature furnace to room temperature, and argon gas is introduced into the furnace chamber of the epitaxial furnace to purge the furnace chamber 4 times, so that the silicon carbide by-products are purged cleanly.

[0043] Example 4 The cleaning method of graphite parts for epitaxial growth of silicon carbide includes: firstly putting 2000g of solid alkali (sodium hydroxide) into a crucible of a high temperature furnace, then heating the high temperature furnace to 600°C to convert the solid alkali into molten alkali, and maintaining it for 30 minutes, then heating it to 1400°C to obtain alkali vapor at a temperature of 1400°C. The alkali vapor is introduced into the furnace chamber of the epitaxial furnace, so that the pressure of the furnace chamber is 800mbar, the flow rate of the alkali vapor is 1000sccm, and the time of introducing the alkali vapor is controlled to be 90min, after which the introduction of the alkali vapor is completed, the high temperature furnace is closed to cool the high temperature furnace to room temperature, and argon gas is introduced into the furnace chamber of the epitaxial furnace to purge the furnace chamber 5 times, so that the silicon carbide by-products are purged cleanly.

[0044] Example 5 The difference between Example 5 and Example 3 is that the alkali is potassium hydroxide, and the high-temperature furnace is heated to 500°C to convert the solid alkali into molten alkali, and maintained for 30 minutes, and then heated to 1350°C to obtain alkali vapor. The pressure of the alkali vapor entering the furnace chamber of the epitaxial furnace is 120 mbar, the flow rate of the alkali vapor is 500 sccm, and the time for passing the alkali vapor is controlled at 80 minutes.

[0045] Take photos of the graphite parts before and after cleaning, and obtain the comparison pictures of the graphite parts before and after cleaning. Figures 2 to 6 ,in, Figure 2 This is a comparison diagram of the surface of the graphite part before and after cleaning using the cleaning method of Example 1. Figure 3 This is a comparison diagram of the surface of the graphite part before and after cleaning using the cleaning method of Example 2. Figure 4 This is a comparison diagram of the surface of the graphite part before and after cleaning using the cleaning method of Example 3. Figure 5 This is a comparison diagram of the surface of a graphite part before and after cleaning using the cleaning method of Example 4. Figure 6 This is a comparison diagram of the surface of a graphite part before and after cleaning using the cleaning method of Example 5. Figure 2-Figure 6 In the figure, A represents the graphite part before cleaning, and B represents the graphite part after cleaning.

[0046] according to Figures 2 to 6 It can be seen that after the epitaxial reaction is completed, a large amount of particulate matter, i.e., silicon carbide by-products, is attached to the surface of the graphite part. After cleaning by the cleaning method of Examples 1-5, the particulate matter falls off, and the original appearance of the graphite part is basically restored. It can be seen that the silicon carbide by-products have been cleaned. It can be seen that the cleaning method of the graphite part for silicon carbide epitaxial growth provided by the present application has a good cleaning effect on the graphite part. However, the prior art needs to remove the graphite part from the epitaxial furnace after the epitaxial growth of silicon carbide is completed, and then clean the silicon carbide by-products on the surface of the graphite part by manual polishing. After that, the graphite part is reinstalled in the epitaxial furnace for baking to remove the moisture in the graphite part, and the operation is very cumbersome. The present application does not need to disassemble and install the graphite part, and eliminates the baking step.

[0047] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0048] The above-described embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the patent application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the scope of patent protection of the present application shall be subject to the attached claims.

Claims

1. A method for cleaning a graphite part for epitaxial growth of silicon carbide, It is characterized in that A graphite part installed in a furnace chamber of an epitaxial furnace is cleaned. The furnace chamber has an air inlet and an exhaust gas outlet. The cleaning method comprises: continuously introducing alkaline vapor into the furnace chamber of the epitaxial furnace through the air inlet.

2. The method for cleaning a graphite piece for epitaxial growth of silicon carbide according to claim 1, It is characterized in that The temperature of the alkali vapor introduced into the furnace chamber of the epitaxial furnace is 900° C. to 1400° C.

3. The method for cleaning a graphite piece for epitaxial growth of silicon carbide according to claim 1, It is characterized in that When the alkali vapor is introduced, the pressure of the furnace chamber of the epitaxial furnace is 100 mbar to 800 mbar.

4. The method for cleaning a graphite piece for epitaxial growth of silicon carbide according to claim 1, It is characterized in that The flow rate of the alkali vapor is 100 sccm~1000 sccm, and the time for passing the alkali vapor is controlled at 60min~90min.

5. The method for cleaning a graphite piece for epitaxial growth of silicon carbide according to claim 1, It is characterized in that The air inlet is connected to a high temperature furnace, and the high temperature furnace is in communication with the air inlet. Before introducing alkali vapor into the furnace chamber of the epitaxial furnace, solid alkali is first placed in the crucible of the high-temperature furnace, and then the high-temperature furnace is heated to 360°C~600°C to convert the solid alkali into molten alkali, and maintained for 10min~30min, and then heated to 900°C~1400°C to obtain alkali vapor.

6. The method for cleaning a graphite piece for epitaxial growth of silicon carbide according to claim 5, It is characterized in that The solid alkali is potassium hydroxide or sodium hydroxide.

7. The method for cleaning a graphite piece for epitaxial growth of silicon carbide according to claim 1, It is characterized in that After the introduction of the alkali vapor is stopped, an inert gas is introduced into the furnace chamber through the gas inlet to purge the furnace chamber, so that the epitaxial reaction byproducts on the graphite piece are purged cleanly.

8. The method for cleaning a graphite piece for epitaxial growth of silicon carbide according to claim 7, It is characterized in that The inert gas is argon.

9. A silicon carbide epitaxial growth device, It is characterized in that include: An epitaxial furnace and a high-temperature furnace, wherein the epitaxial furnace has a furnace chamber, the furnace chamber has an air inlet and an exhaust gas outlet, a graphite part for epitaxial growth of silicon carbide is installed in the furnace chamber, the high-temperature furnace is connected to the air inlet, and the high-temperature furnace is communicated with the air inlet, and the silicon carbide epitaxial growth device is used to implement the cleaning method as described in any one of claims 1 to 8.

10. The silicon carbide epitaxial growth device according to claim 9, It is characterized in that The air inlet and the tail gas outlet are respectively located at two ends of the furnace cavity.

Citation Information

Patent Citations

  • Adjustment method of SiC (silicon carbide) single crystal flatness by wet etching

    CN102569055A

  • Silicon removal method and device for reaction-sintered silicon carbide ceramic

    CN105819905A

  • Treating method for fittings of silicon carbide epitaxial furnace

    CN106087039A

  • Vapor deposition apparatus and techniques using high purity polymer derived silicon carbide

    CN108463580A

  • Device for corroding silicon carbide wafer by alkali steam

    CN113550012A