Degradable non-woven fabric

Through the composite material of polylactic acid, flax fiber and graphene oxide modified viscose fiber, a degradable non-woven fabric that can rapidly degrade under different environmental conditions and has excellent mechanical properties has been prepared, which solves the existing non-woven fabric The problem of different degradation rates in different environmental conditions improves its degradation rate and service life.

CN119061584APending Publication Date: 2024-12-03SHANGHAI EARNTZ NONWOVON CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411387361.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-01
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The degradation rate of existing degradable non-woven fabrics varies according to different environmental conditions, making it difficult to achieve complete degradation in all application scenarios, and the difficulty of degradation of traditional plastic-based non-woven fabrics has a negative impact on the environment.

Method used

The composite material of polylactic acid, flax fiber and graphene oxide modified viscose fiber is used to prepare degradable non-woven fabrics through mechanical carding, cross-meshing and hydrotunneling entanglement processes to improve its degradation rate and mechanical properties.

Benefits of technology

It significantly improves the degradation rate and service life of non-woven fabrics, ensures rapid degradation under different environmental conditions, and provides excellent mechanical properties.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a degradable non-woven fabric, and relates to the technical field of non-woven materials, the degradable non-woven fabric comprises the following raw materials by mass percentage: 50-70% of polylactic acid / flax fiber, and 30-50% of graphene oxide modified viscose fiber; the preparation method comprises the following steps: mixing and opening the polylactic acid / flax fiber and the graphene oxide modified viscose fiber, and then carrying out mechanical carding, cross lapping, spunlace entanglement and drying to prepare the degradable non-woven fabric. The graphene oxide modified viscose fiber is prepared from the following raw materials in parts by weight: 2.5 to 7.5 parts of polyethyleneimine, 0.1 to 0.3 part of graphene oxide, 0.5 to 1.5 parts of anionic viscose fiber and 25 to 75 parts of deionized water. The anionic viscose fiber is prepared from the following raw materials in parts by weight: 3-5 parts of viscose fiber, 19-32 parts of sodium chloroacetate and 10-16 parts of an alkali solvent. The non-woven fabric provided by the invention not only has relatively high mechanical strength, but also has relatively high degradation rate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of nonwoven material technology, and in particular to a degradable nonwoven fabric. Background Art

[0002] Non-woven fabrics, also known as non-woven fabrics, needle-punched cotton, needle-punched non-woven fabrics, etc., are mostly made of plastic particles as raw materials, and are produced by a continuous one-step process of high-temperature melting, spinning, laying, hot pressing and winding. They are widely used in materials in many fields such as daily life, medical and health care, industrial packaging and agricultural coverage. The reason why non-woven fabrics are so popular is not only because of their basic physical properties such as moisture-proof, breathable, flexible and light, but also because they are non-combustible, easy to process and shape, rich in colors and can be customized according to needs.

[0003] However, with the enhancement of global environmental awareness and the popularization of the concept of sustainable development, the difficulty of traditional plastic-based non-woven fabrics to degrade in the natural environment has become an urgent problem to be solved. The massive accumulation of plastic waste not only pollutes the soil and water sources, but also has a long-term and far-reaching negative impact on the ecosystem. Therefore, the research and development and application of degradable non-woven fabrics have become an inevitable trend in the development of the industry. Degradable non-woven fabrics refer to non-woven fabric materials that can gradually decompose in the natural environment or under specific conditions (such as microbial action, photolysis, hydrolysis, etc.), and eventually return to the natural cycle. At present, there are a variety of degradable non-woven fabric products on the market, such as non-woven fabrics produced with bio-based materials such as polylactic acid and polyhydroxyalkanoates, as well as products that give traditional plastic-based non-woven fabrics a certain degree of degradation ability by adding special degradation aids.

[0004] However, the degradation performance of existing degradable nonwoven fabrics is greatly affected by environmental conditions, such as temperature, humidity, microbial species, etc., resulting in different degradation rates and difficulty in achieving complete degradation in all application scenarios. Therefore, providing a highly degradable nonwoven fabric has become an urgent problem to be solved. Summary of the invention

[0005] In order to provide a highly degradable non-woven fabric material and improve the performance of degradable non-woven fabrics, the present application provides a degradable non-woven fabric.

[0006] The biodegradable non-woven fabric provided in this application adopts the following technical solution: A degradable non-woven fabric, the raw materials of which include 50-70% polylactic acid / flax fiber and 30-50% graphene oxide modified viscose fiber by mass percentage; The method for preparing the degradable non-woven fabric comprises the following steps: The polylactic acid / flax fiber and graphene oxide modified viscose fiber are mixed and opened, and then mechanically combed, cross-laid, hydroentangled and dried to prepare a degradable non-woven fabric.

[0007] By adopting the above technical scheme, polylactic acid, flax fiber and viscose fiber are all degradable and environmentally friendly materials, and the composite non-woven fabric has excellent degradability; the polylactic acid / flax fiber prepared by composite polylactic acid and viscose fiber has a synergistic effect in the degradation process, which makes the overall degradation rate of the non-woven fabric faster, and effectively improves the degradation rate of the non-woven fabric; after the viscose is modified by graphene oxide, the tensile strength and wear resistance of the viscose fiber can be significantly improved, which makes the obtained degradable non-woven fabric more stable and reliable when subjected to external forces, thereby extending the service life of the degradable non-woven fabric.

[0008] Preferably, the degradable non-woven fabric raw material comprises 60% polylactic acid / flax fiber and 40% graphene oxide modified viscose fiber by mass percentage.

[0009] Preferably, the graphene oxide modified viscose fiber is prepared from the following raw materials in parts by weight: 2.5-7.5 parts of polyethyleneimine, 0.1-0.3 parts of graphene oxide, 0.5-1.5 parts of anionic viscose fiber, and 25-75 parts of deionized water.

[0010] Preferably, the method for preparing the graphene oxide modified viscose fiber comprises the following steps: Put anionic viscose fiber into a reactor, add polyethyleneimine and graphene oxide, and finally add deionized water, stir evenly, seal the reactor for vacuum drying reaction, cool after the reaction, wash and dry to obtain graphene oxide modified viscose fiber.

[0011] Preferably, the anionic viscose fiber is made from the following raw materials in parts by weight: 3-5 parts of viscose fiber, 19-32 parts of sodium chloroacetate, and 10-16 parts of an alkali solvent.

[0012] Preferably, the alkaline solvent is a 1 mol / L sodium hydroxide aqueous solution.

[0013] Preferably, the method for preparing the anionic viscose fiber comprises the following steps: After drying the viscose fiber, add an alkaline solvent, mix and stir evenly to obtain solution A; add an alkaline solvent into sodium chloroacetate and stir until it is completely dissolved, and then stand at room temperature to obtain solution B; Add solution B to solution A, stir to mix the two solutions evenly, seal, and stir and heat in a water bath at 70-80°C for 4-6 hours; after the reaction, adjust the product to neutral, and finally wash and dry to obtain anionic viscose fiber.

[0014] By adopting the above technical scheme, viscose fiber is used as raw material, sodium hydroxide is used as catalyst, and sodium chloroacetate is used as modifier to perform carboxymethyl modification on viscose fiber to prepare modified anionic viscose fiber; then anionic viscose fiber is used as raw material, polyethyleneimine is used as cross-linking agent, and graphene oxide is used as modifier to prepare graphene oxide modified viscose fiber under high temperature conditions in a high-pressure reactor, which effectively improves the mechanical strength, heat resistance and durability of viscose fiber, and effectively improves the performance of degradable non-woven fabrics.

[0015] Preferably, the raw materials of the polylactic acid / flax fiber include polylactic acid and flax fiber in a mass ratio of 2.5-3.5:1.

[0016] Preferably, the method for preparing the polylactic acid / flax fiber comprises the following steps: After the polylactic acid is dried, it is mixed with flax fibers to obtain a mixture; the mixture is melted by extrusion; and then it is sprayed into fibers through spinnerets, and the polylactic acid / flax fibers are obtained after cooling.

[0017] In summary, the present application includes at least one of the following beneficial technical effects: 1. The polylactic acid / flax fiber prepared by compounding polylactic acid and viscose fiber in the present application has a synergistic effect during the degradation process, which makes the overall degradation rate of the non-woven fabric faster, and effectively improves the degradation rate of the non-woven fabric; 2. After modifying viscose with graphene oxide, the present application can significantly improve the tensile strength and wear resistance of viscose fiber, which makes the obtained degradable non-woven fabric more stable and reliable when subjected to external forces, thereby extending the service life of the degradable non-woven fabric. DETAILED DESCRIPTION

[0018] The present application is further described in detail below with reference to the embodiments.

[0019] The chemical reagents used in the embodiments and comparative examples provided by the present invention are all commercially available products, and their brands and manufacturers are as follows: Viscose fiber, Shandong Yamei Technology Co., Ltd., China; Polyethyleneimine, Shanghai Aladdin Biochemical Technology Co., Ltd., E107079; Graphene oxide, Beijing Bailingwei Technology Co., Ltd., G0443; Polylactic acid, Beijing Thompson Biotechnology Co., Ltd.; Flax fiber, Harbin Sunshine Flax Textile Company.

[0020] Preparation Example Preparation Example 1 Preparation of graphene oxide modified viscose fiber Preparation Example 1.1 S1. After drying 3g of viscose fiber, add 6g of 1mol / L sodium hydroxide aqueous solution, mix and stir for 30min to obtain solution A; add 4g of 1mol / L sodium hydroxide aqueous solution to 19g of sodium chloroacetate and stir until completely dissolved, and stand at room temperature for 30min to obtain solution B; add solution B to solution A, stir to mix the two solutions evenly, seal, and stir and heat in a 70°C water bath for 4h; after the reaction, adjust the product to neutrality with 0.1mol / 1 glacial acetic acid aqueous solution, and finally wash it twice with anhydrous ethanol and vacuum dry it at 65°C to obtain anionic viscose fiber; S2. Put 0.5g of anionic viscose fiber prepared by S1 into a high-pressure reactor, add 2.5g of polyethyleneimine and 0.1g of graphene oxide, and finally add 25g of deionized water, stir evenly, seal the reactor and carry out vacuum drying reaction at 140°C for 16h, cool after the reaction, wash twice with distilled water, and vacuum dry at 65°C to obtain graphene oxide modified viscose fiber.

[0021] Preparation Example 1.2 S1. After drying 4g of viscose fiber, 8g of 1mol / L sodium hydroxide aqueous solution was added, and the mixture was stirred for 35min to obtain solution A; 5g of 1mol / L sodium hydroxide aqueous solution was added to 25g of sodium chloroacetate and stirred until completely dissolved, and the mixture was allowed to stand at room temperature for 35min to obtain solution B; solution B was added to solution A, and the two solutions were stirred to mix evenly, sealed, and stirred and heated in a water bath at 75°C for 5h; after the reaction was completed, the product was adjusted to neutral using 0.1mol / 1 glacial acetic acid aqueous solution, and finally washed 3 times with anhydrous ethanol and dried in vacuo at 70°C to obtain anionic viscose fiber; S2. Put 1g of anionic viscose fiber prepared by S1 into a high-pressure reactor, add 5g of polyethyleneimine and 0.2g of graphene oxide, and finally add 50g of deionized water, stir evenly, seal the reactor and carry out vacuum drying reaction at 150°C for 15h. After the reaction is completed, cool it, wash it with distilled water 3 times, and vacuum dry it at 70°C to obtain graphene oxide modified viscose fiber.

[0022] Preparation Example 1.3 S1. After drying 5g of viscose fiber, 10g of 1mol / L sodium hydroxide aqueous solution was added, and the mixture was stirred for 40min to obtain solution A; 6g of 1mol / L sodium hydroxide aqueous solution was added to 32g of sodium chloroacetate and stirred until completely dissolved, and the mixture was allowed to stand at room temperature for 40min to obtain solution B; solution B was added to solution A, and the two solutions were stirred to mix evenly, sealed, and stirred and heated in a water bath at 80°C for 6h; after the reaction was completed, the product was adjusted to neutrality using 0.1mol / 1 glacial acetic acid aqueous solution, and finally washed 4 times with anhydrous ethanol and dried in vacuo at 75°C to obtain anionic viscose fiber; S2. Put 1.5g of anionic viscose fiber prepared by S1 into a high-pressure reactor, add 7.5g of polyethyleneimine and 0.3g of graphene oxide, and finally add 75g of deionized water, stir evenly, seal the reactor and carry out vacuum drying reaction at 160°C for 14h, cool after the reaction, wash with distilled water 4 times, and vacuum dry at 75°C to obtain graphene oxide modified viscose fiber.

[0023] Preparation Example 2 Polylactic acid / flax fiber Preparation Example 2.1 125g of polylactic acid and 50g of flax fiber are weighed according to the mass ratio; the polylactic acid is dried in a vacuum drying oven at 60°C, and then mixed with the flax fiber through a high-speed mixer to obtain a mixture; the mixture is melted by screw extrusion, the working temperature is controlled at 90°C, and the rotation speed is controlled at 55r / min; the mixture is then sprayed into fibers through a spinneret, the spinneret hole diameter is controlled at 0.15mm, the working speed is controlled at 6000m / min, and the polylactic acid / flax fiber is obtained after cooling.

[0024] Preparation Example 2.2 150g of polylactic acid and 50g of flax fiber are weighed according to the mass ratio; the polylactic acid is dried in a vacuum drying oven at 65°C, and then mixed with the flax fiber through a high-speed mixer to obtain a mixture; the mixture is melted by screw extrusion, the working temperature is controlled at 85°C, and the rotation speed is controlled at 60r / min; the mixture is then sprayed into fibers through a spinneret, the spinneret hole diameter is controlled at 0.15mm, the working speed is controlled at 6500m / min, and the polylactic acid / flax fiber is obtained after cooling.

[0025] Preparation Example 2.3 175g of polylactic acid and 50g of flax fiber are weighed according to the mass ratio; the polylactic acid is dried in a vacuum drying oven at 70°C, and then mixed with the flax fiber through a high-speed mixer to obtain a mixture; the mixture is melted by screw extrusion, the working temperature is controlled at 80°C, and the rotation speed is controlled at 65r / min; the mixture is then sprayed into fibers through a spinneret, the spinneret hole diameter is controlled at 0.15mm, the working speed is controlled at 7000m / min, and the polylactic acid / flax fiber is obtained after cooling. Example

[0026] Example 1 S1. Weigh 50 g of the polylactic acid / flax fiber prepared in Preparation Example 2.1 according to the mass ratio, the fiber fineness is 0.9D, and the length is 21 mm; weigh 50 g of the graphene oxide-modified viscose fiber prepared in Preparation Example 1.1, the fiber fineness is 1.0D, and the length is 38 mm; S2. PLA / flax fiber and graphene oxide modified viscose fiber were mixed and opened, and then mechanically combed by a roller carding machine, cross-laid by a warp lapping machine, and the lapping speed was 150m / min; and then hydroentangled by a hydroentanglement machine, and the hydroentanglement pressure was 5.0×10 6 Pa, after ultrasonic washing with water, was dried at 100°C to prepare a degradable non-woven fabric.

[0027] Example 2 S1. Weigh 60 g of polylactic acid / flax fiber prepared in Preparation Example 2.1 according to the mass ratio, the fiber fineness is 0.9D, and the length is 21 mm; weigh 40 g of graphene oxide modified viscose fiber prepared in Preparation Example 1.1, the fiber fineness is 1.0D, and the length is 38 mm; S2. PLA / flax fiber and graphene oxide modified viscose fiber were mixed and opened, and then mechanically combed by a roller carding machine, cross-laid by a warp lapping machine, and the lapping speed was 150m / min; and then hydroentangled by a hydroentanglement machine, and the hydroentanglement pressure was 5.0×10 6 Pa, after ultrasonic washing with water, was dried at 100°C to prepare a degradable non-woven fabric.

[0028] Example 3 S1. Weigh 70 g of the polylactic acid / flax fiber prepared in Preparation Example 2.1 according to the mass ratio, the fiber fineness is 0.9D, and the length is 21 mm; weigh 30 g of the graphene oxide-modified viscose fiber prepared in Preparation Example 1.1, the fiber fineness is 1.0D, and the length is 38 mm; S2. PLA / flax fiber and graphene oxide modified viscose fiber were mixed and opened, and then mechanically combed by a roller carding machine, cross-laid by a warp lapping machine, and the lapping speed was 150m / min; and then hydroentangled by a hydroentanglement machine, and the hydroentanglement pressure was 5.0×10 6 Pa, after ultrasonic washing with water, was dried at 100°C to prepare a degradable non-woven fabric.

[0029] Example 4 S1. Weigh 50 g of the polylactic acid / flax fiber prepared in Preparation Example 2.1 according to the mass ratio, the fiber fineness is 0.9D, and the length is 21 mm; weigh 50 g of the graphene oxide-modified viscose fiber prepared in Preparation Example 1.1, the fiber fineness is 1.0D, and the length is 38 mm; S2. PLA / flax fiber and graphene oxide modified viscose fiber were mixed and opened, and then mechanically combed by a roller carding machine, cross-laid by a warp lapping machine, and the laying speed was 155 m / min; and then hydroentangled by a hydroentanglement machine, and the hydroentanglement pressure was 6.0×10 6 Pa, after ultrasonic washing with water, was dried at 120°C to prepare a degradable nonwoven fabric.

[0030] Example 5 S1. Weigh 50 g of the polylactic acid / flax fiber prepared in Preparation Example 2.1 according to the mass ratio, the fiber fineness is 0.9D, and the length is 21 mm; weigh 50 g of the graphene oxide-modified viscose fiber prepared in Preparation Example 1.1, the fiber fineness is 1.0D, and the length is 38 mm; S2. PLA / flax fiber and graphene oxide modified viscose fiber were mixed and opened, then mechanically combed by roller carding machine, cross-laid by warp lapping machine, and the laying speed was 160m / min; and then hydroentangled by hydroentanglement machine, and the hydroentanglement pressure was 7.0×10 6 Pa, after ultrasonic washing with water, was dried at 140°C to prepare a degradable nonwoven fabric.

[0031] Example 6 The difference between Example 6 and Example 1 is that the polylactic acid / flax fiber used in Example 6 comes from Preparation Example 2.2.

[0032] Example 7 The difference between Example 7 and Example 1 is that the polylactic acid / flax fiber used in Example 7 comes from Preparation Example 2.3.

[0033] Example 8 The difference between Example 8 and Example 1 is that the graphene oxide-modified viscose fiber used in Example 8 comes from Preparation Example 1.2.

[0034] Example 9 The difference between Example 9 and Example 1 is that the graphene oxide-modified viscose fiber used in Example 9 comes from Preparation Example 1.3.

[0035] Comparative Example Comparative Example 1 S1. Weigh 40 g of the polylactic acid / flax fiber prepared in Preparation Example 2.1 according to the mass ratio, the fiber fineness is 0.9D, and the length is 21 mm; weigh 60 g of the graphene oxide-modified viscose fiber prepared in Preparation Example 1.1, the fiber fineness is 1.0D, and the length is 38 mm; S2. PLA / flax fiber and graphene oxide modified viscose fiber were mixed and opened, and then mechanically combed by a roller carding machine, cross-laid by a warp lapping machine, and the lapping speed was 150m / min; and then hydroentangled by a hydroentanglement machine, and the hydroentanglement pressure was 5.0×10 6 Pa, after ultrasonic washing with water, was dried at 100°C to prepare a degradable non-woven fabric.

[0036] Comparative Example 2 S1. Weigh 80 g of the polylactic acid / flax fiber prepared in Preparation Example 2.1 according to the mass ratio, the fiber fineness is 0.9D, and the length is 21 mm; weigh 20 g of the graphene oxide-modified viscose fiber prepared in Preparation Example 1.1, the fiber fineness is 1.0D, and the length is 38 mm; S2. PLA / flax fiber and graphene oxide modified viscose fiber were mixed and opened, and then mechanically combed by a roller carding machine, cross-laid by a warp lapping machine, and the lapping speed was 150m / min; and then hydroentangled by a hydroentanglement machine, and the hydroentanglement pressure was 5.0×10 6 Pa, after ultrasonic washing with water, was dried at 100°C to prepare a degradable non-woven fabric.

[0037] Comparative Example 3 The difference between Comparative Example 3 and Example 1 is that the common flax fiber which has not been treated with polylactic acid is used in Comparative Example 3.

[0038] Comparative Example 4 The difference between Comparative Example 4 and Example 1 is that the common viscose fiber which is not modified with graphene oxide is used in Comparative Example 4.

[0039] Performance testing 1. The tensile strength of the degradable nonwoven fabrics obtained in Examples 1-9 and Comparative Examples 1-4 was tested using an Instron 3365 universal material testing machine. The results are shown in Table 1.

[0040] 2. The degradation rates of the degradable nonwoven fabrics obtained in Examples 1-9 and Comparative Examples 1-4 were tested with reference to the standard GB / T19277.1-2011 "Determination of the ultimate aerobic biodegradability of materials under controlled composting conditions by measuring the released carbon dioxide Part 1: General method", and the results are shown in Table 1.

[0041] The specific test results are as follows: Tensile strength / MPa 145 days degradation rate / % Example 1 456 15.3 Example 2 469 15.9 Example 3 451 15.2 Example 4 456 15.3 Example 5 454 15.1 Example 6 460 15.6 Example 7 458 15.4 Example 8 457 15.5 Example 9 455 15.3 Comparative Example 1 410 11.9 Comparative Example 2 428 12.7 Comparative Example 3 420 10.9 Comparative Example 4 404 11.5 It can be seen from the test results in Table 1 that the degradable non-woven fabric provided by the present application has a tensile strength of more than 450 MPa, indicating that it has strong mechanical properties; the degradation rate after 145 days can reach 15.3% or more, indicating that the degradation rate of the degradable non-woven fabric provided by the present application is relatively high.

[0042] It can be seen from the test results of Examples 1-5 and Comparative Examples 1-2 that the formula and preparation method of the degradable non-woven fabric provided in the present application can obtain a non-woven fabric with higher mechanical properties and higher degradation rate, and the preferred percentage of the raw material polylactic acid / flax fiber is 50-70%, and the percentage of graphene oxide modified viscose fiber is 30-50%.

[0043] It can be seen from the test results of Examples 1, 6, 7 and Comparative Example 4 that the formula and preparation method of graphene oxide modified viscose fiber provided in the present application are conducive to obtaining a non-woven fabric with higher mechanical properties and higher degradation rate.

[0044] It can be seen from the test results of Examples 1, 8, 9 and Comparative Example 3 that the formula and preparation method of polylactic acid / flax fiber provided in the present application are conducive to obtaining a non-woven fabric with higher mechanical properties and higher degradation rate.

[0045] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A degradable non-woven fabric, characterized in that: The raw materials include 50-70% polylactic acid / flax fiber and 30-50% graphene oxide modified viscose fiber by mass percentage; The method for preparing the degradable non-woven fabric comprises the following steps: The polylactic acid / flax fiber and graphene oxide modified viscose fiber are mixed and opened, and then mechanically combed, cross-laid, hydroentangled and dried to prepare a degradable non-woven fabric.

2. The degradable nonwoven fabric according to claim 1, characterized in that: The degradable non-woven fabric raw material comprises 60% polylactic acid / flax fiber and 40% graphene oxide modified viscose fiber by mass percentage.

3. A degradable nonwoven fabric according to claim 1 or 2, characterized in that: The graphene oxide modified viscose fiber is prepared from the following raw materials in parts by weight: 2.5-7.5 parts of polyethyleneimine, 0.1-0.3 parts of graphene oxide, 0.5-1.5 parts of anionic viscose fiber, and 25-75 parts of deionized water.

4. The degradable nonwoven fabric according to claim 3, characterized in that: The method for preparing the graphene oxide modified viscose fiber comprises the following steps: Put anionic viscose fiber into a reactor, add polyethyleneimine and graphene oxide, and finally add deionized water, stir evenly, seal the reactor for vacuum drying reaction, cool after the reaction, wash and dry to obtain graphene oxide modified viscose fiber.

5. A degradable nonwoven fabric according to claim 3 or 4, characterized in that: The anionic viscose fiber is prepared from the following raw materials in parts by weight: 3-5 parts of viscose fiber, 19-32 parts of sodium chloroacetate, and 10-16 parts of an alkali solvent.

6. The degradable nonwoven fabric according to claim 5, characterized in that: The alkaline solvent is a 1 mol / L sodium hydroxide aqueous solution.

7. The degradable nonwoven fabric according to claim 5, characterized in that: The preparation method of the anionic viscose fiber comprises the following steps: After drying the viscose fiber, add an alkaline solvent, mix and stir evenly to obtain solution A; add an alkaline solvent into sodium chloroacetate and stir until it is completely dissolved, and then stand at room temperature to obtain solution B; Add solution B to solution A, stir to mix the two solutions evenly, seal, and stir and heat in a water bath at 70-80°C for 4-6 hours; after the reaction, adjust the product to neutral, and finally wash and dry to obtain anionic viscose fiber.

8. The degradable nonwoven fabric according to claim 1, characterized in that: The raw materials of the polylactic acid / flax fiber include polylactic acid and flax fiber, and the mass ratio is 2.5-3.5:

1.

9. The degradable nonwoven fabric according to claim 8, characterized in that: The preparation method of the polylactic acid / flax fiber comprises the following steps: After the polylactic acid is dried, it is mixed with flax fibers to obtain a mixture; the mixture is melted by extrusion; and then it is sprayed into fibers through spinnerets, and after cooling, polylactic acid / flax fibers are obtained.

Citation Information

Patent Citations

  • Sheath-core fibrilia and manufacturing method thereof

    CN101671866A

  • Preparation method of multifunctional viscose fiber composite material

    CN109281161A

  • Biodegradable mulch dust suppression net and preparation method thereof

    CN109610034A

  • Preparation method of composite textile fiber material

    CN111826723A

  • Plant fibrous leather base cloth and manufacturing method thereof

    CN114086313A