Preparation method of water-soluble carbon fiber sizing agent

Through the preparation method of water-soluble carbon fiber sizing agent, the problems of poor wetting and high cost of large tow carbon fiber sizing agents are solved by using technologies such as oxidized nanocellulose fibers and polydopamine modification MXene, and the mechanical properties of carbon fibers and composite materials are improved. Interface performance enables low-cost and high-performance carbon fiber preparation.

CN119061697APending Publication Date: 2024-12-03HARBIN INST OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411234988.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The application of large tow carbon fiber in the field of wind power blades is troubled by the problems of poor wetting properties of sizing agents, uneven sizing and high cost, which leads to the dispersion of the mechanical properties of the composite material and the low interface bonding strength, which affects the overall performance of the material.

Method used

Using a preparation method of water-soluble carbon fiber sizing agent, dynamic boron ester bonds and ions are formed by combining oxidized nanocellulose fibers, polydopamine modified MXene, composite CNTs (GO)/MXene@PDA materials and benzeneboric acid-ionic liquid. The liquid enhances the bonding strength between carbon fiber and resin, and constructs a tight interface layer by modifying graphene oxide MXene@PDA.

Benefits of technology

It improves the strength, toughness and wear resistance of carbon fibers, enhances the interface performance of composite materials, reduces manufacturing costs, simplifies the process, is suitable for industrial production, and improves electromagnetic shielding performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119061697A_ABST
    Figure CN119061697A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a water-soluble carbon fiber sizing agent, and relates to a preparation method of a sizing agent. The preparation method comprises the following steps: fully mixing PBA-IL and TOCNF (TBC) / CNTs (GO) / MXene (at) PDA at room temperature, then mixing EP and the mixture according to different mass fractions, uniformly stirring, and then carrying out vacuum extraction. And after no bubble exists in the mixture under the vacuum condition, adding waterborne emulsion polyurethane as a curing agent, and fully mixing by using a homogenizer to obtain the water-soluble carbon fiber sizing agent. The problems of high cost of imported sizing agents in the carbon fiber manufacturing process, broken filaments and damage generated in fiber manufacturing and the like are solved, the carbon fiber manufacturing cost is reduced, and the carbon fiber performance is improved. Due to the existence of the multi-dimensional conductive network on the surface of the carbon fiber, the composite carbon fiber material is endowed with excellent electromagnetic shielding performance, and the strength, toughness, wear resistance and the like of the carbon fiber are also improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of sizing agent preparation, and particularly relates to a method for preparing a water-soluble carbon fiber sizing agent. Background Art

[0002] In recent years, with the development of large-scale and lightweight wind turbines, the ultra-long blades have put forward higher requirements on the strength and stiffness of materials, which provides a premise for the widespread application of carbon fiber and its composite materials in the field of wind turbine blades. Although small-tow carbon fiber has excellent mechanical properties, it has long been constrained by cost factors, and the rapid development of large-tow carbon fiber is precisely due to the rapid growth of composite blades in the global wind power business. Due to the large tow of large-tow carbon fiber, the wettability of the sizing agent on the fiber becomes poor, which is prone to problems such as insufficient wettability and uneven sizing, which in turn causes lint or even broken yarns in the yarn spreading stage during the preparation of the composite material, affecting the preparation process of the composite material, resulting in a large dispersion of the mechanical properties of the composite material, and further increasing the difficulty of applying large-tow carbon fiber.

[0003] At the same time, large-tow carbon fiber has higher requirements for the interface due to its large tow. Sizing can protect the carbon fiber without damaging it, improve the wettability between the carbon fiber and the resin, and the components in the sizing agent participate in the curing reaction of the resin through the action of chemical bonds, improve the interface performance of the composite material, and improve the comprehensive performance of the composite material. Therefore, the research on sizing agents is crucial to the molding and processing technology of carbon fiber and the performance of composite materials.

[0004] CN101858037A discloses an emulsion-type carbon fiber sizing agent, and discloses that the sizing agent includes vinyl ester resin, modified epoxy resin, emulsifier, diluent, penetrant and water. By adjusting the main slurry ratio, emulsifier and emulsification process, an emulsion-type sizing agent suitable for an unsaturated polyester resin matrix is ​​prepared. However, due to the poor compatibility between the main slurry and the matrix resin, a certain influence is produced on the interface performance of the composite material, resulting in a reduction in the interface bonding strength. Summary of the invention

[0005] The purpose of the present invention is to solve the problems of high cost of imported sizing agents, hair and damage caused by fiber manufacturing in the process of carbon fiber manufacturing, and provide a preparation method of a water-soluble carbon fiber sizing agent, which can form a strong bonding strength with carbon fiber and resin matrix, and the raw materials are easily available and the steps are simple and environmentally friendly. And this method reduces the cost of carbon fiber manufacturing and improves the performance of carbon fiber. Due to the presence of a multidimensional conductive network on the surface of carbon fiber, the composite carbon fiber material is endowed with excellent electromagnetic shielding performance, and the strength, toughness and wear resistance of carbon fiber are also improved.

[0006] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0007] A method for preparing a water-soluble carbon fiber sizing agent, the method comprising:

[0008] Step 1: Preparation of oxidized nanocellulose fibers:

[0009] TEMPO and NaBr are added to a suspension of CNF or BC with a mass fraction of 0.5%-3%, and the mixture is evenly mixed under magnetic stirring. NaClO is used to adjust the pH of the reaction solution to 10-11, and the reaction is carried out for 0.5-3 hours. After the reaction, the pH of the reaction solution is adjusted to 7 with a standard hydrochloric acid solution, and then the reaction solution is repeatedly centrifuged and washed with deionized water for 4-6 times to obtain TOCNF or TBC. CNF: nanocellulose fibers derived from wood or cotton; BC: bacterial cellulose.

[0010] Step 2: Modification of MXene with polydopamine (PDA):

[0011] Take 5-50 mg of 8-10 mg / ml MXene aqueous dispersion and wash it three times by centrifugation with Tris buffer, then disperse it in 40 mL Tris buffer to obtain a MXene solution, add 80 mg of polydopamine to the MXene solution, react at room temperature for 1-3 h, and obtain a PDA-modified MXene nanosheet solution;

[0012] Step 3: Preparation of composite CNTs(GO) / MXene@PDA materials

[0013] PDA-modified MXene nanosheet solution was added to the CNTs (GO) dispersion and the volume was adjusted to 500 ml, followed by ultrasonication for 10 min and continuous stirring for 6 h-12 h.

[0014] Step 4: Synthesis of phenylboronic acid-ionic liquid (PBA-IL)

[0015] Using 4-(bromomethyl)phenylboronic acid (PBA) and 1-(3-aminopropyl)imidazole (MZ) as raw materials, PBA (0.4297 g, 2 mmol) was dissolved in anhydrous ethanol (15 mL) in a three-necked round-bottom flask, and then MZ (0.281 mL, 2.5 mmol) was added to the solution, and the mixture was refluxed at 90°C for 24 h; the crude product was precipitated and purified with a mixture of ethyl acetate and ethanol, and the solvent was evaporated under vacuum to obtain an ionic liquid; it was vacuum dried at 70°C for 12 h to obtain a PBA-IL monomer;

[0016] Step 5: Preparation of water-soluble carbon fiber sizing agent

[0017] PBA-IL, TOCNF (TBC) and CNTs (GO) / MXene @ PDA were fully mixed at room temperature; then, EP was mixed with the mixture and stirred evenly, and then vacuum extraction was performed; after there were no bubbles in the mixture under vacuum conditions, aqueous emulsion polyurethane was added as a curing agent, and the mixture was fully mixed with a homogenizer to obtain a water-soluble carbon fiber sizing agent.

[0018] Furthermore, in step 1, the mass ratio of CNF(BC), TEMPO and NaBr is controlled to be 150-350:4-10:25.

[0019] Furthermore, in step 2, the concentration of the Tris buffer is 10 mmol / L and the pH is 8.5.

[0020] Furthermore, in step three, the volume ratio of the CNTs (GO) dispersion to the PDA-modified MXene nanosheet solution is 0.5-10:1; and the mass volume fraction of the CNTs (GO) dispersion is 0.05%-1%.

[0021] Furthermore, in step 4, the molar ratio of PBA to MZ is 2:2.5.

[0022] Furthermore, in step five, the mass ratio of the EP, PBA-IL, TOCNF (TBC), CNTs (GO) / MXene @ PDA and polyurethane is 100: 0.5: 0.5-3: 0.05-1: 10-20.

[0023] The beneficial effects of the present invention compared to the prior art are:

[0024] 1. The molecular structure of polydopamine used in the present invention is similar to that of mussel adhesion protein, and can undergo a phenolic hydroxyl chemical reaction similar to that on the dopa molecule in the adhesion protein. Therefore, polydopamine has mussel induction properties. MXene is modified by oxidation and polymerization on the surface of MXene. The modified MXene can improve the adhesion between the MXene and the carbon fiber, and prevent the MXene from falling off from the surface or gap of the carbon fiber.

[0025] 2. The phenylboronic acid groups in the ionic liquid react with the cis-diol in TOCNF (TBC) to form dynamic boron ester bonds. TOCNF (TBC) is used as a stress-enhanced phase to construct an interpenetrating network. The carboxylic acid anions on the surface of TOCNF (TBC) can interact with the cations of the ionic liquid, thereby promoting the dispersion of TOCNF (TBC) in the epoxy resin matrix. The multi-component synergistically improves the heat resistance of epoxy sizing agent carbon fiber and enhances the toughness of epoxy carbon fiber composites.

[0026] 3. The method of the present invention is simple to prepare, has a short preparation process, mild conditions, low raw material cost, is easy to convert into products, is conducive to industrial-scale production, and no toxic or harmful substances are emitted during the preparation process, which is a green and pollution-free processing process.

[0027] 4. Graphene oxide (carbon nanotubes) modifies MXene@PDA in an intercalation manner. On the one hand, it can effectively slow down the self-stacking of MXene. On the other hand, the hybrid material bonded by Ti-OC covalent bonds can induce the compact deposition of two-dimensional materials on the surface of carbon fibers. It does not only rely on the active functional groups at the edges of graphene oxide or carbon nanotubes. The functional groups in the MXene plane induce the hybrid nanomaterials to form a "face-to-face" interaction with carbon fibers by dispersing in the resin, thereby constructing an interlayer interaction, orderly arrangement and dense interface layer on the surface of carbon fibers. The introduction of graphene oxide / carbon nanotubes and MXene increases the surface energy of carbon fibers and enhances the interfacial bonding between carbon fibers and resin matrix. Moreover, since the design of the "brick and mortar" structure can effectively transmit stress, the orderly arranged two-dimensional nanomaterials are more conducive to stable slippage, thereby dissipating a large amount of energy, and enhancing the strength of the composite material while improving the toughness of the composite material. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 is the SEM image of BC;

[0029] Figure 2 is the SEM image of TBC;

[0030] Figure 3 TEM image of PDA@MXene. DETAILED DESCRIPTION

[0031] The technical scheme of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are only a part of the embodiments of the invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work belong to the protection scope of the present invention. If the specific conditions are not specified in the embodiments, they are carried out according to the conventional conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified in the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0032] Example 1

[0033] Step 1: Add 1wt% BC (such as Figure 1TEMPO and NaBr were added to the suspension to oxidize it under magnetic stirring, and the mass ratio of BC, TEMPO and NaBr was controlled to be 200:4:25, and the pH of the reaction solution was adjusted to 10-11 by NaClO, and the reaction was carried out for 1.5 hours; after the reaction, the pH of the reaction solution was adjusted to 7 with a standard hydrochloric acid solution, and then the reaction was repeatedly centrifuged and washed with deionized water for 4-6 times to obtain TBC (as shown in FIG. Figure 2 shown).

[0034] Step 2: (1) Add 0.5g LiF to 20mL HCl solution with a concentration of 6mol / L, and stir magnetically for 30min to obtain a uniform and stable LiF / HCl solution. Then add 1g MAX powder to the LiF / HCl solution, stir at 35°C for 18h to obtain a suspension, and then repeatedly centrifuge and wash the suspension with deionized water until the pH of the supernatant is 6 to obtain a water-containing MXene precipitate; ultrasonically treat the water-containing MXene precipitate for 0.5-2h, and then centrifuge at 3500rpm for 0.5-1h to obtain a MXene aqueous dispersion; the concentration of the MXene aqueous dispersion is 9mg / mL; the MXene in the obtained MXene aqueous dispersion is a single-layer structure nanosheet (such as Figure 3 As shown), it is dark green, indicating that the yield of MXene obtained is high;

[0035] The MAX powder has a molecular formula of Mn+1AXn(Ti3AlC2), wherein n=1, 2 or 3, M is Ti, V, Cr, Zr, Nb, Mo, Hf or Ta, A is Al, Si, P, S, Ga, Ge, As, Cd, In, Sn, Tl or Pb, and X is C or N.

[0036] (2) 30 mg of MXene aqueous dispersion was taken and washed three times with Tris buffer, and then dispersed in 40 mL of Tris buffer to obtain a MXene solution, 80 mg of polydopamine was added to the MXene solution, and reacted at room temperature for 2 h to obtain a PDA-modified MXene nanosheet solution; the Tris buffer concentration was 10 mmol / L and the pH was 8.5;

[0037] (3) Preparation of composite CNTs(GO) / MXene@PDA materials

[0038] A certain amount of PDA modified MXene nanosheet solution was added to the CNTs (GO) dispersion, and the volume was adjusted to 500 ml, and then ultrasonicated for 10 minutes, and then stirred for 60 hours. The volume ratio of the CNTs (GO) dispersion to the PDA modified MXene nanosheet solution was 8:1; the mass volume fraction of the CNTs (GO) dispersion was 0.8%.

[0039] Step 3: Using 4-(bromomethyl)phenylboronic acid (PBA) and 1-(3-aminopropyl)imidazole (MZ) as raw materials, PBA (0.4297 g, 2 mmol) was dissolved in anhydrous ethanol (15 mL) in a three-necked round-bottom flask, and then MZ (0.281 mL, 2.5 mmol) was added to the solution, and the mixture was refluxed at 90°C for 24 h; the crude product was precipitated and purified with a mixture of ethyl acetate and ethanol, and the solvent was evaporated under vacuum to obtain an ionic liquid; it was vacuum dried at 70°C for 12 h to obtain a PBA-IL monomer.

[0040] Step 4: PBA-IL, TOCNF (TBC) and CNTs (GO) / MXene @ PDA are fully mixed at room temperature; then, EP is mixed with the mixture and stirred evenly, and then vacuum extraction is performed; after there are no bubbles in the mixture under vacuum conditions, aqueous emulsion polyurethane is added as a curing agent, and the mixture is fully mixed with a homogenizer to obtain a water-soluble carbon fiber sizing agent. The mass ratio of EP to PBA-IL, TOCNF (TBC), CNTs (GO) / MXene @ PDA and WPU is 100: 0.5: 2: 0.7: 15.

[0041] Some properties of the sizing agent for carbon fiber prepared by this method are tested as shown in the following table.

[0042]

Claims

1. A method for preparing a water-soluble carbon fiber sizing agent, Features: The method is: Step 1: Preparation of oxidized nanocellulose fibers: Add TEMPO and NaBr to a suspension of CNF or BC with a mass fraction of 0.5%-3%, mix them evenly under magnetic stirring, and use NaClO to adjust the pH of the reaction solution to maintain at 10-11, and react for 0.5-3h; after the reaction, use a standard hydrochloric acid solution to adjust the pH of the reaction solution to 7, and then repeatedly centrifuge and wash with deionized water for 4-6 times to obtain TOCNF or TBC; Step 2: Modification of MXene with polydopamine (PDA): Take 5-50 mg of 8-10 mg / ml MXene aqueous dispersion and wash it three times by centrifugation with Tris buffer, then disperse it in 40 mL Tris buffer to obtain a MXene solution, add 80 mg of polydopamine to the MXene solution, react at room temperature for 1-3 h, and obtain a PDA-modified MXene nanosheet solution; Step 3: Preparation of composite CNTs(GO) / MXene@PDA materials PDA-modified MXene nanosheet solution was added to the CNTs (GO) dispersion and the volume was adjusted to 500 ml, followed by ultrasonication for 10 min and continuous stirring for 6 h-12 h. Step 4: Synthesis of phenylboronic acid-ionic liquid (PBA-IL) Using 4-(bromomethyl)phenylboronic acid (PBA) and 1-(3-aminopropyl)imidazole (MZ) as raw materials, PBA was dissolved in anhydrous ethanol, and then MZ was added to the solution, and the mixture was refluxed at 90°C for 24 hours; the crude product was precipitated and purified with a mixture of ethyl acetate and ethanol, and the solvent was evaporated under vacuum to obtain an ionic liquid; it was vacuum dried at 70°C for 12 hours to obtain a PBA-IL monomer; Step 5: Preparation of a water-soluble carbon fiber sizing agent PBA-IL, TOCNF (TBC) and CNTs (GO) / MXene @ PDA were fully mixed at room temperature; then, EP was mixed with the mixture and stirred evenly, and then vacuum extraction was performed; after there were no bubbles in the mixture under vacuum conditions, aqueous emulsion polyurethane was added as a curing agent, and the mixture was fully mixed with a homogenizer to obtain a water-soluble carbon fiber sizing agent.

2. A method for preparing a water-soluble carbon fiber sizing agent according to claim 1, Features: In step 1, the mass ratio of CNF(BC), TEMPO and NaBr is controlled to be 150-350:4-10:

25.

3. A method for preparing a water-soluble carbon fiber sizing agent according to claim 1, Features: In step 2, the concentration of the Tris buffer is 10 mmol / L and the pH is 8.

5.

4. A method for preparing a water-soluble carbon fiber sizing agent according to claim 1, Features: In step three, the volume ratio of the CNTs (GO) dispersion to the PDA-modified MXene nanosheet solution is 0.5-10:1; the mass volume fraction of the CNTs (GO) dispersion is 0.05%-1%.

5. A method for preparing a water-soluble carbon fiber sizing agent according to claim 1, Features: In step 4, the molar ratio of PBA to MZ is 2:2.

5.