Black core paperboard and preparation method thereof
Through the five-layer base paper structure and coating formula, the existing black core playing card paper has been solved, and the high cost of processing is achieved, which has achieved simple process and low cost and high-pressure resistance and anti-perspective performance, meeting the thickness of high-end playing cards and blackness requirements.
Patent Information
- Application Number
- CN202410967856.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-12-03
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing high-end black core playing card paper has complex processing technology, high losses, high cost, and is difficult to achieve a perspective-proof black layer with an integrated thickness and blackness equivalent to that of the mounted playing card, as well as good beat resistance.
Using five-layer base paper structure, including the surface layer, surface liner layer, core layer, base liner layer and bottom layer. The core layer is dyed with vulcanized black dye, and the surface is coated with ceramic clay and rutile titanium dioxide and other materials, and is polymerized and chlorinated. Additives such as aluminum, polyacrylamide retention agents and cationic starch improve the strength of paper pages and the bonding strength between layers, and combine them with coating formula to improve opacity.
It realizes the preparation of black core jam paper with simple process and low cost, improves the paper sheet's punch resistance and perspective resistance, meets the requirements of high-end playing cards, and ensures the strength of the paper sheet and the bonding strength between layers.
Smart Images

Figure CN119061735A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of papermaking, and in particular to a black core cardboard and a preparation method thereof. Background Art
[0002] Playing cards are a kind of cultural and entertainment tool that is not limited to any age and has few restrictions. With the continuous enrichment of entertainment life, the demand for playing cards has grown rapidly, and there are also higher requirements for the quality of playing cards. The most high-end playing cards on the market are black core playing cards, which have the characteristics of good toughness and anti-see-through. At present, high-end black core playing card paper relies on foreign imports, mainly using the preparation technology of mounting. The scheme structural design in the prior art has a structure of two coated papers, two layers of black coating layers and one layer of glue layer. In addition, a black polymer adhesive configured with polyvinyl alcohol, phosphate starch, and polyether with black dye is coated on the surface of the coated paper, and a black coated paper is made after drying; two coated papers with black coating are compositely mounted with black faces against black faces by a mounting machine to make black core cardboard. The processing technology is complicated, the loss is large, and the cost is high.
[0003] Therefore, there is currently no one-piece playing card process technology that can give the playing cards an anti-see-through black layer with a thickness and blackness comparable to that of mounted playing cards, as well as good striking resistance. Summary of the invention
[0004] A first aspect of an embodiment of the present application provides a method for preparing black core card paper, the method comprising:
[0005] Papermaking base paper; the base paper comprises a surface layer, a surface lining layer, a core layer, a bottom lining layer and a bottom layer which are stacked in sequence; wherein the core layer is dyed with sulfur black dye, and the addition amount of the sulfur black dye is 6-10% of the absolute dry pulp of the core layer;
[0006] A coating is applied on the surface of the base paper.
[0007] In some embodiments, in the step of dyeing the core layer with sulphur black dye, the ratio of polyaluminium chloride to sulphur black is 0.9-1.1:1.0.
[0008] In some embodiments, in the step of dyeing the core layer with sulfur black dye, polyacrylamide retention aid and polyacrylamide dry strength agent or cationic starch are also added, wherein the amount of polyacrylamide retention aid added is 150-250ppm; the amount of polyacrylamide dry strength agent or cationic starch added is 1.5-2.0% of the absolute dry weight of the core layer.
[0009] In some embodiments, the order of adding the raw materials in the step of dyeing the core layer with sulphur black dye is as follows: when the slurry is flowing or stirring, polyaluminium chloride is added to the slurry, then sulphur black dye is added, after mixing and reacting for 1-5 minutes, a dry strength agent or cationic starch is added, and then a retention aid of polyacrylamide is added.
[0010] In some embodiments, the core layer includes 30±5% softwood pulp, 50±10% hardwood pulp, and 20±10% broke pulp.
[0011] In some embodiments, in the step of making base paper, the amount of each layer of the base paper is: surface layer 30±5gsm, surface lining layer 30±5gsm, core layer 80±5gsm, bottom lining layer 30±5gsm, bottom layer 45±5gsm.
[0012] In some embodiments, the slurry and process of the surface layer and the bottom layer include: the paper sheet includes 25±10% coniferous pulp and 75±10% hardwood pulp; 150-250ppm of polyacrylamide retention agent is added, the amount of cationic starch added is 0.5-1.0% of the absolute dry weight of the paper sheet, and the amount of covering agent added is 5-15% of the absolute dry weight of the paper sheet.
[0013] In some embodiments, the slurry and process of the surface lining layer and the bottom lining layer include: the paper sheet includes 25±10% coniferous pulp and 75±10% hardwood pulp; 150-250ppm of polyacrylamide retention agent is added, the amount of cationic starch added is 0.5-1.0% of the absolute dry weight of the paper sheet, the amount of covering agent added is 5-20% of the absolute dry weight of the paper sheet, and the amount of silica sol added is 0.2-0.3% of the absolute dry weight of the paper sheet.
[0014] In some embodiments, in the step of applying coating on the surface of the base paper, china clay and rutile titanium dioxide are used as pigments in the middle coating and the top coating, and the china clay has a particle size of less than 1um, accounting for 88.5%, and the particle size of rutile titanium dioxide is 0.2-0.3um; calcium carbonate is used as a pigment in the top coating, and the particle size is less than 2um, accounting for 95%.
[0015] In a second aspect, an embodiment of the present application provides a black core cardboard, which is prepared by the preparation method described in the above embodiment.
[0016] The method for preparing black core cardboard provided in the embodiment of the present application adopts a base paper process in combination with a coating technology, which solves the problems of decreased strength, poor hitting resistance, and black transmission on both sides of the one-piece black core playing card paper after the paper sheets are dyed with sulphur black in conventional solutions, and has the characteristics of simple process and low cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0018] Figure 1 It is a schematic flow chart of an embodiment of a method for preparing black core cardboard of the present application;
[0019] Figure 2 This is a schematic diagram of the stacked structure of an embodiment of the base paper of the present application;
[0020] Figure 3 It is a structural schematic diagram of an embodiment of the black core cardboard of the present application. DETAILED DESCRIPTION
[0021] The present application is further described in detail below in conjunction with the accompanying drawings and examples. It is particularly noted that the following examples are only used to illustrate the present application, but are not intended to limit the scope of the present application. Similarly, the following examples are only some embodiments of the present application rather than all embodiments, and all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present application.
[0022] The terms "first", "second", and "third" in the embodiments of the present application are only used for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of indicated technical features. Thus, the features defined as "first", "second", and "third" can expressly or implicitly include at least one of the features. In the description of the present application, the meaning of "multiple" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined. In the embodiments of the present application, all directional indications (such as up, down, left, right, front, back...) are only used to explain the relative position relationship, movement, etc. between the components under a certain specific posture (as shown in the accompanying drawings). If the specific posture changes, the directional indication also changes accordingly. The terms "including" and "having" in the embodiments of the present application and any of their variations are intended to cover non-exclusive inclusions. For example, a process, method, system, product, or device that includes a series of steps or units is not limited to the listed steps or units, but optionally also includes steps or units that are not listed, or optionally also includes other steps or components inherent to these processes, methods, products, or devices.
[0023] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.
[0024] Please also read Figure 1 , Figure 1 This is a flow chart of an embodiment of a method for preparing black core cardboard of the present application. It should be noted that the black core cardboard obtained in the embodiment of the present application can be used in paper products such as playing cards. The preparation method includes but is not limited to the following steps.
[0025] Step S100, making base paper.
[0026] See also Figure 2 , Figure 2 1 is a schematic diagram of the stacking structure of an embodiment of the base paper of the present application, wherein the base paper 100 in this embodiment includes a surface layer 110, a surface lining layer 120, a core layer 130, a bottom lining layer 140 and a bottom layer 150 stacked in sequence. The weight of each layer of the base paper 100 is: the surface layer 110 is 30±5gsm, the surface lining layer 120 is 30±5gsm, the core layer 130 is 80±5gsm, the bottom lining layer 140 is 30±5gsm, and the bottom layer 150 is 45±5gsm. The core layer 130 is dyed by adding black dye. The ISO whiteness of the core layer 130 after dyeing is <15%.
[0027] Optionally, the core layer 130 includes 30±5% of coniferous pulp, 50±10% of hardwood pulp and 20±10% of damaged pulp; the core layer 130 is dyed with sulphur black dye, and the amount of sulphur black dye added is 6-10% of the absolute dry pulp of the core layer, specifically 6%, 6.5%, 7%, 8%, 8.5%, 9% and 10%.
[0028] In addition, polyaluminium chloride is added during the dyeing process, and the ratio of polyaluminium chloride to sulphur black is 0.9-1.1:1.0. Optionally, polyacrylamide retention aids and polyacrylamide dry strength agents or cationic starch are added during the dyeing process, wherein the amount of polyacrylamide retention aids (molecular weight of 8 million or more) added is 150-250ppm, specifically 150ppm, 180ppm, 190ppm, 200ppm, 220ppm and 250ppm. The amount of polyacrylamide dry strength agents (molecular weight of 2 million or more) or cationic starch added is 1.5-2.0% of the absolute dry weight of the core layer, specifically 1.5%, 1.6%, 1.65%, 1.8%, 1.9% and 2.0%.
[0029] Among them, the order of adding the raw materials in the step of dyeing the core layer 130 with sulfur black dye is: when the slurry is flowing or stirring, polyaluminum chloride is added to the slurry, and then sulfur black dye is added. After mixing and reacting for 1-5 minutes (for example, about 2 minutes), a dry strength agent or cationic starch is added, and then a retention aid of polyacrylamide is added.
[0030] Optionally, see Figure 2 , the pulp and process of the surface layer 110 and the bottom layer 150 of the base paper 100 in this embodiment include: the paper includes 25±10% of coniferous pulp and 75±10% of hardwood pulp; polyacrylamide (molecular weight above 8 million) retention agent is added at 150-250ppm, specifically 150ppm, 180ppm, 190ppm, 200ppm, 220ppm and 250ppm. The amount of cationic starch added is 0.5-1.0% of the absolute dry weight of the paper, specifically 0.5%, 0.6%, 0.65%, 0.8%, 0.9% and 1.0%. The amount of covering agent added is 5-15% of the absolute dry weight of the paper, specifically 5%, 6%, 8%, 10%, 12% and 15%.
[0031] Optionally, see Figure 2 The pulp and process of the surface lining layer 120 and the bottom lining layer 140 of the base paper 100 in this embodiment include: the paper sheet includes 25±10% of coniferous pulp and 75±10% of hardwood pulp; the addition of polyacrylamide (molecular weight above 8 million) retention agent is 150-250ppm, specifically, it can be 150ppm, 180ppm, 190ppm, 200ppm, 220ppm and 250ppm.
[0032] The amount of cationic starch added is 0.5-1.0% of the absolute dry weight of the paper sheet, and specifically can be 0.5%, 0.6%, 0.65%, 0.8%, 0.9% and 1.0%. The amount of covering agent added is 5-20% of the absolute dry weight of the paper sheet, and specifically can be 5%, 6%, 8%, 10%, 12%, 15% and 20%. The amount of silica sol added is 0.2-0.3% of the absolute dry weight of the paper sheet, and specifically can be 0.2%, 0.21%, 0.25%, 0.28% and 0.3%. The order of adding each raw material is: cationic starch, covering agent, retention agent and silica sol are added to the slurry in a flowing or stirring state.
[0033] After each layer of pulp is formed on the screen, the compounding order of the five layers of paper sheets is core layer 130, bottom lining layer 140, surface lining layer 120, bottom layer 150 and surface layer 110; after compounding, the whiteness of the base paper 100 reaches> 70%.
[0034] Please refer to the table below, which compares the parameters of several different embodiments.
[0035]
[0036]
[0037] The technical solution in the embodiment of the present application realizes the preparation of the product on a five-layer fourdrinier paper machine, and is designed to add sulphur black dye to the core layer for dyeing. Since the particle charge (PCD) of the sulphur black dye and the surface of the papermaking fiber as a whole is negative, a strongly cationic polyaluminium chloride is selected to fully fix the sulphur black on the fiber surface. After research, it is found that the optimal ratio of the two is 0.9-1.1. Since paper sheet enhancers such as dry strength agents and cationic starch are also positively charged, there will be a certain competitive effect with polyaluminium chloride in the fixation of sulphur black. However, after the fiber surface to which sulphur black is added in large quantities is covered by sulphur black, the hydrogen bonding force between the fibers is weakened, and the strength of the paper sheet is reduced. Therefore, after the polyaluminium chloride is fixed, dry strength agents and cationic starch are added in the paper sheet in an appropriate amount for fiber reinforcement, which does not affect the fixation efficiency of polyaluminium chloride. Adding ultra-high molecular weight polyacrylamide (molecular weight above 8 million) retention aids to micro-flocculate the fibers, improve the retention rate of fibers in the net forming, and reduce the pollution of sulphur black fibers to the paper machine system. After the single-layer paper sheet is formed, when the lining layer and the core layer are compounded, starch is sprayed on the paper sheet. Part of the starch will penetrate into the paper sheet of the lining layer. After the starch is gelatinized, the bonding strength of the fibers in the paper sheet can be improved, and part of it will adhere to the fibers of the core layer and the bottom lining layer to improve the bonding strength between the layers. This ensures that when a large amount of sulphur black is added to the core layer and a large amount of covering agent is added to the other four layers, the strength of the paper sheet can still meet the requirements of playing card paper with a durability of >800 times and interlayer bonding strength higher than 500.
[0038] The covering agent in the technical solution of the embodiment of the present application can be an inorganic filler with a high refractive index, and the average particle size of the filler is less than 1um. The surface layer, bottom layer and lining layer have low quantitative content. In order to improve the retention rate of the covering agent, the covering agent is pretreated, and the pretreatment agent used is one or two of dimethylamine-epichlorohydrin polymer and polyacrylamide polymer. The titanium dioxide dispersant is a polyacrylic acid salt anion polymer, and a polymer with a strong cationic PCD>1 million ueq / l is used to micro-flocculate the small filler particles through the charge interaction between anions and cations to increase the particle size of the filler. At the same time, the filler surface can carry partial positive charges to jointly improve the filler retention rate.
[0039] Optionally, see Figure 1 The method for preparing black core cardboard in this embodiment further includes step S200 of coating a coating on the surface of the base paper.
[0040] Optionally, see Figure 3 , Figure 3 1 is a schematic diagram of the structure of an embodiment of the black core paper of the present application, wherein the black core paper is provided with coatings 200 on both sides of the base paper 100. The coatings 200 each include a pre-coating layer 210, a middle coating layer 220 and a top coating layer 230 which are stacked in sequence.
[0041] Among them, the pre-coat layer 210 in the coating fills the gaps on the surface of the paper fiber and modifies the paper surface. The coatings of the middle coating layer 220 and the top coating layer 230 use flat china clay and rutile titanium dioxide with a high refractive index as pigments, wherein the china clay particle size is less than 1um, accounting for 88.5%, the rutile titanium dioxide particle size is 0.2-0.3um, and calcium carbonate is used as a pigment in the top coating layer 230, and the particle size of calcium carbonate is less than 2um, accounting for 95%, which are all particle size ranges with good scattering power of the pigment. Therefore, the coating has good opacity and good covering power for the blackness of the base paper. After coating, the whiteness of the paper surface reaches>80%, and there is no difference between the two sides. Regarding other components in the coatings of the pre-coat layer 210, the middle coating layer 220 and the top coating layer 230, such as latex, adhesives, dispersants, etc., the detailed features of this part are within the understanding of those skilled in the art and will not be repeated here.
[0042] The following table is a comparison of parameters of several specific embodiments.
[0043]
[0044]
[0045] The preparation method of the black core cardboard in the embodiment of the present application, through the core layer dyeing process and the process design of the base paper, makes the cardboard have good anti-see-through performance, beating resistance and processability, develops a new base paper covering technology, and combines it with the coating formula to improve the covering property, i.e., opacity, of the cardboard, so that the front and back sides of the playing card paper have the same high whiteness. The present invention can produce black core playing card paper with good anti-see-through performance in one piece through a five-layer fourdrinier paper machine.
[0046] The above descriptions are only some embodiments of the present application, and do not limit the protection scope of the present application. Any equivalent device or equivalent process transformation made using the contents of the present application specification and drawings, or directly or indirectly used in other related technical fields, are also included in the patent protection scope of the present application.
Claims
1. A method for preparing black core cardboard, It is characterized in that The preparation method comprises: Papermaking base paper; the base paper comprises a surface layer, a surface lining layer, a core layer, a bottom lining layer and a bottom layer which are stacked in sequence; wherein the core layer is dyed with sulfur black dye, and the addition amount of the sulfur black dye is 6-10% of the absolute dry pulp of the core layer; A coating is applied on the surface of the base paper.
2. The preparation method according to claim 1, It is characterized in that In the step of dyeing the core layer with sulphur black dye, the ratio of polyaluminium chloride to sulphur black is 0.9-1.1:1.
0.
3. The preparation method according to claim 2, It is characterized in that In the step of dyeing the core layer with sulfur black dye, polyacrylamide retention aid and polyacrylamide dry strength agent or cationic starch are also added, wherein the amount of polyacrylamide retention aid added is 150-250ppm; the amount of polyacrylamide dry strength agent or cationic starch added is 1.5-2.0% of the absolute dry weight of the core layer.
4. The preparation method according to claim 3, It is characterized in that The order of adding the raw materials in the step of dyeing the core layer with sulfur black dye is as follows: when the slurry is flowing or stirring, polyaluminium chloride is added to the slurry, then sulfur black dye is added, after mixing and reacting for 1-5 minutes, a dry strength agent or cationic starch is added, and then a retention aid of polyacrylamide is added.
5. The preparation method according to claim 4, It is characterized in that The core layer comprises 30±5% of conifer pulp, 50±10% of hardwood pulp and 20±10% of broke pulp.
6. The preparation method according to claim 1, It is characterized in that In the step of making base paper, the weight of each layer of the base paper is: surface layer 30±5gsm, surface lining layer 30±5gsm, core layer 80±5gsm, bottom lining layer 30±5gsm, bottom layer 45±5gsm.
7. The preparation method according to claim 1, It is characterized in that The pulp and process of the surface layer and the bottom layer include: the paper sheet includes 25±10% of conifer pulp and 75±10% of hardwood pulp; 150-250ppm of polyacrylamide retention aid is added, the addition amount of cationic starch is 0.5-1.0% of the absolute dry weight of the paper sheet, and the addition amount of covering agent is 5-15% of the absolute dry weight of the paper sheet.
8. The preparation method according to claim 7, It is characterized in that The slurry and process of the surface lining layer and the bottom lining layer include: the paper sheet includes 25±10% of coniferous pulp and 75±10% of hardwood pulp; 150-250ppm of polyacrylamide retention aid is added, the amount of cationic starch added is 0.5-1.0% of the absolute dry weight of the paper sheet, the amount of covering agent added is 5-20% of the absolute dry weight of the paper sheet, and the amount of silica sol added is 0.2-0.3% of the absolute dry weight of the paper sheet.
9. The preparation method according to claim 1, It is characterized in that In the step of applying coating on the surface of the base paper, china clay and rutile titanium dioxide are used as pigments in both the middle coating and the top coating, and the china clay has a particle size of less than 1um, accounting for 88.5%, and the rutile titanium dioxide has a particle size of 0.2-0.3um; calcium carbonate is used as a pigment in the top coating, and the particle size of less than 2um accounts for 95%.
10. A black core cardboard, It is characterized in that The black core cardboard is prepared by the preparation method described in any one of claims 1 to 9.
Citation Information
Patent Citations
Processing method of block-core playing card paper
CN101851876A
Composite decorative paper for artificial board and preparation method thereof
CN104313936A
Playing card paper and preparation method thereof
CN117779518A
Production of two-side coated paper
JP1995119085A