Anti-slip emery blind track nail and preparation method thereof

By using stainless steel material and carbam anti-slip part on the blind path nails combined with high-hardness silicon carbide sand particles and phenolic resin, the problem of long anti-slip pattern of blind path nails is solved, and the wear resistance and service life are significantly improved .

CN119061816APending Publication Date: 2024-12-03WUYI XIONGCHANG HARDWARE MFG CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202310646010.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-06-01
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The anti-slip pattern of existing blind path nails is made by integrated die-casting molding process, which is not durable, easily wears and loses its anti-slip function.

Method used

The blind path nail body is made of stainless steel, with grooves formed on the top, and the anti-slip part of the cartilage is formed inside, and anti-slip convex strips are formed on the surface of the anti-slip part of the cartilage is formed, and the high-hardness silicon carbide sand particles and phenolic resin are combined for sectional heating and pressing.

Benefits of technology

It significantly improves the wear resistance and service life of blind path nails, the material is hard, and the anti-slip pattern is easy to form, which enhances the strength and anti-slip performance of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119061816A_ABST
    Figure CN119061816A_ABST
Patent Text Reader

Abstract

The invention discloses an anti-skid emery blind sidewalk nail which comprises a blind sidewalk nail body, the top of the blind sidewalk nail body is concaved downwards to form a groove, an emery anti-skid part is formed in the groove, and anti-skid protruding strips protruding out of the surface of the emery anti-skid part are integrally formed on the upper surface of the emery anti-skid part. According to the blind sidewalk nail, the anti-skid part is formed on the blind sidewalk nail body through the cooperation of the carborundum material and the phenolic resin in a heating and pressing mode, due to the fact that the material is hard, the strength and abrasion resistance of the manufactured product are greatly improved, and in addition, the anti-skid patterns are easy to form.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of blind road spike installation, and in particular relates to an anti-slip diamond sand blind road spike and a preparation method thereof. Background Art

[0002] Blind path indicator nails are used to indicate blind paths because of their unique patterns or colors. Publication No. CN202809438U discloses an embossed one-piece blind path board, including a rectangular plate body and a number of blind path nails distributed on the surface of the rectangular plate body in a rectangular array, each blind path nail has an anti-slip pattern on its upper surface, the blind path nail and its surface anti-slip pattern are integrally die-cast with the rectangular plate body, the anti-slip pattern of this structure and the rectangular plate body are integrally die-cast, the anti-slip pattern made by this process is not durable and is easily worn, thereby losing its function;

[0003] Therefore, developing a blind road stud that can improve the wear resistance, anti-skid performance and service life of the product is an urgent problem to be solved. Summary of the invention

[0004] In view of the problems mentioned in the background technology, the purpose of the present invention is to provide an anti-slip diamond sand blind road spike and a preparation method to solve the problems existing in the existing background technology.

[0005] The above technical objectives of the present invention are achieved through the following technical solutions:

[0006] A non-slip diamond grit tactile road stud comprises a tactile road stud body, the top of the tactile road stud body is concave to form a groove, a diamond grit anti-slip part is formed in the groove, and an anti-slip convex strip protruding from the surface of the diamond grit anti-slip part is integrally formed on the upper surface of the diamond grit anti-slip part.

[0007] Preferably, a plurality of annular anti-skid convex strips are formed on the surface of the diamond anti-skid portion.

[0008] Preferably, the blind road spike body is made of stainless steel.

[0009] A method for preparing anti-slip diamond sand blind road studs comprises the following steps:

[0010] S1: Molded stainless steel blind stud body;

[0011] S2: ingredients; including high hardness silicon carbide sand and curing agent according to weight percentage;

[0012] S3: Put the above ingredients into a stirring device according to the proportion and pre-mix for 2-3 hours;

[0013] S4: Filling the mixed material prepared in step S3 into the groove of the blind road stud body;

[0014] S5: compaction;

[0015] S6: placing the semi-finished product obtained in step S5 into a hot press for segmented heating;

[0016] S7: Cooling to form a finished product.

[0017] Preferably, the method for performing segmented heating in step S6 comprises the following steps:

[0018] S61: heating at a temperature of 100-120° C. for 5-8 hours;

[0019] S62: heating at 150-160° C. for 10-12 hours;

[0020] S63: Heat at 180-220°C for 5-8h.

[0021] Preferably, the composition comprises the following components by weight: 75-90% of high-hardness silicon carbide sand particles and 10-25% of a curing agent.

[0022] Preferably, the curing agent is phenolic resin.

[0023] In summary, the present invention mainly has the following beneficial effects:

[0024] In the present application, the anti-skid portion is formed on the main body of the blind stud by heating and pressing the diamond abrasive material and phenolic resin. Due to the hardness of the material, the strength and wear resistance of the product are greatly improved. In addition, the anti-skid pattern is easy to form. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 It is a schematic diagram of the structure of the present invention;

[0026] Figure 2 It is a cross-sectional view of the present invention. DETAILED DESCRIPTION

[0027] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] Example 1

[0029] refer to Figure 1-2A non-slip diamond grit tactile road spike, comprising a tactile road spike body 1, the top of the tactile road spike body is concave to form a groove 2, a diamond grit anti-slip part 3 is formed in the groove, and an anti-slip convex strip 4 protruding from the surface of the diamond grit anti-slip part is integrally formed on the upper surface of the diamond grit anti-slip part, and a plurality of annular anti-slip convex strips are formed on the surface of the diamond grit anti-slip part. The tactile road spike body is made of stainless steel.

[0030] A method for preparing anti-slip diamond sand blind road studs comprises the following steps:

[0031] S1: Molded stainless steel blind stud body;

[0032] S2: ingredients; including high hardness silicon carbide sand and curing agent according to weight percentage;

[0033] S3: Put the above ingredients into a stirring device according to the proportion and pre-mix for 3 hours;

[0034] S4: Filling the mixed material prepared in step S3 into the groove of the blind road stud body;

[0035] S5: compaction;

[0036] S6: placing the semi-finished product obtained in step S5 into a hot press for segmented heating;

[0037] S7: Cooling to form a finished product.

[0038] The method for performing segmented heating in step S6 includes the following steps:

[0039] S61: heating at 100° C. for 6 h;

[0040] S62: heating at 160° C. for 10 h;

[0041] S63: heating at 200° C. for 5 hours.

[0042] In this embodiment, the following components are included by weight: 85% of high-hardness silicon carbide sand particles and 15% of a curing agent; the curing agent is a phenolic resin.

[0043] Example 2

[0044] refer to Figure 1-2 A non-slip diamond grit tactile road spike, comprising a tactile road spike body, the top of the tactile road spike body is concave to form a groove, a diamond grit anti-slip part is formed in the groove, an anti-slip convex strip protruding from the surface of the diamond grit anti-slip part is integrally formed on the upper surface of the diamond grit anti-slip part, and a plurality of annular anti-slip convex strips are formed on the surface of the diamond grit anti-slip part. The tactile road spike body is made of stainless steel.

[0045] A method for preparing anti-slip diamond sand blind road studs comprises the following steps:

[0046] S1: Molded stainless steel blind stud body;

[0047] S2: ingredients; including high hardness silicon carbide sand and curing agent according to weight percentage;

[0048] S3: Put the above ingredients into a stirring device according to the proportion and pre-mix for 2-3 hours;

[0049] S4: Filling the mixed material prepared in step S3 into the groove of the blind road stud body;

[0050] S5: compaction;

[0051] S6: placing the semi-finished product obtained in step S5 into a hot press for segmented heating;

[0052] S7: Cooling to form a finished product.

[0053] The method for performing segmented heating in step S6 includes the following steps:

[0054] S61: heating at 110° C. for 8 h;

[0055] S62: heating at 160° C. for 10 h;

[0056] S63: Heat at 220° C. for 5 hours.

[0057] In this embodiment, the following components are included by weight: 90% of high-hardness silicon carbide sand particles and 10% of a curing agent; the curing agent is a phenolic resin.

[0058] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. An anti-slip diamond sand blind stud, Features: The invention comprises a blind stud body, the top of which is concave to form a groove, a diamond abrasive anti-skid part is formed in the groove, and an anti-skid convex strip protruding from the surface of the diamond abrasive anti-skid part is integrally formed on the upper surface of the diamond abrasive anti-skid part.

2. The anti-slip diamond sand blind stud according to claim 1, Features: A plurality of annular anti-skid convex strips are formed on the surface of the diamond anti-skid portion.

3. The anti-slip diamond grit blind stud according to claim 1, Features: The blind road spike body is made of stainless steel.

4. A method for preparing anti-skid diamond sand blind road studs, Features: The steps include: S1: Molded stainless steel blind stud body; S2: ingredients; including high hardness silicon carbide sand and curing agent according to weight percentage; S3: Put the above ingredients into a stirring device according to the proportion and pre-mix for 2-3 hours; S4: Filling the mixed material prepared in step S3 into the groove of the blind road stud body; S5: compaction; S6: placing the semi-finished product obtained in step S5 into a hot press for segmented heating; S7: Cooling to form a finished product.

5. A method for preparing anti-slip diamond sand blind road studs according to claim 4, Features: The method for performing segmented heating in step S6 comprises the following steps: S61: heating at a temperature of 100-120° C. for 5-8 hours; S62: heating at 150-160° C. for 10-12 hours; S63: Heat at 180-220°C for 5-8h.

6. A method for preparing anti-slip diamond sand blind road studs according to claim 4, Features: The invention comprises the following components by weight: 75-90% of high-hardness silicon carbide sand particles and 10-25% of a curing agent.

7. A method for preparing anti-slip diamond sand blind road studs according to claim 4, Features: The curing agent is phenolic resin.

Citation Information

Patent Citations

  • Integrally molded embossed blind track plate

    CN202809438U

  • Rail polishing and grinding wheel

    CN107363737A

  • Grinding wheel low-temperature curing process

    CN109623684A

  • Metal dumm drift nail

    CN201121297Y

  • Antiskid road stud

    CN201485801U