Powdery medicament feeding device and pyrogenic process refining oxidation impurity removal method for metal
The powdered medicament dosing device addresses low efficiency and high consumption in traditional methods by directly adding reagents to high-temperature molten metal with compressed air, enhancing reaction speed and reducing waste.
Patent Information
- Application Number
- CN202411110017.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-12-03
AI Technical Summary
Traditional methods for adding powdered reagents in metal fire refining require manual operation, leading to low reaction efficiency, high fuel consumption, and reagent wastage due to insufficient contact area and slow reaction times.
A powdered medicament dosing device with a medicine storage bin, discharge valve, metering tank, and high-temperature resistant medicine pipe, combined with compressed air, allows direct addition of powdered reagents into high-temperature molten metal, ensuring rapid reaction and reduced consumption.
The device enables rapid melting and oxidation of powdered reagents within the molten metal, improving reaction efficiency and reducing fuel and reagent consumption by ensuring full contact and uniform distribution.
Smart Images

Figure CN119063480A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of powdered medicament dosing, in particular to a powdered medicament dosing device and a metal pyro-refining oxidation and impurity removal method. Background Art
[0002] An oxidation impurity removal method is often used in the process of fire refining of metals, such as oxidation to remove arsenic and lead in the process of antimony refining. Powdered reagents are usually used in the oxidation impurity removal process, such as soda ash is needed to remove arsenic in the process of antimony refining, and monoammonium phosphate is needed to remove lead. Usually, the reagent is added manually at the top of the furnace feed port. After the reagent is added, it will first float on the surface of the molten metal, and then gradually melt at high temperature; then compressed air is blown into the molten metal through a special pipeline, so that the molten metal continues to surge, which not only plays the role of oxidizing impurities, but also stirs the molten metal; as oxidation and stirring occur, the reagent reacts with the impurities to generate a slag that does not melt in the molten metal and floats on the surface of the molten metal. After the reaction is complete, the slag is scraped out to complete the removal of impurities. However, the addition of reagents in the above impurity removal process requires manual operation, and the production labor intensity is relatively high; and after the reagents are added, they gather and float on the surface of the molten metal, which requires a certain amount of time to melt, wasting fuel and production time; the reagents are light and float on the surface, and during the compressed air stirring and oxidation process, the contact area between the impurities and the reagents is small, the reaction is slow, and a lot of reagents are wasted.
[0003] Therefore, there is an urgent need for a powdered reagent dosing device and a metal fire refining oxidation impurity removal method, which can add powdered reagents into the high-temperature molten metal without manual operation, thereby improving reaction efficiency and reducing fuel and reagent consumption. Summary of the invention
[0004] The purpose of the present invention is to provide a powder reagent dosing device and a method for fire refining and oxidation impurity removal of metals, aiming to solve the technical problems of low reaction efficiency and high fuel and reagent consumption in traditional powder reagent dosing methods.
[0005] To achieve the above objectives, in a first aspect, the present invention provides a powdered medicament dosing device, comprising:
[0006] A medicine storage bin is used to store powdered medicines;
[0007] A discharge valve, disposed at the bottom of the medicine storage bin, for controlling the release of the powdered medicine therein;
[0008] A metering tank is arranged directly below the discharge valve, and is used to receive the powdered medicine released by the discharge valve, and is capable of weighing and metering the received powdered medicine;
[0009] The metering tank is also provided with a medicine delivery pipe, and the end of the medicine delivery pipe is also provided with a high-temperature resistant medicine pipe, which is used to extend into the high-temperature molten metal to deliver the powdered medicine in the metering tank to the inside of the high-temperature molten metal;
[0010] An air inlet pipe is provided at the bottom of the metering tank for connecting compressed air to provide power for conveying the powdered medicine.
[0011] As a further improvement of the above solution, a metering module is provided in the metering tank for weighing the powdered medicine dropped therein; and the metering module is communicatively connected with the discharge valve to control the switch of the discharge valve.
[0012] As a further improvement of the above solution, the discharge valve is a star-shaped discharge valve.
[0013] As a further improvement of the above scheme, the powdered medicine dosing device also includes an adjusting structure, which is arranged between the medicine delivery pipe and the high-temperature resistant medicine pipe so that the high-temperature resistant medicine pipe can be flexibly moved, thereby being able to deliver the powdered medicine to different positions and different depths of the high-temperature molten metal; preferably, the adjusting structure is a connecting hose.
[0014] As a further improvement of the above solution, a first control valve is provided on the air intake pipe for controlling the on and off of compressed air.
[0015] As a further improvement of the above solution, a second control valve is provided on the medicine delivery pipe to control the on-off of powdered medicine delivery.
[0016] In a second aspect, the present invention further provides a method for fire refining oxidation and impurity removal of metals, using a powdered agent dosing device as provided in the first aspect, the steps of which include:
[0017] S1. Sampling the high-temperature crude metal liquid in the refining furnace to detect the impurity content in the crude metal liquid;
[0018] S2. Calculate the amount of impurities in the crude molten metal and the required amount of powdered impurity removal agent according to the obtained impurity content;
[0019] S3, setting the required dosage of the powdered impurity-removing agent, releasing the powdered impurity-removing agent from the agent storage bin into the metering tank and measuring it;
[0020] S4. Connect the air inlet pipe at the bottom of the metering tank to compressed air. Under the action of the compressed air, the powdered impurity-removing agent is sequentially transported through the agent delivery pipe and the high-temperature resistant agent pipe to the inside of the high-temperature molten metal for oxidation and impurity-removing reaction.
[0021] As a further improvement of the above scheme, in step S4, the angle, position and / or depth of the high-temperature resistant agent tube extending into the high-temperature crude metal liquid is adjusted so that the impurity removal agent melts in the high-temperature metal liquid and reacts quickly with the impurities for full oxidation.
[0022] As a further improvement of the above scheme, in step S4, the angle, position and / or depth of the high temperature resistant agent tube extending into the high temperature molten metal is adjusted by means of an adjustment structure provided between the agent delivery tube and the high temperature resistant agent tube.
[0023] As a further improvement of the above scheme, in step S4, the impurity removal efficiency is controlled by controlling the size of the valve opening corresponding to the compressed air and / or controlling the size of the compressed air pressure.
[0024] As a further improvement of the above scheme, the average particle size of the powdery impurity-removing agent is less than 3 mm.
[0025] Since the present invention adopts the above technical solution, the beneficial effects of this application are:
[0026] The present invention provides a powder medicine dosing device, comprising: a medicine storage bin for storing powder medicine; a discharge valve arranged at the bottom of the medicine storage bin for controlling the release of the powder medicine therein; a metering tank arranged directly below the discharge valve for receiving the powder medicine released by the discharge valve and being able to weigh and meter the received powder medicine; the metering tank is also provided with a medicine delivery pipe, and the end of the medicine delivery pipe is also provided with a high-temperature resistant medicine pipe for extending into high-temperature molten metal to deliver the powder medicine in the metering tank to the inside of the high-temperature molten metal; the bottom of the metering tank is provided with an air inlet pipe for connecting compressed air to feed the powder medicine The device provides power for conveying; with such a configuration, a predetermined weight of powdered medicine can be obtained through the metering tank, and an air inlet pipe for introducing compressed air is provided at the bottom of the metering tank. When in use, the predetermined weight of powdered medicine in the metering tank is conveyed to the corresponding high-temperature molten metal through the medicine conveying pipe and the high-temperature resistant medicine pipe by compressed air. Compared with the traditional method of adding medicine on the surface of the high-temperature molten metal, the device can directly add the powdered medicine to the interior of the high-temperature molten metal, thereby realizing rapid melting, and immediately reacting with the medicine after the impurities are rapidly oxidized together with the compressed air, thereby improving the reaction efficiency and reducing the consumption of fuel and medicine;
[0027] In some preferred embodiments, an adjustment structure is also provided, and the adjustment structure is provided between the agent delivery pipe and the high-temperature resistant agent pipe. Preferably, the adjustment structure is a connecting hose, and the setting of the adjustment structure can flexibly move the high-temperature resistant agent pipe, so that the powdered agent can be transported to different positions and different heights of the high-temperature molten metal, so that the powdered agent can fully react with the high-temperature molten metal, thereby improving the reaction efficiency and reducing fuel and agent consumption.
[0028] 2. The present invention also provides a method for oxidative impurity removal of metal by fire refining, the steps of which include: first sampling the high-temperature crude metal liquid in the refining furnace, detecting the impurity content in the crude metal liquid, and then calculating the impurity amount in the crude metal liquid and the required amount of powdered impurity removal agent; then releasing the powdered impurity removal agent from the agent storage bin into the metering tank and metering it; finally connecting the air inlet pipe at the bottom of the metering tank to compressed air, and the powdered impurity removal agent is sequentially transported to the interior of the high-temperature crude metal liquid through the agent delivery pipe and the high-temperature resistant agent pipe under the action of compressed air for oxidative impurity removal reaction; such an arrangement, under the action of compressed air, a certain amount of powdered impurity removal agent is transported to the interior of the high-temperature metal liquid, so that the powdered impurity removal agent can It can melt quickly, and immediately react with the impurities in it after being quickly oxidized by the compressed air, thereby improving the reaction efficiency and reducing the consumption of fuel and reagents. In some preferred embodiments, the angle, position and / or depth of the high-temperature resistant reagent tube extending into the high-temperature crude metal liquid is adjusted, so that the impurity-removing reagent can be relatively evenly distributed in the high-temperature metal liquid, and react quickly with the impurities to fully oxidize, thereby improving the reaction efficiency. And because the powdered impurity-removing reagent can be evenly transported to the high-temperature crude antimony liquid, the reaction is more complete, so that the quantitative addition of the impurity-removing reagent can be achieved, which can greatly reduce the reagent consumption compared with the traditional method of sprinkling the impurity-removing reagent on the surface of the high-temperature metal liquid. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying any creative work.
[0030] Figure 1 The present invention is a schematic diagram of a powdered medicine dosing device conveying powdered medicine to a refining furnace.
[0031] Reference numerals:
[0032] 1. Medicine storage bin; 2. Discharge valve; 3. Metering tank; 31. Medicine delivery pipe; 32. High temperature resistant medicine pipe; 33. Second control valve; 34. Air inlet pipe; 35. First control valve; 36. Connecting hose;
[0033] 4. Working door; 5. Refining furnace; 6. High-temperature molten metal.
[0034] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with the implementation methods and with reference to the accompanying drawings. DETAILED DESCRIPTION
[0035] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0036] Furthermore, the technical solutions between the various embodiments of the present invention may be combined with each other, but this must be based on the fact that they can be implemented by ordinary technicians in the field. When the combination of technical solutions is mutually contradictory or cannot be implemented, it should be deemed that such combination of technical solutions does not exist and is not within the scope of protection required by the present invention.
[0037] Example 1
[0038] See also Figure 1 The present invention provides a powdered medicine dosing device, comprising:
[0039] A medicine storage bin 1 is used for storing powdered medicine;
[0040] A discharge valve 2 is provided at the bottom of the medicine storage bin 1 and is used to control the release of the powdered medicine therein;
[0041] The metering tank 3 is arranged directly below the discharge valve 2, and is used to receive the powdered medicine released through the discharge valve 2, and can weigh and measure the received powdered medicine;
[0042] The metering tank is also provided with a medicine delivery pipe 31, and the end of the medicine delivery pipe 31 is also provided with a high temperature resistant medicine pipe 32, which is used to extend into the high temperature molten metal 6 to deliver the powdered medicine in the metering tank 3 to the inside of the high temperature molten metal 6; in this embodiment, the medicine delivery pipe 31 is provided with a second control valve 33, which is used to control the on and off of the powdered medicine delivery;
[0043] An air inlet pipe 34 is provided at the bottom of the metering tank 3 for connecting compressed air to provide power for the delivery of the powdered medicine; in this embodiment, a first control valve 35 is provided on the air inlet pipe 34 for controlling the on and off of the compressed air;
[0044] With such an arrangement, a predetermined weight of powdered medicine can be obtained through the metering tank 3, and an air inlet pipe 34 for introducing compressed air is provided at the bottom of the metering tank. When in use, the predetermined weight of powdered medicine in the metering tank 3 is transported to the corresponding high-temperature molten metal 6 through the medicine delivery pipe 31 and the high-temperature resistant medicine pipe 32 by compressed air. Compared with the traditional method of adding medicine on the surface of the high-temperature molten metal 6, the present device can directly add the powdered medicine to the interior of the high-temperature molten metal 6, thereby achieving rapid melting, and immediately together with the compressed air, the impurities are rapidly oxidized and react with the medicine, thereby improving the reaction efficiency and reducing the consumption of fuel and medicine.
[0045] As a preferred embodiment, a metering module is provided in the metering tank 3 for weighing the powdered medicine dropped therein; and the metering module is communicatively connected with the discharge valve 2 to control the switch of the discharge valve 2; specifically, when the weight measured by the weighing module reaches a predetermined weight, a closing signal is sent to the discharge valve 2, and the discharge valve 2 that receives the closing signal is closed to stop discharging; the metering module is communicatively connected with the discharge valve 2 to realize automatic release of a predetermined weight of powdered medicine without manual intervention, and only the predetermined weight needs to be input in advance on the controller of the metering tank 3.
[0046] As a preferred embodiment, the discharge valve 2 is a star-shaped discharge valve 2, which can achieve fast and uniform discharge during material transportation, thereby improving production efficiency. In addition, the star-shaped discharge valve 2 can also be adjusted according to the characteristics of the material to achieve the best discharge effect, further improving production efficiency; the use of advanced transmission devices and control systems can achieve automatic operation, reduce manual intervention, and thus improve the stability and reliability of the equipment.
[0047] As a preferred embodiment, the powdered medicament dosing device further includes an adjustment structure. In this embodiment, the adjustment structure is a connecting hose 36, and the connecting hose 36 is arranged between the medicament delivery pipe 31 and the high temperature resistant medicament pipe 32 so as to flexibly move the high temperature resistant medicament pipe 32;
[0048] Preferably, the connecting hose 36 includes but is not limited to a nylon hose, a stainless steel hose, a PVC hose, a rubber hose, etc., and can also be a retractable hose so as to flexibly adjust the depth and position of the high-temperature resistant agent tube 32 extending into the high-temperature molten metal 6; thereby, the powdered agent can be transported to different positions and different heights of the high-temperature molten metal 6, so that the powdered agent can fully react with the high-temperature molten metal 6, thereby improving the reaction efficiency and reducing fuel and agent consumption.
[0049] In order to further illustrate the inventive concept of the present invention, the following Figure 1 The process of adding the powdered medicine adding device to the refining furnace 5 is described as follows:
[0050] First, the high-temperature molten metal 6 in the refining furnace 5 is sampled, and the impurity amount and the reagent requirement (i.e., the predetermined weight) are calculated; the powdered reagent is stored in the reagent storage bin 1, and falls into the metering tank 3 through the star-shaped discharge valve 2, thereby realizing the metering of the powdered reagent; after the powdered reagent reaches the predetermined weight, the feeding is stopped, and the star-shaped discharge valve 2 is closed; the second control valve 33 on the reagent output pipe is opened, and the first control valve 35 on the air inlet pipe 34 is opened, and the powdered reagent enters the refining furnace 5 through the reagent delivery pipe 31 with compressed air as the power; the high-temperature resistant reagent pipe 32 is inserted into the high-temperature molten metal 6 from the working door 4 of the refining furnace 5; the depth of the high-temperature reagent pipe outlet is adjusted by connecting the hose 36, and the powdered reagent is melted in the antimony liquid, and the impurities are oxidized and react quickly with the reagent, thereby realizing efficient impurity removal.
[0051] Example 2
[0052] The present invention also provides a method for fire refining oxidation impurity removal of metals, using a powdered reagent dosing device as provided in Example 1. In this embodiment, fire refining oxidation impurity removal of antimony is taken as an example for description. Specifically, the steps include:
[0053] S1, sampling the high-temperature crude antimony liquid in the refining furnace 5, and detecting the impurity content in the crude antimony liquid;
[0054] S2. Calculating the amount of impurities in the crude antimony liquid and the required amount of powdered impurity-removing agent according to the obtained impurity content;
[0055] S3, setting the required dosage of the powdered impurity-removing agent, releasing the powdered impurity-removing agent from the agent storage bin 1 into the metering tank 3 and measuring it;
[0056] S4, connecting the air inlet pipe 34 at the bottom of the metering tank 3 to compressed air, and the powdered impurity-removing agent is transported to the high-temperature crude antimony liquid through the agent delivery pipe 31 and the high-temperature resistant agent pipe 32 in sequence under the action of the compressed air for oxidation and impurity-removing reaction;
[0057] With such an arrangement, a quantitative amount of powdered impurity-removing agent is transported into the high-temperature antimony liquid under the action of compressed air, so that the powdered impurity-removing agent can be quickly melted and immediately react with the impurities in the high-temperature antimony liquid after being rapidly oxidized together with the compressed air, thereby improving the reaction efficiency and reducing the consumption of fuel and agents. In certain preferred embodiments, the angle, position and / or depth of the high-temperature resistant agent tube 32 extending into the high-temperature crude antimony liquid is adjusted, so that the impurity-removing agent can be relatively evenly distributed in the high-temperature antimony liquid and react rapidly with the impurities to be fully oxidized, thereby improving the reaction efficiency. Moreover, since the powdered impurity-removing agent can be evenly transported into the high-temperature crude antimony liquid, the reaction is more complete, thereby realizing the quantitative addition of the impurity-removing agent. Compared with the traditional method of sprinkling the impurity-removing agent on the surface of the high-temperature antimony liquid, the agent consumption can be greatly reduced.
[0058] As a preferred embodiment, in step S4, the angle, position and / or depth of the high temperature resistant agent tube 32 extending into the high temperature crude antimony liquid is adjusted by means of an adjustment structure provided between the agent delivery tube 31 and the high temperature resistant agent tube 32;
[0059] Preferably, the regulating structure is a connecting hose 36 connecting the reagent delivery pipe 31 and the high temperature resistant reagent pipe 32. Since the connecting hose 36 is flexible, the angle, position and / or depth of the high temperature resistant reagent pipe 32 extending into the high temperature crude antimony liquid can be flexibly adjusted by setting the connecting hose 36, and under the action of compressed air, the powdered impurity removal agent is fully diffused into the high temperature crude antimony liquid, so that the impurities can be quickly oxidized and reacted with the impurity removal agent, thereby improving the reaction efficiency;
[0060] In certain preferred embodiments, the adjustment structure includes a telescopic tube and a universal joint arranged at either end of the telescopic tube, the universal joint can adjust the angle at which the high-temperature resistant agent tube 32 extends into the high-temperature crude antimony liquid, and the telescopic tube can adjust the position and / or depth of the high-temperature resistant agent tube 32 extending into the high-temperature crude antimony liquid. Under the adjustment of the universal joint and the telescopic tube, combined with the action of compressed air, the powdered impurity removal agent is fully diffused into the high-temperature crude antimony liquid, so that the impurities can be quickly oxidized and react with the impurity removal agent, thereby improving the reaction efficiency.
[0061] As a preferred embodiment, in step S4, the impurity removal efficiency is controlled by controlling the opening of the valve corresponding to the compressed air. Specifically, the opening of the first control valve 35 is controlled according to the amount of high-temperature crude antimony liquid in the refining furnace 5, thereby controlling the flow rate of the compressed air.
[0062] In some preferred embodiments, the pressure of the compressed air can also be controlled to control the tumbling degree of the powdered impurity-removing agent in the high-temperature crude antimony liquid, thereby controlling the diffusion degree of the powdered impurity-removing agent in the high-temperature crude antimony liquid and further controlling the reaction efficiency of the impurity-removing agent.
[0063] As a preferred embodiment, the average particle size of the powdery impurity-removing agent is less than 3 mm;
[0064] In order to further illustrate the inventive concept of the present invention, the following is a comparative explanation of the reaction efficiency and impurity removal agent consumption of the antimony refining oxidation impurity removal method using the traditional impurity removal method and the antimony pyrometallurgical refining oxidation impurity removal method provided by the present invention in combination with the antimony refining oxidation impurity removal mechanism.
[0065] The antimony pyrorefining oxidation impurity removal described in the present invention refers to a process in which the impurity components are first oxidized and then react with the powdery impurity removal agent to generate scum which is removed;
[0066] The reaction mechanism of using soda ash to remove arsenic impurities is as follows:
[0067] As+2.5O2+3Na2CO3=2Na3AsO4+3CO2
[0068] 2As+1.5O2+3Na2CO3=2Na2AsO3+3CO2
[0069] The reaction mechanism of using monoammonium phosphate to remove lead impurities is as follows:
[0070] 2Pb+2NH4H2PO4+O2=Pb2P2O7+2NH3+3H2O
[0071] While the above reaction is taking place, the antimony liquid will also be oxidized by the air, and then react with the impurity removal agent to generate antimonate, forming scum and causing antimony loss. By utilizing the mechanism that impurities are more reactive, it is necessary to increase the contact between the impurities and the air and impurity removal agent. The present invention uses compressed air as a power to transport the impurity removal agent into the high-temperature crude antimony liquid, so that the impurities are in full contact with the air and the impurity removal agent, thereby achieving a good impurity removal effect.
[0072] Comparative Example 1:
[0073] In a 16m 2Refining furnace 5 produces No. 1 refined antimony. First, crude antimony oxygen is used to reduce and smelt 60 tons of crude antimony under the action of a reducing agent. The crude antimony contains 0.93% arsenic. Soda ash and flake caustic soda mixed alkali oxidation arsenic removal process is used. The traditional impurity removal method is adopted. A total of 9,500 kg of soda ash is added to the furnace top feed port in batches for 5 times, and finally 1,000 kg of flake caustic soda is added. The refining process takes 33 hours. After refining, the antimony contains 0.036% arsenic, and the output of qualified products is 53.3 tons. The produced arsenic alkali slag is 15.8 tons, containing 31.10% antimony and 3.47% arsenic.
[0074] Embodiment 21:
[0075] In the comparative example 1, the same 16m 2 Refined antimony No. 1 is produced in refining furnace 5; 60.5 tons of crude antimony are first smelted by oxygen reduction of crude antimony, and the crude antimony contains 0.95% arsenic. Similarly, the arsenic removal process is carried out by mixed alkali oxidation of soda ash and caustic soda flakes, and the antimony pyrometallurgical refining oxidation impurity removal method provided by the present invention is adopted. A total of 5500 kg of soda ash is added in 3 batches, and finally 1000 kg of caustic soda flakes are added. The refining process takes 20 hours. After refining, the antimony contains 0.032% arsenic, and the output of qualified products is 56.6 tons; 9.6 tons of arsenic alkali slag is produced, containing 26.30% antimony and 5.82% arsenic.
[0076] Comparative Example 2:
[0077] In a 16m 2 Ultra-pure refined antimony is produced in refining furnace 5. First, 60 tons of crude antimony are reduced and smelted under the action of a reducing agent using crude antimony oxide, and the crude antimony contains 0.33% lead. The lead removal process using monoammonium phosphate oxidation is adopted. The traditional impurity removal method is adopted. A total of 2,500 kg of monoammonium phosphate is added to the furnace top feed port at one time. The refining process takes 5 hours. After refining, the antimony contains 0.066% lead, and the output of qualified products is 53.3 tons. The produced lead slag is 3.5 tons, containing 32.30% antimony and 5.17% lead.
[0078] Embodiment 22:
[0079] The same 16m 2 Ultra-pure refined antimony is produced in the refining furnace 5; 60.5 tons of crude antimony is first smelted by oxygen reduction of crude antimony, and the crude antimony contains 0.35% lead. The arsenic removal process is carried out by oxidation of monoammonium phosphate, and the antimony pyrometallurgical refining oxidation and impurity removal method provided by the present invention is adopted. A total of 1500 kg of monoammonium phosphate is added, and the refining process takes 3.5 hours. After refining, the antimony contains 0.044% lead, and the output of qualified products is 56.6 tons; 2.3 tons of lead slag is produced, containing 25.50% antimony and 8.42% lead.
[0080] Table 1 is a comparison of the traditional impurity removal method and the impurity removal method provided by the present invention.
[0081]
[0082] As shown in Table 1, when using the soda ash and flake caustic soda mixed alkali oxidation removal process, under almost the same crude antimony weight, the antimony fire refining oxidation removal method provided by the present invention can greatly reduce the amount of soda ash (that is, the impurity removal agent), and the refining time is less, the weight of the obtained qualified product is larger, and the antimony content in the arsenic slag is lower (which means less antimony loss);
[0083] Using the same MAP oxidation arsenic removal process, under almost the same crude antimony weight, the antimony fire refining oxidation impurity removal method provided by the present invention can greatly reduce the amount of MAP (i.e., impurity removal agent), and take less time to refine, obtain a higher weight of qualified products, and have a lower antimony percentage in the lead slag (which means less antimony loss);
[0084] It is fully demonstrated that the antimony pyrorefining oxidation impurity removal method provided by the present invention can achieve good impurity removal effect compared with the traditional impurity removal method, regardless of whether it is a process of arsenic removal by oxidation using soda ash, mixed alkali flakes, or a process of arsenic removal by oxidation using monoammonium phosphate; it is further demonstrated that, under the action of compressed air, the powdered impurity removal agent is transported to the interior of the high-temperature antimony liquid, so that the powdered impurity removal agent can be quickly melted, and immediately, together with the compressed air, the impurities in the powdered impurity removal agent are quickly oxidized and react with the impurity removal agent, thereby improving the reaction efficiency and reducing the consumption of fuel and agents.
[0085] The above are only preferred embodiments of the present invention, and are not intended to limit the patent scope of the present invention. All equivalent structural changes made using the contents of the present invention's specification and drawings, or directly / indirectly applied in other related technical fields, are included in the patent protection scope of the present invention.
Claims
1. A powdered medicine dosing device, characterized in that: include: Medicine storage bin, used for storing powdered medicine; a discharge valve, disposed at the bottom of the medicine storage bin, for controlling the release of the powdered medicine therein; A metering tank is provided directly below the discharge valve, and is used to receive the powdered medicine released through the discharge valve and to weigh and measure the received powdered medicine; The metering tank is also provided with a medicine delivery pipe, and the end of the medicine delivery pipe is also provided with a high-temperature resistant medicine pipe for extending into the high-temperature molten metal to deliver the powdered medicine in the metering tank to the interior of the high-temperature molten metal; An air inlet pipe is provided at the bottom of the metering tank for connecting compressed air to provide power for conveying the powdered medicine.
2. A powdered medicine dosing device according to claim 1, characterized in that: The metering tank is provided with a metering module for weighing the powdered medicine dropped therein; The metering module is in communication with the discharge valve to control the opening and closing of the discharge valve.
3. A powdered medicine dosing device according to claim 1 or 2, characterized in that: The discharge valve is a star-shaped discharge valve.
4. A powdered medicine dosing device according to claim 1 or 2, characterized in that: The powdered medicine dosing device further includes an adjusting structure, which is arranged between the medicine delivery pipe and the high-temperature resistant medicine pipe so as to flexibly move the high-temperature resistant medicine pipe.
5. A powdered medicine dosing device according to claim 1 or 2, characterized in that: The air inlet pipe is provided with a first control valve for controlling the on / off and flow of compressed air.
6. A powdered medicine dosing device according to claim 1 or 2, characterized in that: The medicine delivery pipe is provided with a second control valve for controlling the on and off of powdered medicine delivery.
7. A method for fire refining, oxidation and impurity removal of metals, using a powdered reagent dosing device according to any one of claims 1 to 6, characterized in that: The steps include: S1. Sampling the high-temperature molten metal in the refining furnace to detect the impurity content in the crude molten metal; S2. Calculating the amount of impurities in the molten metal and the required amount of powdered impurity removal agent based on the obtained impurity content; S3. Setting the required dosage of the powdered impurity removal agent, releasing the powdered impurity removal agent from the agent storage bin into the metering tank and metering the agent; S4. Connect the air inlet pipe at the bottom of the metering tank to compressed air. Under the action of the compressed air, the powdered impurity-removing agent is sequentially transported through the agent delivery pipe and the high-temperature resistant agent pipe to the interior of the high-temperature molten metal for oxidation and impurity-removing reaction.
8. The method for fire refining, oxidation and impurity removal of metal according to claim 7, characterized in that: In step S4, the angle, position and / or depth of the high-temperature resistant agent tube extending into the high-temperature crude metal liquid is adjusted so that the impurity removal agent melts in the high-temperature metal liquid and fully oxidizes and reacts quickly with the impurities.
9. The method for fire refining, oxidation and impurity removal of metal according to claim 7 or 8, characterized in that: In step S4, the impurity removal efficiency is controlled by controlling the size of the opening of the valve corresponding to the compressed air and / or controlling the size of the compressed air pressure.
10. The method for fire refining, oxidation and impurity removal of metal according to claim 7 or 8, characterized in that: The average particle size of the powdery impurity-removing agent is less than 3 mm.