Cavern slag stone powder activity index test method
By curing hole slag stone powder specimens at 80±3°C in a heated curing box, combined with a standardized fineness screen, the problem of long detection time and uncertain fineness of hole slag stone powder in the prior art is solved, and the problem of long detection time and uncertain fineness of hole slag stone powder in the prior art is achieved. Fast and accurate activity index detection.
Patent Information
- Application Number
- CN202411188644.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-12-03
AI Technical Summary
The prior art cannot quickly, simply and accurately detect the activity index of cave slag and stone powder, resulting in lithologic changes in the tunnel excavation process affecting engineering applications, and the uncertainty of fineness increases the difficulty of detection.
The test cycle was shortened by the method of curing the heated curing box at 80±3°C for 24 hours. Combined with the standardized fineness screen to fix the particle size, the 28-day activity index of the hole slag stone powder was calculated by measuring the compressive strength of the test piece.
The detection time is significantly shortened from 28 days to 2 days, ensuring the detection accuracy, facilitating the rapid grasp of the activity indicators of cave slag powder on site, and fixing the particle distribution through standardized fineness, improving the reliability of the detection.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of mineral admixtures and relates to a method for testing the activity index of slag stone powder. Background Art
[0002] Mineral admixtures are an indispensable and important component of modern concrete. After being mixed with cement, sand, stone, water and admixtures in a certain proportion, concrete is formed after going through stages such as mixing, pouring, curing and hardening.
[0003] The role of mineral admixtures in concrete can be divided into three effects, namely, volcanic ash effect, micro-aggregate effect, and morphological effect. The volcanic ash effect refers to the active silicon oxide (SiO2) and active aluminum oxide (Al2O3) contained in the mineral admixtures. These components react with the alkaline hydration product Ca(OH)2 of cement to produce calcium silicate hydrate (CSH), calcium aluminate hydrate (CAH) and other hydraulic substances under the stimulation of cement, and fill the capillary pores to enhance the strength of concrete. The micro-aggregate effect refers to the fine particles in the mineral admixtures being evenly distributed in the base phase of the cement paste, just like fine aggregates, filling the gap between sand particles and cement particles, making the mortar system in the concrete more compact. The morphological effect refers to the smooth particles such as some glass beads contained in the mineral admixtures. These particles make the particles in the cement paste evenly dispersed, reduce the friction between the particles, and make the paste more fluid.
[0004] The development of mineral admixtures has gone through several stages. The first stage is the stage of single, traditional material types such as fly ash and mineral powder. The second stage is the stage of single, new materials such as various metallurgical solid waste powders (steel slag powder, gold / tungsten / copper tailings powder), rock powders of different lithology (limestone, granite, gneiss), etc. In the third stage, which is also the current stage, mineral admixtures are gradually moving towards composites based on a variety of new single materials, that is, new, composite materials mixed with two or more of the above materials. At present, traditional mineral admixtures such as fly ash and mineral powder are becoming increasingly difficult to obtain, but the slag from tunnel excavation in mountainous projects can be used to prepare rock powder, which is then used to prepare suitable raw materials for new composite mineral admixtures.
[0005] The performance of mineral admixtures has a significant impact on the performance of concrete, and its three major effects affect the final strength of concrete to varying degrees. Among the many properties of mineral admixtures, the most critical one is the activity performance, which is defined by the indicator of "activity index" in engineering applications. In the current standards, the test methods specified in different standards are consistent, such as Table C.1 of "Fly ash used in cement and concrete" (GB / T1596-2017) and Table A.1 of "Composite mineral admixtures for concrete" (JG / T486-2015). Both are formed according to GB / T17671 "Cement mortar strength test" test blocks, and the 28d compressive strength of the test mortar and the comparison mortar is measured under standard curing conditions of 20±1℃ and relative humidity above 90%, and the strength activity index of the mineral admixture is determined by the ratio of the two.
[0006] The above method is not suitable for slag powder for the following reasons: ① The test cycle is too long. In engineering, the strength results at the age of 28 days are generally used as the basis for material judgment. For tunnel slag powder, it is different from conventional fly ash, mineral powder and other materials. Its activity index fluctuates greatly due to the changes in rock properties during tunnel excavation, while the activity index of fly ash and mineral powder is relatively stable. This means that if the traditional method is used, it will take 28 days to know its activity index. During this process, the rock properties of the tunnel slag may have changed again, which has brought a great degree of interference to the application of tunnel slag powder admixtures in the project; ② The fineness of mineral admixtures has an important influence on their activity index. Generally speaking, the smaller the particle size, the greater the activity index. Therefore, the same material has different activity indexes at different finenesses. The fineness of materials such as fly ash and mineral powder is generally determined when they are produced at the factory and is fixed. However, the admixture of slag and stone powder is affected by its production method and is generally processed and produced directly at the project site, so the fineness is not clear.
[0007] Therefore, how to detect the activity index of slag stone powder more quickly, simply and accurately is of great significance. Summary of the invention
[0008] The invention provides a method for testing the activity index of slag stone powder, which can detect the activity index of slag stone powder more quickly, simply and accurately.
[0009] The technical solution of the present invention is achieved in this way: A method for testing the activity index of slag stone powder comprises the following steps: A. Sample Preparation The slag rock sample is crushed into particles, and ground to a fineness of ≥ 200 meshes to obtain a slag rock powder sample; B. Specimen Forming The reference group mortar and the experimental group mortar were prepared and the test blocks were formed according to GB / T 17671 "Test Method for Strength of Cement Mortar". The test pieces were made by using a vibrating table, and then the molds were removed after curing in a standard curing box for 24 hours to obtain the reference group test pieces and the experimental group test pieces. The reference group mortar is composed of cement, Chinese ISO standard sand and water in a mass ratio of 450±2:1350±5:225±1, and the experimental group mortar is composed of cement, slag stone powder, Chinese ISO standard sand and water in a mass ratio of 315±1:135±1:1350±5:225±1; C. Heating and curing The demoulding test piece is immediately placed in a heating and curing box, in which a heating device and water are provided. The water temperature in the water tank is stabilized at 80±3°C, and the water temperature difference at each position inside the entire box does not exceed 2°C. The distance between the test pieces is ≥5cm, the distance from the heating device and the inner wall of the box is ≥5cm, and the distance from the top of the test piece to the water liquid surface is also ≥5cm. Curing in the heating and curing box for 24h±1h; wherein the tap water can also be distilled water; the distance between the test pieces is set to be ≥5cm, the distance from the test piece to the heating device and the inner wall of the box is ≥5cm, and the distance from the top of the test piece to the water liquid surface is also ≥5cm, this is to ensure uniform temperature distribution, wherein there is a temperature gradient near the edge of the heating box, resulting in unevenness, and then resulting in inaccurate rapid detection results; and 80±3°C is the key to the detection method of the present invention. If the temperature is high, although the curing time is shortened, there is a potential destructive effect on the test block, which affects the strength development. If the temperature is low, the heating and curing time will be extended, and the purpose of rapid detection cannot be achieved.
[0010] D. Calculate the activity index After heating and curing, the specimens were taken out, and the compressive strength of the reference group specimens and the experimental group specimens were measured according to GB / T 17671 "Test Method for Strength of Cement Mortar". The predicted 28-day activity index of the slag stone powder was calculated by the formula as follows: In the formula, Ap——predicted activity index of slag powder in 28 days, %; Ra,o——compressive strength of test specimens in the experimental group, in MPa; Ra,t – compressive strength of benchmark specimens, in MPa.
[0011] Furthermore, the particle size of the particles is below 7 mm.
[0012] Furthermore, the grinding speed is 48r / min and the grinding time is 30min.
[0013] Furthermore, the reference group mortar is composed of cement, Chinese ISO standard sand and water in a mass ratio of 450:1350:225, and the experimental group mortar is composed of cement, slag stone powder, Chinese ISO standard sand and water in a mass ratio of 315:135:1350:225.
[0014] Furthermore, the preparation method of the reference group mortar includes: adding water into a mortar mixing pot, adding reference cement, placing the mortar mixing pot on a fixed bracket, and shaking the handle to raise it to a fixed position; starting the cement mortar mixer, stirring at a rate of 140±1r / min for 30 seconds, and then putting Chinese ISO standard sand into the cement mortar mixing pot, first stirring at a rate of 285±1r / min for 15 seconds, using a rubber scraper to scrape the mortar on the blades and the wall of the mixing pot into the pot, and then stirring at a rate of 285±1r / min for 15 seconds; stopping stirring for 90 seconds, and then stirring at a rate of 285±1r / min for 60 seconds; completing the production of the test piece by using a vibration compaction table, and removing the mold after curing in a standard curing box for 24 hours.
[0015] Furthermore, the preparation method of the experimental group mortar includes: adding water into the mortar mixing pot, adding reference cement and slag stone powder, placing the mortar mixing pot on a fixed bracket, and shaking the handle to raise it to a fixed position; starting the cement mortar mixer, stirring at a rate of 140±1r / min for 30 seconds, and then putting Chinese ISO standard sand into the cement mortar mixing pot, first stirring at a rate of 285±1r / min for 15 seconds, using a rubber scraper to scrape the mortar on the blades and the wall of the mixing pot into the pot, and then stirring at a rate of 285±1r / min for 15 seconds; stopping stirring for 90 seconds, and then stirring at a rate of 285±1r / min for 60 seconds; completing the production of the test piece by using a vibration compaction table, and removing the mold after curing in a standard curing box for 24 hours.
[0016] The working principle and beneficial effects of the present invention are: 1. The present invention accelerates the secondary hydration reaction of cement hydration products and mineral admixtures by heating and curing, shortening the curing age to 2 days. Compared with the technical solutions specified in the existing standards, the present invention has the advantages of saving test time and greatly shortening the test cycle from 28 days to 2 days, while ensuring a high degree of accuracy. It is convenient for on-site technicians to quickly and easily grasp the activity index of slag stone powder.
[0017] 2. The present invention adopts a fixed-size screen to fix the fineness of the stone powder within a certain range and standardize it. DETAILED DESCRIPTION
[0018] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0019] Example 1 A method for testing the activity index of slag stone powder comprises the following steps: A. Sample Preparation Collect a cave slag rock sample with a mass of ≥10kg and a clean surface without soil adhesion. Use hammer, small jaw crusher and other tools to crush the cave slag rock sample into particles with a particle size of less than 7mm. Weigh 5kg of the above-mentioned granular material and put it into a Φ500×500 standard cement test mill for grinding. Grind it at a grinding speed of 48r / min, grinding time of 30min, grinding body loading of 100KG, and then pass it through a 325-mesh sieve. Take out and collect the material under the sieve to obtain a cave slag stone powder sample; the most economical production fineness for on-site production is 325 mesh, so the powder fineness is controlled at 325 mesh in this embodiment; B. Specimen Forming According to GB / T 17671 "Test Method for Strength of Cement Mortar", the reference group mortar and the experimental group mortar were prepared, with 3 pieces in each group. The test pieces were formed by a vibrating table, and the molds were removed after curing in a standard curing box for 24 hours to obtain the reference group test pieces and the experimental group test pieces. The reference group mortar was composed of cement, Chinese ISO standard sand and water in a mass ratio of 450:1350:225, and the experimental group mortar was composed of cement, slag stone powder, Chinese ISO standard sand and water in a mass ratio of 315:135:1350:225. That is, the preparation method of the reference group mortar includes: adding water into a mortar mixing pot, adding reference cement, placing the mortar mixing pot on a fixed bracket, and shaking the handle to raise it to a fixed position; starting the cement mortar mixer, stirring at a rate of 140r / min for 30 seconds, and then adding Chinese ISO standard sand into the cement mortar mixing pot, stirring at a rate of 285r / min for 15 seconds, scraping the mortar on the blades and the wall of the mixing pot into the pot with a rubber scraper, and then stirring at a rate of 285r / min for 15 seconds; stopping stirring for 90 seconds, and then stirring at a rate of 285r / min for 60 seconds; completing the production of the test piece by using a vibration compaction table, and removing the mold after curing in a standard curing box for 24 hours; The preparation method of the experimental group mortar includes: adding water into a mortar mixing pot, adding reference cement and slag stone powder, placing the mortar mixing pot on a fixed bracket, and shaking the handle to raise it to a fixed position; starting the cement mortar mixer, stirring at a rate of 140r / min for 30 seconds, and then adding Chinese ISO standard sand into the cement mortar mixing pot, stirring at a rate of 285r / min for 15 seconds, scraping the mortar on the blades and the wall of the mixing pot into the pot with a rubber scraper, and then stirring at a rate of 285r / min for 15 seconds; stopping stirring for 90 seconds, and then stirring at a rate of 285r / min for 60 seconds; completing the production of the test piece by using a vibration compaction table, and removing the mold after curing in a standard curing box for 24 hours; C. Heating and curing After demoulding, the specimens are immediately placed in a heating and curing box with a size of ≥40cm*30cm*40cm. The heating and curing box is equipped with a heating device and tap water. The specimens are completely immersed in water. The water temperature in the water tank is stabilized at 80°C, and the water temperature difference at various positions inside the entire box does not exceed 2°C. The distance between the specimens is 8cm, the distance from the heating device and the inner wall of the box is 8cm, and the distance from the top of the specimen to the water surface is also 8cm. Curing in the heating and curing box for 24 hours; D. Calculate the activity index After heating and curing, the specimens were taken out, and the compressive strength of the reference group specimens and the experimental group specimens were measured according to GB / T 17671 "Test Method for Strength of Cement Mortar". The predicted 28-day activity index of the slag stone powder was calculated by the formula as follows: In the formula, Ap——predicted activity index of slag powder in 28 days, %; Ra,o——compressive strength of test specimens in the experimental group, in MPa; Ra,t – compressive strength of benchmark specimens, in MPa.
[0020] Comparative Example 1 (Current Standard Test Method) A. Sample Preparation Collect a piece of slag rock sample with a mass of ≥10kg and a clean surface without soil. Use hammer, small jaw crusher and other tools to crush the slag rock sample into particles with a particle size of less than 7mm. Weigh 5kg of the above-mentioned granular material and put it into a Φ500×500 standard cement test mill for grinding. Grind it at a grinding speed of 48r / min, grinding time of 30min, grinding body loading of 100KG, and then pass it through a 325-mesh sieve. Take out and collect the material under the sieve to obtain the slag stone powder sample; B. Specimen Forming According to GB / T 17671 "Test Method for Strength of Cement Mortar", the reference group mortar and the experimental group mortar were prepared, with 3 pieces in each group. The test pieces were formed by a vibrating table, and the molds were removed after curing in a standard curing box for 24 hours to obtain the reference group test pieces and the experimental group test pieces. The reference group mortar was composed of cement, Chinese ISO standard sand and water in a mass ratio of 450:1350:225, and the experimental group mortar was composed of cement, slag stone powder, Chinese ISO standard sand and water in a mass ratio of 315:135:1350:225. That is, the preparation method of the reference group mortar includes: adding water into a mortar mixing pot, adding reference cement, placing the mortar mixing pot on a fixed bracket, and shaking the handle to raise it to a fixed position; starting the cement mortar mixer, stirring at a rate of 140r / min for 30 seconds, and then adding Chinese ISO standard sand into the cement mortar mixing pot, stirring at a rate of 285r / min for 15 seconds, scraping the mortar on the blades and the wall of the mixing pot into the pot with a rubber scraper, and then stirring at a rate of 285r / min for 15 seconds; stopping stirring for 90 seconds, and then stirring at a rate of 285r / min for 60 seconds; completing the production of the test piece by using a vibration compaction table, and removing the mold after curing in a standard curing box for 24 hours; The preparation method of the experimental group mortar includes: adding water into a mortar mixing pot, adding reference cement and slag stone powder, placing the mortar mixing pot on a fixed bracket, and shaking the handle to raise it to a fixed position; starting the cement mortar mixer, stirring at a rate of 140r / min for 30 seconds, and then adding Chinese ISO standard sand into the cement mortar mixing pot, stirring at a rate of 285r / min for 15 seconds, scraping the mortar on the blades and the wall of the mixing pot into the pot with a rubber scraper, and then stirring at a rate of 285r / min for 15 seconds; stopping stirring for 90 seconds, and then stirring at a rate of 285r / min for 60 seconds; completing the production of the test piece by using a vibration compaction table, and removing the mold after curing in a standard curing box for 24 hours; C. Water maintenance After demoulding, the specimens shall be immediately placed horizontally in water at 20℃±1℃ for curing for 28 days. When placed horizontally, the scraped surface shall face upwards. The relative humidity of the curing box shall not be less than 90%. The specimens shall be placed on a non-perishable grate and kept at a certain distance from each other so that water can contact the six surfaces of the specimens. During the curing period, the distance between the specimens or the water depth on the upper surface of the specimens shall not be less than 5mm; D. Calculate the activity index After heating and curing, the specimens were taken out, and the compressive strength of the reference group specimens and the experimental group specimens were measured according to GB / T 17671 "Test Method for Strength of Cement Mortar". The 28-day activity index of the slag stone powder was calculated by the formula as follows: In the formula, Ap——28-day activity index of slag powder, %; Ro——compressive strength of the benchmark specimens, in MPa; Rt is the compressive strength of the test specimens in the experimental group, in MPa.
[0021] The results of the test methods of Example 1 and Comparative Example 1 are shown in Table 1 below.
[0022] Table 1 Comparative Example 2 Compared with Example 1, the only difference is the heating and curing step C, and the specific steps are as follows: The demoulding specimens are immediately placed in a heating and curing box with a size of ≥40cm*30cm*40cm. The heating and curing box is equipped with a heating device and tap water. The water temperature in the water tank is stabilized at 80°C, and the water temperature difference at various positions inside the entire box does not exceed 2°C. The specimens are 3cm apart, 3cm away from the heating device and the inner wall of the box, and 3cm away from the top of the specimen to the water surface. Cured in the heating and curing box for 24 hours.
[0023] Comparing this comparative example with the current standard test method, the absolute value of the error between the predicted and standard activity index is 3.2-8.5%.
[0024] Comparative Example 3 Compared with Example 1, the only difference is the heating and curing step C, and the specific steps are as follows: The demoulding specimens are immediately placed in a heating and curing box with a size of ≥40cm*30cm*40cm. The heating and curing box is equipped with a heating device and tap water. The water temperature in the water tank is stabilized at 90°C, and the water temperature difference at various positions inside the entire box does not exceed 2°C. The specimens are 8cm apart, 8cm away from the heating device and the inner wall of the box, and 8cm away from the top of the specimen to the water surface. Cured in the heating and curing box for 24 hours.
[0025] Comparing this comparative example with the current standard test method, the absolute value of the error between the predicted and standard activity index is 4.7-10.1%.
[0026] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for testing the activity index of slag powder, characterized in that: The steps include: A. Sample Preparation The slag rock sample is crushed into particles, and ground to a fineness of ≥ 200 meshes to obtain a slag rock powder sample; B. Specimen Forming The reference group mortar and the experimental group mortar were prepared and the test blocks were formed according to GB / T 17671 "Test Method for Cement Mortar Strength". The test pieces were made by using a vibrating table, and then the molds were removed after curing in a standard curing box for 24 hours to obtain the reference group test pieces and the experimental group test pieces. The reference group mortar is composed of cement, Chinese ISO standard sand and water in a mass ratio of 450±2:1350±5:225±1, and the experimental group mortar is composed of cement, slag stone powder, Chinese ISO standard sand and water in a mass ratio of 315±1:135±1:1350±5:225±1; C. Heating and curing The demoulded specimens are immediately placed in a heating and curing box, which is equipped with a heating device and water. The water temperature in the water tank is stabilized at 80±3℃, and the water temperature difference at various positions inside the entire box is no more than 2℃. The distance between the specimens is ≥5cm, the distance from the heating device and the inner wall of the box is ≥5cm, and the distance from the top of the specimen to the water surface is ≥5cm. Cured in the heating and curing box for 24h±1h; D. Calculate the activity index After heating and curing, the specimens were taken out, and the compressive strength of the reference group specimens and the experimental group specimens were measured according to GB / T 17671 "Test Method for Strength of Cement Mortar". The predicted 28-day activity index of the slag stone powder was calculated by the formula as follows: In the formula, A p ——Predicted activity index of slag powder in 28 days, %; R a,o ——compressive strength of test specimens in the experimental group, in MPa; R a,t ——Compressive strength of benchmark specimens, in MPa.
2. A method for testing the activity index of slag powder according to claim 1, characterized in that: The particle size of the particles is below 7 mm.
3. A method for testing the activity index of slag powder according to claim 1, characterized in that: The rotation speed of the grinding mill is 48 r / min, and the grinding time is 30 min.
4. A method for testing the activity index of slag powder according to claim 1, characterized in that: The reference group mortar is composed of cement, Chinese ISO standard sand and water in a mass ratio of 450:1350:225, and the experimental group mortar is composed of cement, slag stone powder, Chinese ISO standard sand and water in a mass ratio of 315:135:1350:
225.
5. A method for testing the activity index of slag powder according to claim 1, characterized in that: The preparation method of the reference group mortar includes: adding water into a mortar mixing pot, adding reference cement, placing the mortar mixing pot on a fixed bracket, and shaking the handle to raise it to a fixed position; starting the cement mortar mixer, stirring at a rate of 140±1r / min for 30 seconds, and then putting Chinese ISO standard sand into the cement mortar mixing pot, first stirring at a rate of 285±1r / min for 15 seconds, scraping the mortar on the blades and the wall of the mixing pot into the pot with a rubber scraper, and then stirring at a rate of 285±1r / min for 15 seconds; stopping stirring for 90 seconds, and then stirring at a rate of 285±1r / min for 60 seconds; completing the production of the test piece by using a vibration compaction table, and removing the mold after curing in a standard curing box for 24 hours.
6. A method for testing the activity index of slag powder according to claim 1, characterized in that: The preparation method of the experimental group mortar includes: adding water into a mortar mixing pot, adding reference cement and slag stone powder, placing the mortar mixing pot on a fixed bracket, and shaking the handle to raise it to a fixed position; starting the cement mortar mixer, stirring at a rate of 140±1r / min for 30 seconds, and then putting Chinese ISO standard sand into the cement mortar mixing pot, first stirring at a rate of 285±1r / min for 15 seconds, scraping the mortar on the blades and the wall of the mixing pot into the pot with a rubber scraper, and then stirring at a rate of 285±1r / min for 15 seconds; stopping stirring for 90 seconds, and then stirring at a rate of 285±1r / min for 60 seconds; completing the production of the test piece by using a vibration compaction table, and removing the mold after curing in a standard curing box for 24 hours.
Citation Information
Cited By
Waste glass activity rapid comprehensive evaluation method based on dissolution kinetics analysis
CN119780070A