Photoresist composition and application thereof

Through the photoresist composition composed of phenolic resin and specific adhesion enhancer, the existing photoresist's shortcomings in resolution, adhesion and cost are solved, and an efficient semiconductor chip manufacturing process is achieved, providing high-quality Resolution, strong adhesion and good peeling properties are suitable for thick coating processes and reduce production costs.

CN119065202APending Publication Date: 2024-12-03TIANJIN JIURI SEMICON MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411427700.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-14
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Existing positive and negative photoresist have problems such as insufficient resolution, poor adhesion, high cost and poor peeling performance in semiconductor and display panel manufacturing, especially in thick coating processes, production efficiency and cost are difficult to meet. need.

Method used

The photoresist composition consisting of phenolic resin, photoacid generator, melamine resin containing ether bonds, hydroxypyridone, etc., is used to generate acid substances through light to form a three-dimensional network structure of polymer, enhance adhesion and peeling ability. The light source is exposed to the g/i-linewidth spectrum without the need for photosensitizers, and can work efficiently in commonly used developer and peeling liquid.

Benefits of technology

It realizes high resolution, high photosensitiveness and excellent etching resistance, simplifies the process flow, reduces production costs, and is suitable for etching of 3-10 micron thick aluminum, copper or its alloy film and silica insulating layer. The process significantly improves production efficiency and product quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119065202A_ABST
    Figure CN119065202A_ABST
Patent Text Reader

Abstract

The invention relates to a photoresist composition and application thereof. The photoresist composition comprises the following components: phenolic resin, a photoacid generator, an adhesion enhancer and a solvent, the adhesion enhancer comprises melamine resin containing ether bonds and / or hydroxypyridone. The photoresist composition does not need to use a photosensitizer and has the characteristics of short exposure time and strong adhesion, a g / i-line and g, h and i-wide spectrum exposure light source can be adopted, a formed coating has the advantages of high resolution, high photosensitivity, excellent etching resistance and the like, a common stripping liquid can be adopted for photoresist removal, and the stripping capability is strong; the photoresist composition has the advantages and characteristics of various negative photoresists, overcomes the defects of the existing negative photoresists, is convenient to use and can be applied to semiconductors. The embodiment of the invention also provides application of the photoresist composition in a semiconductor, and the thickness of a coating of the photoresist composition in the semiconductor is 3-10 microns.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of semiconductor technology, in particular to a photoresist composition and application thereof, and particularly to a negative photoresist composition and application thereof. Background Art

[0002] Photoresist, also known as photoresist, can be divided into positive photoresist and negative photoresist according to its different photoreaction properties. The solubility of the part of positive photoresist exposed to ultraviolet light changes and dissolves in the developer, while the part not exposed to light remains on the substrate to form a pattern; negative photoresist is just the opposite. The part exposed to light does not dissolve in the developer and remains on the substrate, while the part not exposed to light dissolves in the developer, thus forming a pattern.

[0003] Positive photoresist has excellent resolution, good adhesion to metal substrates, excellent etching resistance, and good pattern uniformity, so it is widely used in semiconductor and flat panel display manufacturing processes. Its use process includes the following steps: first, the glue is coated on a silicon wafer or glass substrate, and then a hot plate is used to perform soft baking in a temperature range of 90 to 110°C to remove the organic solvent contained therein, and then an exposure device is used for exposure. After exposure, a hot plate is used for heat baking again to eliminate the standing wave effect generated during the exposure process (this heat baking is called post-exposure baking, referred to as PEB). Finally, it is developed with a 2.38% concentration of tetramethylammonium hydroxide solution to complete the production of the desired pattern on the substrate. However, positive photoresist also has obvious limitations and is difficult to be used in thick coating processes in semiconductor and display panel manufacturing, because as the thickness of the glue layer increases, the required exposure amount will increase significantly, thereby significantly reducing production efficiency.

[0004] One of the main reasons for using negative photoresist in semiconductor manufacturing is that in process layers with obvious step differences, thick-coated photoresist with a layer thickness of more than 5μm must be used. At this thickness, if positive photoresist is used, the exposure time needs to be significantly extended, resulting in a significant reduction in productivity; at the same time, from the perspective of photoresist cost, thick-coated photoresist needs to have high viscosity and high solid content, and more expensive photosensitizers need to be used, which will also cause the cost of using thick-coated positive photoresist to increase rapidly.

[0005] The most commonly used negative photoresist is usually composed of a photoinitiator, a multifunctional monomer and an acrylic resin, and is mainly used in RGB color glue or OC glue in flat panel display manufacturing. However, this type of negative photoresist cannot be used in semiconductor and flat panel display manufacturing processes that use wet etching because acrylic resin has poor adhesion to metal substrates. In addition, this type of negative photoresist usually uses a 0.4% KOH solution as a developer, rather than the 2.38% tetramethylammonium hydroxide solution commonly used in positive photoresists. The most important point is that this type of negative photoresist has poor resolution and is not suitable for use in semiconductor manufacturing processes that require high resolution.

[0006] Another type of negative photoresist is cyclized rubber, which has excellent adhesion and can be used in wet etching processes with a film thickness of more than 2 microns in semiconductor manufacturing processes, and the etching time can exceed 10 minutes. However, cyclized rubber negative photoresists also have the following shortcomings: first, only organic solvents can be used as developers, and the 2.38% tetramethylammonium hydroxide developer commonly used in positive photoresists cannot be used; second, the stripping performance of this type of negative photoresist is poor, and defects often occur when using organic solvent strippers; in addition, cyclized rubber negative photoresists use phenol and xylenol substances that are toxic and harmful to the human body as solvents, so it is difficult to apply to large-scale semiconductor production lines.

[0007] Another type of negative photoresist is phenolic resin negative photoresist. Chemically amplified photoresist often refers to photoresist with ultra-high resolution, which is used in semiconductor chip manufacturing processes with photolithography accuracy higher than 250nm, and is not used in flat panel display manufacturing processes. In the semiconductor chip manufacturing process, the exposure light source uses a deep ultraviolet light source with a wavelength of 248nm, 193nm and 157nm. Phenolic resin and resorcinol polymer have obvious absorption of deep ultraviolet light, so they cannot be used as film-forming materials for this type of chemically amplified photoresist in the prior art.

[0008] Therefore, it is very important to develop a photoresist composition that can overcome the above-mentioned defects. Summary of the invention

[0009] In view of the deficiencies in the prior art, the purpose of the present invention is to provide a photoresist composition and its application. The photoresist composition does not require the use of a photosensitizer, has the characteristics of short exposure time and strong adhesion, can use g / i-line and g,h,i-wide spectrum exposure light sources, and the formed coating has the advantages of high resolution, high sensitivity and excellent etching resistance, and can be removed by ordinary stripping liquid, with strong stripping ability; the photoresist composition has the advantages and characteristics of various negative photoresists, while improving the deficiencies of existing negative photoresists, is easy to use, can be applied to semiconductor chip manufacturing processes, and is suitable for the etching process of 3-10 micron thick aluminum, copper or their alloy films and silicon dioxide insulating layers.

[0010] To achieve this object, the present invention adopts the following technical solutions:

[0011] In a first aspect, the present invention provides a photoresist composition, comprising the following components: a phenolic resin, a photoacid generator, an adhesion enhancer and a solvent; the adhesion enhancer comprises a melamine resin containing an ether bond and / or hydroxypyridone.

[0012] Preferably, the structural formula of the melamine resin containing an ether bond is as shown in Formula I:

[0013]

[0014] Wherein, R1, R2, R3, R4, R5, and R6 are each independently selected from any one of hydrogen, hydroxy, substituted or unsubstituted C1-C20 (e.g., C2, C4, C6, C8, C10, C12, C14, C16, C18, etc.) alkyl, and substituted or unsubstituted C1-C20 (e.g., C2, C4, C6, C8, C10, C12, C14, C16, C18, etc.) alkoxy, and R1, R2, R3, R 4. At least one (for example, 2, 3, 4, 5, 6, etc.) of R5 and R6 is selected from substituted or unsubstituted ether groups; when the above groups have substituents, the substituents include hydroxyl, C1-C20 (for example, C2, C4, C6, C8, C10, C12, C14, C16, C18, etc.) alkyl, C1-C20 (for example, C2, C4, C6, C8, C10, C12, C14, C16, C18, etc.) alkoxy.

[0015] In the present invention, C2~C20 ether groups represent that the number of main chain carbon atoms is 2 to 20 (for example, 2, 4, 6, 8, 10, 12, 14, 16, 18, etc.). The number of ether groups is not limited to 1, and can be 1 or more, such as 2, 4, 6, 8, etc., and the same applies to other similar expressions.

[0016] In the present invention, the photoresist composition uses phenolic resin as the main resin, is matched with a photoacid generator and an adhesion enhancer of a specific structure, has the advantages and characteristics of multiple negative photoresists, and improves the shortcomings of existing negative photoresists. The photoresist composition belongs to a chemically amplified photoresist, and its resolution reaches or even exceeds the level of positive photoresists, and meets the requirements of thick coating lithography technology. In addition, unlike the existing cyclized rubber negative photoresist, the photoresist composition of the present invention can adopt the same developer, stripper and process as the existing positive photoresist, so it is very suitable for application in large-scale production lines.

[0017] Specifically, in the present invention, during the process of forming the coating layer of the photoresist composition, the photoacid generator generates an acidic substance after being illuminated, and the adhesion enhancer and the phenolic resin can quickly form a polymer three-dimensional network structure under the catalysis of the acidic substance. A chelate bond can be formed between the adhesion enhancer and the oxide on the surface of the coating, thereby enhancing the bonding force between the photoresist composition and the coating. Among them, hydroxypyridone has a strong absorption of ultraviolet light and a high molar extinction coefficient, which can reduce the exposure time of the photoresist and increase sensitivity. At the same time, hydroxypyridone is a small molecule substance, and an appropriate amount of addition can improve the stripping ability of the photoresist composition in a general stripping solution. Further, in the present invention, the three-dimensional network structure formed by the melamine resin, hydroxypyridone and phenolic resin containing an ether bond is more dense, which improves the strong acid etching resistance and hydrofluoric acid penetration resistance of the coating formed by the photoresist composition.

[0018] In summary, the photoresist composition of the present invention has the characteristics of short exposure time and strong adhesion, and the formed coating has good etching resistance and strong stripping ability. The photoresist composition, as a chemically amplified photoresist, is different from the chemically amplified photoresist with a photolithography accuracy higher than 250nm in the semiconductor chip manufacturing process. It can be applied to the semiconductor chip and flat panel display manufacturing process, and adopts g / i-line and g,h,i-wide spectrum exposure light source, and has the advantages of high resolution, high sensitivity and excellent etching resistance. In addition, ordinary stripping liquid can be used for degumming, and it is easy to use and can be applied to the semiconductor chip manufacturing process. It is suitable for the etching process of 3-10 micron thick aluminum, copper or its alloy film and silicon dioxide insulating layer.

[0019] In the present invention, C1-C20 refers to the number of main chain carbon atoms being 1-20, such as 2, 4, 6, 8, 10, 12, 14, 16, 18, etc., and other similar expressions are the same.

[0020] Preferably, the photoresist composition does not include a photosensitizer.

[0021] In the present invention, the photoresist composition does not need to use expensive photosensitizers, and can still achieve excellent comprehensive performance, thereby reducing production costs.

[0022] Preferably, the number of ether groups in the melamine resin containing ether bonds is 2-6, for example, 3, 4, 5, 6, etc.

[0023] Preferably, the structural formula of the melamine resin containing ether bonds is as follows:

[0024]

[0025] Preferably, the structural formula of hydroxypyridone is as shown in Formula II:

[0026]

[0027] Among them, R7, R8, R9, R 10 Each of R7, R8, R9, R 10 At least one (for example, 2, 3, 4, etc.) contains a hydroxyl group; when the above groups have substituents, the substituents include hydroxyl, C1-C20 (for example, C2, C4, C6, C8, C10, C12, C14, C16, C18, etc.) alkyl, C1-C20 (for example, C2, C4, C6, C8, C10, C12, C14, C16, C18, etc.) alkoxy.

[0028] Preferably, the number of hydroxyl groups in the hydroxypyridone is 1-4, such as 2, 3, 4, etc.

[0029] Preferably, the structural formula of hydroxypyridone is as follows:

[0030]

[0031] Preferably, based on the total solid content of the photoresist composition as 100%, the amount of melamine resin containing ether bonds added is 2%-40%, for example 5%, 10%, 15%, 20%, 25%, 30%, 35%, etc.; the amount of hydroxypyridone added is 0.1%-10%, for example 0.5%, 1%, 2%, 4%, 6%, 8%, etc.; the amount of phenolic resin added is 55%-95%, for example 60%, 65%, 70%, 75%, 80%, 85%, 90%, etc.; the amount of photoacid generator added is 0.001%-5%, for example 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 33%, .5%, 4%, 4.5%, etc., and further preferably 0.1%-0.5%.

[0032] Preferably, the mass ratio of the melamine resin containing an ether bond to the hydroxypyridone is (0.1-100):1, wherein 0.1-100 can be 0.5, 1, 5, 10, 20, 30, 40, 50, 60, 70, 80, 90, etc., and further preferably (1-20):1, wherein 1-20 can be 2, 4, 6, 8, 10, 12, 14, 16, 18, etc.

[0033] In the present invention, the mass ratio of the melamine resin containing ether bonds and the hydroxypyridone is within the preferred range because at this ratio, the excess melamine resin containing ether bonds and the hydroxypyridone form a three-dimensional network structure, which can fill the gaps generated in the negative photoresist during the cross-linking process, thereby improving the overall etching resistance of the photoresist; if the mass ratio of the two is too high, the melamine resin will react preferentially with the hydroxypyridone, thereby causing the negative photoresist to be unable to form an image as a whole; if the mass ratio of the two is too low, the three-dimensional network structure that plays an anti-corrosion role cannot be formed.

[0034] Preferably, based on the total mass of the phenolic resin as 100%, the total mass of the melamine resin containing ether bonds and the hydroxypyridone is 0.1%-100%, for example, 0.5%, 1%, 5%, 10%, 20%, 30%, 40%, 50%, 60%, 70%, 80%, 90%, etc., and further preferably 5%-50% (for example, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, etc.).

[0035] In the present invention, based on the total mass of the phenolic resin as 100%, the total mass of the melamine resin containing ether bonds and the hydroxypyridone is within the preferred range because the negative photoresist within this range can form a stable and reliable morphology; if the mass of the two is too high, the negative photoresist requires high energy to cross-link to form a pattern, resulting in a decrease in production efficiency; if the mass of the two is too low, the negative photoresist will have insufficient etching resistance.

[0036] Preferably, the phenolic resin comprises any one of m-cresol phenolic resin, p-cresol phenolic resin, m-cresol-p-cresol copolymer phenolic resin, xylenol-cresol copolymer phenolic resin or tricresol-cresol copolymer phenolic resin or a combination of at least two thereof, wherein a typical but non-limiting combination comprises: a combination of m-cresol phenolic resin and p-cresol phenolic resin, a combination of m-cresol-p-cresol copolymer phenolic resin, xylenol-cresol copolymer phenolic resin and tricresol-cresol copolymer phenolic resin , a combination of p-cresol phenolic resin, m-cresol-p-cresol copolymer phenolic resin, xylenol-cresol copolymer phenolic resin and trimethylol-cresol copolymer phenolic resin, etc., further preferably a combination of m-cresol phenolic resin and p-cresol phenolic resin, further preferably a combination of m-cresol phenolic resin and p-cresol phenolic resin in a mass ratio of (0.2-2): 1, wherein 0.2-2 can be 0.4, 0.6, 0.8, 1, 1.2, 1.4, 1.6, 1.8, etc.

[0037] Preferably, the weight average molecular weight of the phenolic resin is 1000-60000, for example, 5000, 10000, 15000, 20000, 25000, 30000, 35000, 40000, 45000, 50000, 55000, etc., more preferably 8000-20000.

[0038] Preferably, the dissolution rate of the phenolic resin in a tetramethylammonium hydroxide aqueous solution having a mass concentration of 2% to 3% (e.g., 2.2%, 2.4%, 2.6%, 2.8%, etc., more preferably 2.38%) is For example etc., further preferred

[0039] Preferably, the photoacid generator includes any one or a combination of at least two of the compounds shown in the following structures:

[0040]

[0041] Among them, n-Bu is n-butyl, Ph is phenyl, and the wavy line represents that the benzene ring is a cis or trans structure.

[0042] In the present invention, based on the total solid content of the photoresist composition as 100%, the added amount of the photoacid generator is within the preferred range of 0.1%-0.5%; if the added amount is too high, the negative photoresist will be unstable and easily affected by temperature, and the size of the formed pattern will fluctuate greatly; if the added amount is too low, the required exposure energy will be too large, affecting production efficiency.

[0043] Preferably, the solvent includes any one of propylene glycol monomethyl ether acetate, propylene glycol monomethyl ether, benzyl alcohol, n-butyl acetate, methyl methoxypropionate, ethyl lactate, ethyl ethoxypropionate or diethylene glycol methyl ethyl ether, or a combination of at least two of them, wherein typical but non-limiting combinations include: a combination of propylene glycol monomethyl ether acetate and propylene glycol monomethyl ether, a combination of benzyl alcohol, n-butyl acetate and methyl methoxypropionate, a combination of methyl methoxypropionate, ethyl lactate, ethyl ethoxypropionate and diethylene glycol methyl ethyl ether, and the like.

[0044] Preferably, the photoresist composition further comprises other additives.

[0045] Preferably, the other additives include an alkaline neutralizer and / or a surfactant.

[0046] Preferably, the alkaline neutralizer includes any one or a combination of at least two of N,N-bis(2-hydroxyethyl)pivalic acid amide, N,N-dimethylacetamide, N1,N1,N3,N3-tetrabutylmaleamide, pyridine, N-tert-butylethanolamine, 2-(dibutylamino)ethanol, 2-aminoethanol, 1-pyrrolidonecarboxylic acid tert-butyl ester, 2-ethyl-1H-imidazole-1-carboxylic acid tert-butyl ester or triethylamine, wherein typical but non-limiting combinations include: a combination of N,N-bis(2-hydroxyethyl)pivalic acid amide and N,N-dimethylacetamide, a combination of N1,N1,N3,N3-tetrabutylmaleamide, pyridine and N-tert-butylethanolamine, a combination of 2-(dibutylamino)ethanol, 2-aminoethanol, 1-pyrrolidonecarboxylic acid tert-butyl ester, 2-ethyl-1H-imidazole-1-carboxylic acid tert-butyl ester and triethylamine, etc.

[0047] Preferably, based on the total solid content of the photoresist composition as 100%, the added amount of the alkaline neutralizer is 0.001%-5%, for example 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 33%, .5%, 4%, 4.5%, etc., and more preferably 0.1%-0.5%.

[0048] Preferably, the surfactant includes a silicone ether surfactant and / or a fluorine-containing surfactant.

[0049] Preferably, the silicone ether surfactant includes any one of a polyether siloxane copolymer, a polyether-modified siloxane copolymer or a polyester-modified polydimethylsiloxane copolymer, or a combination of at least two of them, wherein typical but non-limiting combinations include: a combination of a polyether siloxane copolymer and a polyether-modified siloxane copolymer, a combination of a polyether-modified siloxane copolymer and a polyester-modified polydimethylsiloxane copolymer, a combination of a polyether siloxane copolymer, a polyether-modified siloxane copolymer and a polyester-modified polydimethylsiloxane copolymer, and the like.

[0050] Preferably, the fluorine-containing surfactant includes any one of a carboxylate fluorocarbon surfactant, a sulfonate fluorocarbon surfactant or a phosphate fluorocarbon surfactant, or a combination of at least two of them, wherein typical but non-limiting combinations include: a combination of a carboxylate fluorocarbon surfactant and a sulfonate fluorocarbon surfactant, a combination of a sulfonate fluorocarbon surfactant and a phosphate fluorocarbon surfactant, a combination of a carboxylate fluorocarbon surfactant, a sulfonate fluorocarbon surfactant and a phosphate fluorocarbon surfactant, etc.

[0051] Preferably, based on 100% total solid content of the photoresist composition, the added amount of the surfactant is 200-10000 ppm, for example 500 ppm, 1000 ppm, 2000 ppm, 4000 ppm, 6000 ppm, 8000 ppm, etc., more preferably 300-1000 ppm.

[0052] In a second aspect, the present invention provides a use of the photoresist composition of the first aspect in a semiconductor.

[0053] Preferably, the thickness of the coating of the photoresist composition in the semiconductor is 3-10 μm, for example, 3.2 μm, 3.4 μm, 3.6 μm, 3.8 μm, 4 μm, 4.2 μm, 4.4 μm, 4.6 μm, 4.8 μm, 6 μm, 8 μm, 8.5 μm, 9 μm, 9.5 μm, etc.

[0054] Compared with the prior art, the present invention has the following beneficial effects:

[0055] (1) The photoresist composition of the present invention does not require the use of photosensitizers, has the characteristics of short exposure time and strong adhesion, can use g / i-line and g, h, i-wide spectrum exposure light sources, and the formed coating has the advantages of high resolution, high sensitivity and excellent etching resistance, etc., and can be stripped using ordinary stripping liquid, with strong stripping ability; the photoresist composition has the advantages and characteristics of multiple negative photoresists, while improving the shortcomings of existing negative photoresists, is easy to use and can be applied to semiconductor chip manufacturing processes, and is suitable for the etching process of 3 to 10 micron thick aluminum, copper or their alloy films and silicon dioxide insulating layers.

[0056] (2) After the photoresist composition described in the present invention forms a coating, the etching deviation of the etching experiment is within 32 μm, and the stripping time of the stripping experiment is within 100 s; the resolution of the photoresist composition described in the present invention is between 0.8-5 μm, and the exposure time is between 25-46 s. BRIEF DESCRIPTION OF THE DRAWINGS

[0057] Figure 1 is a graph showing the etching experimental results of the photoresist composition described in Example 1;

[0058] Figure 2 is a graph showing the etching experimental results of the photoresist composition described in Example 2;

[0059] Figure 3 This is a graph showing the etching experimental results of the photoresist composition described in Example 1. DETAILED DESCRIPTION

[0060] For the convenience of understanding the present invention, the present invention lists the following embodiments. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0061] Example 1

[0062] This embodiment provides a photoresist composition, which is composed of the following components:

[0063] Components Addition amount Phenolic resin 30 servings Photoacid generator 2 servings Melamine resin containing ether bonds 5 servings Hydroxypyridone 1 serving Solvents 62.5 copies Surfactants 500ppm (relative to total solid content)

[0064] Specifically, the phenolic resin is a copolymer of m-cresol phenolic resin and p-cresol phenolic resin with a segment ratio of 1.5:1, a weight average molecular weight of 15,000, and is purchased from Jinan Shengquan Group Co., Ltd.; the photoacid generator is 2-(4-methoxyphenylvinyl)-4,6-bis(trichloromethyl)-1,3,5-triazine; the melamine resin containing an ether bond is hexa(methoxymethyl)melamine, with a structural formula of The hydroxypyridone is 3-hydroxy-4-pyridone, and the structural formula is The solvent is propylene glycol monomethyl ether acetate; the surfactant is a polysiloxane surfactant purchased from Digo (International) Group Co., Ltd.

[0065] Example 2

[0066] This embodiment provides a photoresist composition, which is composed of the following components:

[0067] Components Addition amount Phenolic resin 30 servings Photoacid generator 2 servings Melamine resin containing ether bonds 5 servings Hydroxypyridone 1 serving Solvents 62.5 copies Surfactants 500ppm (relative to total solid content)

[0068] Specifically, the phenolic resin is the same as that in Example 1; the photoacid generator is 2-(4-methoxyphenylvinyl)-4,6-bis(trichloromethyl)-1,3,5-triazine; the melamine resin containing an ether bond is hexa(methoxymethyl)melamine, and the structural formula is The hydroxypyridone is 3,5-dihydroxy-4-pyridone, and the structural formula is The solvent is propylene glycol monomethyl ether acetate; the surfactant is a polysiloxane surfactant purchased from Digo (International) Group Co., Ltd.

[0069] Example 3

[0070] This embodiment provides a photoresist composition, which is composed of the following components:

[0071] Components Addition amount Phenolic resin 30 servings Photoacid generator 2 servings Melamine resin containing ether bonds 5 servings Hydroxypyridone 1 serving Solvents 62.5 copies Surfactants 500ppm (relative to total solid content)

[0072] Specifically, the phenolic resin is the same as that in Example 1; the photoacid generator is The melamine resin containing ether bonds is The hydroxypyridone is The solvent is propylene glycol monomethyl ether acetate; the surfactant is a polysiloxane surfactant purchased from Digo (International) Group Co., Ltd.

[0073] Example 4

[0074] The difference between this embodiment and embodiment 1 is that the 3-hydroxy-4-pyridone is replaced by an equal mass of hexa(methoxymethyl)melamine, and the added amount of the hexa(methoxymethyl)melamine in the photoresist composition is 6 parts, and the rest is the same as embodiment 1.

[0075] Embodiment 5-8

[0076] The difference between Examples 5-8 and Example 1 is that the mass ratios of hexa(methoxymethyl)melamine and 3-hydroxy-4-pyridone are different, namely 0.5:1 (Example 5), 1:1 (Example 6), 20:1 (Example 7), and 21:1 (Example 8), respectively. The total mass of the two is 6 parts, and the rest is the same as Example 1.

[0077] Examples 9-12

[0078] The difference between Examples 9-12 and Example 1 is that, based on the total mass of the phenolic resin being 100%, the total mass of the melamine resin containing ether bonds and the hydroxypyridone are different, namely 3% (Example 9), 5% (Example 10), 50% (Example 11) and 52% (Example 12), respectively, and the mass ratio between the two is 5:1. The amount of phenolic resin added is 30 parts, and the rest is the same as Example 1.

[0079] Comparative Example 1

[0080] This comparative example provides a photoresist composition, which is composed of the following components:

[0081] Components Addition amount Polyisoprene rubber 33 servings 4,4'-Diazidobenzophenone 2 servings Solvent (o-diphenol) 65.56 copies Surfactants 500ppm (relative to total solid content)

[0082] Specifically, the polyisoprene rubber has a weight average molecular weight of 22.1w and a cyclization rate of 60%-75%; the surfactant is a polysiloxane surfactant purchased from Digo (International) Group Co., Ltd.

[0083] Comparative Example 2

[0084] The difference between this comparative example and Example 1 is that the adhesion enhancer is replaced with bisphenol A of equal mass, and the rest is the same as Example 1.

[0085] Performance Testing

[0086] The photoresist compositions described in Examples 1-12 and Comparative Examples 1-2 were prepared into coatings:

[0087] The components of the photoresist composition are uniformly stirred to prepare a negative photoresist sample; the negative photoresist sample is coated on the surface of a silicon wafer deposited with a 3 μm metal aluminum film with a thickness of 5 μm, and exposed for 30 seconds under an MPA-500 scanning exposure machine, and then baked at 120° C. for 10 minutes, and finally developed with a 2.38% tetramethylammonium hydroxide aqueous solution for 60 seconds, thereby obtaining a pattern.

[0088] The resulting pattern was tested as follows:

[0089] (1) Etching experiment: The obtained pattern was etched by an etching solution at 40° C. for 20 minutes, and the etching morphology and etching deviation were counted. The etching solution used contained 2% nitric acid, 48% phosphoric acid, 7% acetic acid and 43% hydrogen peroxide in a weight ratio.

[0090] (2) Stripping experiment: The obtained pattern was heated to 60° C. in a stripping solution, and the stripping time was counted. The stripping solution was N-methylpyrrolidone containing 10% (by weight) ethanolamine.

[0091] (3) Resolution: The pattern is observed from large to small size using a scanning electron microscope until the pattern cannot be fully developed.

[0092] (4) Photosensitivity: Measure the size of the pattern at different energies until the resulting pattern is the same size as the mask pattern, and record the exposure time to obtain the pattern.

[0093] The test results are summarized in Figure 1-3 And in Table 1:

[0094] Table 1

[0095] Etching deviation / μm Stripping time / s Resolution / μm Exposure time / s Example 1 26 60 0.8 35 Example 2 21 50 1 30 Example 3 25 50 1.5 27 Example 4 32 80 1.5 37 Example 5 31 30 5 25 Example 6 28 40 3 36 Example 7 30 60 1 32 Example 8 32 70 1.5 37 Example 9 32 60 1 33 Example 10 27 60 1 34 Embodiment 11 28 80 3 44 Example 12 32 100 5 46 Comparative Example 1 34 240 10 50 Comparative Example 2 41 100 6 35

[0096] Analysis of the data in Table 1 shows that after the photoresist composition of the present invention forms a coating, the etching deviation of the etching experiment is within 32 μm, and the stripping time of the stripping experiment is within 100 s; the resolution of the photoresist composition of the present invention is between 0.8-5 μm, and the exposure time is between 25-46 s; the photoresist composition of the present invention does not require the use of a photosensitizer, has the characteristics of short exposure time and strong adhesion, can use g / i-line and g,h,i-wide spectrum exposure light sources, and the formed coating has the advantages of high resolution, high photosensitivity and excellent etching resistance, and can use ordinary stripping liquid for degumming, and has strong stripping ability; the photoresist composition has the advantages and characteristics of multiple negative photoresists, while improving the shortcomings of existing negative photoresists, is easy to use, can be applied to semiconductor chip manufacturing processes, and is suitable for the etching process of 3-10 micron thick aluminum, copper or their alloy films and silicon dioxide insulating layers.

[0097] Analysis of Comparative Examples 1-2 and Example 1 shows that the performance of Comparative Examples 1-2 is not as good as that of Example 1, proving that the photoresist composition of the present invention has better performance. Further, from the etching experimental result diagrams of Comparative Example 1, Example 1 and Example 2, it can be seen that the pattern of the photoresist composition of Comparative Example 1 is severely deformed after etching, proving that the photoresist composition of the present invention has excellent anti-etching performance.

[0098] Analysis of Comparative Example 2 and Example 1 shows that the performance of Comparative Example 2 is not as good as that of Example 1, which proves that the photoresist composition formed by using the adhesion enhancer of the present invention has better performance.

[0099] Analysis of Example 4 and Example 1 shows that the performance of Example 4 is not as good as that of Example 1, which proves that the photoresist composition formed by the combination of the adhesion enhancer preferably containing melamine resin with ether bonds and hydroxypyridone described in the present invention has better performance.

[0100] Analysis of Examples 5-8 shows that Examples 5 and 8 are not as good as Examples 6-7, proving that the photoresist composition formed by the mass ratio of the melamine resin containing ether bonds and hydroxypyridone within the preferred range has better performance.

[0101] Analysis of Examples 9-12 shows that Examples 9 and 12 are not as good as Examples 10-11, proving that the photoresist composition formed by the total mass of the melamine resin containing ether bonds and hydroxypyridone within the preferred range has better performance, based on the total mass of the phenolic resin as 100%.

[0102] The applicant declares that the present invention illustrates the detailed method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed method, that is, it does not mean that the present invention must rely on the above-mentioned detailed method to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A photoresist composition, characterized in that The photoresist composition comprises the following components: phenolic resin, photoacid generator, adhesion enhancer and solvent; The adhesion enhancer includes melamine resin and / or hydroxypyridone containing an ether bond.

2. The photoresist composition according to claim 1, characterized in that The photoresist composition does not include a photosensitizer.

3. The photoresist composition according to claim 1, characterized in that The structural formula of the melamine resin containing ether bonds is shown in Formula I: Wherein, R1, R2, R3, R4, R5, and R6 are each independently selected from any one of hydrogen, hydroxyl, substituted or unsubstituted C1-C20 alkyl, and substituted or unsubstituted C1-C20 alkoxy, and at least one of R1, R2, R3, R4, R5, and R6 is selected from substituted or unsubstituted ether; When the above groups have substituents, the substituents include hydroxyl, C1-C20 alkyl, C1-C20 alkoxy; Preferably, the structural formula of the melamine resin containing ether bonds is as follows:

4. The photoresist composition according to claim 1, characterized in that The structural formula of the hydroxypyridone is shown in Formula II: Among them, R7, R8, R9, R 10 Each of R7, R8, R9, R 10 At least one contains a hydroxyl group; When the above groups have substituents, the substituents include hydroxyl, C1-C20 alkyl, C1-C20 alkoxy; Preferably, the structural formula of the hydroxypyridone is as follows:

5. The photoresist composition according to claim 1, characterized in that Based on the total solid content of the photoresist composition as 100%, the amount of the melamine resin containing an ether bond is 2%-40%, the amount of the hydroxypyridone is 0.1%-10%, the amount of the phenolic resin is 55%-95%, and the amount of the photoacid generator is 0.001%-5%; Preferably, the mass ratio of the melamine resin containing an ether bond to the hydroxypyridone is (0.1-100):1, more preferably (1-20):1; Preferably, based on the total mass of the phenolic resin being 100%, the total mass of the melamine resin containing an ether bond and the hydroxypyridone is 0.1%-100%, more preferably 5%-50%; More preferably, the added amount of the photoacid generator is 0.1%-0.5%.

6. The photoresist composition according to claim 1, characterized in that The phenolic resin includes any one of m-cresol phenolic resin, p-cresol phenolic resin, m-cresol-p-cresol copolymer phenolic resin, xylenol-cresol copolymer phenolic resin or tris-cresol-cresol copolymer phenolic resin or a combination of at least two thereof; Preferably, the weight average molecular weight of the phenolic resin is 1000-60000, more preferably 8000-20000; Preferably, the dissolution rate of the phenolic resin in a tetramethylammonium hydroxide aqueous solution with a mass concentration of 2%-3% is Further preferably 7. The photoresist composition according to claim 1, characterized in that The photoacid generator includes any one or a combination of at least two of the compounds shown in the following structures: Among them, n-Bu is n-butyl, Ph is phenyl, and the wavy line represents that the benzene ring is a cis or trans structure.

8. The photoresist composition according to claim 1, characterized in that The solvent includes any one of propylene glycol monomethyl ether acetate, propylene glycol monomethyl ether, benzyl alcohol, n-butyl acetate, methyl methoxypropionate, ethyl lactate, ethyl ethoxypropionate or diethylene glycol methyl ethyl ether, or a combination of at least two thereof.

9. The photoresist composition according to claim 1, characterized in that The photoresist composition further comprises other additives; Preferably, the other additives include alkaline neutralizers and / or surfactants; Preferably, the alkaline neutralizer includes any one or a combination of at least two of N,N-bis(2-hydroxyethyl)pivalic acid amide, N,N-dimethylacetamide, N1,N1,N3,N3-tetrabutylmaleamide, pyridine, N-tert-butylethanolamine, 2-(dibutylamino)ethanol, 2-aminoethanol, tert-butyl 1-pyrrolidonecarboxylate, tert-butyl 2-ethyl-1H-imidazole-1-carboxylate or triethylamine; Preferably, the surfactant includes a silicone ether surfactant and / or a fluorine-containing surfactant; Preferably, the silicone ether surfactant includes any one or a combination of at least two of a polyether siloxane copolymer, a polyether-modified siloxane copolymer or a polyester-modified polydimethylsiloxane copolymer; Preferably, the fluorine-containing surfactant includes any one or a combination of at least two of a carboxylate fluorocarbon surfactant, a sulfonate fluorocarbon surfactant or a phosphate fluorocarbon surfactant; Preferably, based on the total solid content of the photoresist composition being 100%, the amount of the alkaline neutralizer added is 0.001%-5%, and more preferably 0.1%-0.5%; Preferably, based on 100% total solid content of the photoresist composition, the added amount of the surfactant is 200-10000 ppm, more preferably 300-1000 ppm.

10. Use of the photoresist composition according to any one of claims 1 to 9 in semiconductors; The thickness of the coating of the photoresist composition in the semiconductor is 3-10 μm.