Mica insulating material for battery cell and preparation method of mica insulating material

By combining mica sheets, PU foam, ceramic fiber and other materials into the battery cell mica insulation material, the problem of unstability of existing materials in high temperature environments is solved, the insulation, flame retardant and mechanical properties are improved, and it is suitable for new energy sources. High-end fields such as automobiles.

CN119069159APending Publication Date: 2024-12-03HANFER (SHANGHAI) PLASTIC TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411209020.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing battery cell mica insulation materials lack flame retardant materials and increase mechanical strength, which makes them unsuitable for high-end fields such as new energy vehicles, and are unstable in high-temperature environments, which can easily lead to overheating of the battery.

Method used

The battery cell is prepared through specific proportions and processes by combining materials such as mica sheets, PU foam, ceramic fibers, phosphate flame retardants, glass flakes, carbon fibers, alumina micropowder, melamine cyanurate and montmorillonite. Mica insulation material, enhances insulation, flame retardant, mechanical properties and thermal stability.

Benefits of technology

It significantly improves the insulation performance, flame retardant properties, mechanical properties and thermal stability of the battery cell mica insulating material, ensures the safe and stable operation of the battery in high temperature environments, and reduces fire risks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069159A_ABST
    Figure CN119069159A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of insulating materials for new energy automobiles, and discloses a battery cell mica insulating material which is prepared from the following raw materials in parts by weight: 40-50 parts of mica sheets, 25-35 parts of PU foam, 12-18 parts of ceramic fibers, 4-7 parts of a phosphate flame retardant, 25-35 parts of an organic silicon resin adhesive, 6-9 parts of glass flakes, 6-9 parts of carbon fibers, 10-13 parts of polyimide, 4-7 parts of alumina micro powder and 4-6 parts of vermiculite powder. 3 to 4 parts of melamine cyanurate and 5 to 8 parts of montmorillonite. According to the battery cell mica insulating material and the manufacturing method thereof, the mica sheet, the PU foam and other components are contained, the mica sheet ensures normal work of a battery, the PU foam provides buffering and enhances stability, all the components synergistically improve the thermal stability, mechanical strength, flame retardance and the like of the insulating material, the glass flakes enhance hardness and insulativity, the multiple materials jointly provide protection for the battery, and the service life of the battery is prolonged. The safety and durability are improved, and the stable operation of the battery is ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of insulating materials for new energy vehicles, and in particular to a mica insulating material for a battery core and a method for making the same. Background Art

[0002] With the continuous popularization of electronic devices and the rapid development of new energy vehicles, higher and higher performance requirements are placed on batteries. Batteries need to have characteristics such as high energy density, long cycle life, and high safety. In the battery structure, the battery cell is the core component, and its performance and safety directly affect the performance of the entire battery. Inside the battery, the battery will generate a certain electric field during the charging and discharging process. The insulating material can effectively block the leakage of the electric field to ensure the normal operation of the battery. Due to the irregularity of the gaps between the cylindrical battery cells, in order to facilitate the filling of buffer materials, rows of square modules are often arranged. This arrangement can effectively fill the buffer material and provide certain battery cell protection.

[0003] China invention patent announcement number: CN 116779215 B, discloses: a battery cell mica insulation material and its preparation method and application, the battery cell mica insulation material has excellent high temperature insulation, flame retardancy, fire resistance, and heat insulation, and can improve the safety of the battery pack while improving the space utilization of the battery cell, but its high thermal stability is not high, and the battery is prone to overheating when used for a long time in a high temperature environment. At the same time, the battery cell mica insulation material is prepared by mica powder, organic silica gel, alkali-free glass cloth short fiber, silane coupling agent, silicon dioxide hollow microbead powder, magnesium hydroxide powder, and polyurethane adhesive. It does not add flame retardant materials and materials that improve mechanical strength, and it does not have the function of protecting the battery, and is not suitable for high-end fields such as new energy vehicle batteries. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a battery cell mica insulating material and a method for producing the same, which can effectively solve the problem in the prior art that it does not have the added flame retardant material and the material for improving the mechanical strength, and at the same time it does not have the function of protecting the battery and is not suitable for high-end fields such as new energy vehicle batteries.

[0006] The technical solution adopted by the present invention is: a battery cell mica insulating material is prepared from the following raw materials in parts by weight: 40 to 50 parts of mica sheets, 25 to 35 parts of PU foam, 12 to 18 parts of ceramic fibers, 4 to 7 parts of phosphate flame retardants, 25 to 35 parts of silicone resin adhesives, 6 to 9 parts of glass flakes, 6 to 9 parts of carbon fibers, 10 to 13 parts of polyimide, 4 to 7 parts of alumina powder, 4 to 6 parts of vermiculite powder, 3 to 4 parts of melamine cyanurate, and 5 to 8 parts of montmorillonite.

[0007] Through the above technical scheme, mica flakes, as one of the main components, have natural high insulation properties. Their specific length, width and thickness can form an effective insulation layer in the battery cell to prevent current leakage, thereby improving the safety and stability of the battery. The silicone resin adhesive not only ensures the good combination of various components, but also has good insulation properties, further enhancing the insulation effect of the overall insulating material. After adding flame retardant ingredients such as phosphate flame retardants and melamine cyanurate, when an abnormal situation occurs in the battery, it can effectively prevent the spread of fire and reduce the risk of fire. The silica, alumina and calcium oxide in the glass flakes can not only enhance the mechanical properties of the material at a specific ratio, but also improve the flame retardant properties to a certain extent. When encountering high temperature, the glass flakes can form an insulating layer to prevent heat transfer and slow down the combustion rate. The PU foam provides a certain flexibility and buffering performance for the insulating material within a specific density and pore diameter range, which can reduce the external force impact on the battery during use and prevent insulation. Material rupture, ceramic fiber is made of a variety of ingredients, its specific diameter and length make it have high strength and toughness, in the insulating material, ceramic fiber can play a reinforcing role, improve the tensile strength, bending resistance and impact resistance of the material, carbon fiber has extremely high strength and stiffness, can further enhance the mechanical properties of the insulating material, so that it can maintain stable performance even in harsh use environments, alumina powder, vermiculite powder and other ingredients have good thermal stability, can withstand the high temperature generated during the operation of the battery, and maintain the stability of the performance of the insulating material, alumina, silica, magnesium oxide and other ingredients in ceramic fiber have good stability at high temperatures, can effectively resist thermal stress, and prevent the insulating material from being deformed or damaged due to high temperature, polyimide has excellent high temperature resistance, corrosion resistance and insulation performance, its addition can further improve the comprehensive performance of the insulating material, meet the needs of the battery under different working conditions, the addition of montmorillonite can improve the structural stability and adsorption performance of the insulating material, and improve the corrosion resistance and aging resistance of the material.

[0008] Preferably, the length of the mica sheet is 5 mm to 10 mm, the width is 2 mm to 6 mm, the thickness is 0.1 mm to 0.3 mm, and the density of the PU foam is 20 kg / m 3 ~30kg / m 3 The pore diameter is 0.1 mm to 0.5 mm, the diameter of the ceramic fiber is 3 μm to 8 μm, and the length is 5 mm to 10 mm.

[0009] The mica insulation material for battery cells prepared through the above technical scheme has significant advantages in insulation performance, flame retardancy, mechanical properties, thermal stability, etc., and can provide reliable guarantee for the safe and stable operation of the battery.

[0010] Preferably, the glass flakes are prepared from silica, alumina and calcium oxide, and the weight ratio of silica, alumina and calcium oxide is in the range of 70 to 80 parts of silica, 10 to 20 parts of alumina and 5 to 15 parts of calcium oxide.

[0011] Through the above technical scheme, the glass flakes prepared from silicon dioxide, aluminum oxide and calcium oxide have many advantages. First, it has good insulation properties and can effectively prevent current conduction, thereby improving the overall insulation effect of the mica insulation material of the battery cell. Secondly, the glass flakes can resist the erosion of chemicals such as acids and alkalis, and can protect the battery cells from the influence of the external chemical environment. Furthermore, it improves its own hardness and strength, can withstand certain external force impacts, is not easy to break or damage, and enhances the reliability of the insulating material. In addition, the presence of aluminum oxide can reduce the thermal expansion coefficient of the glass, improve the heat resistance of the glass flakes, and enable it to better adapt to the temperature changes during the operation of the battery.

[0012] Preferably, the ceramic fiber is prepared from alumina, silica, magnesium oxide, lanthanum oxide and yttrium oxide, and the weight ratio of alumina, silica, magnesium oxide, lanthanum oxide and yttrium oxide is in the range of 40 to 50 parts of alumina, 25 to 35 parts of silica, 10 to 15 parts of magnesium oxide, 3 to 6 parts of lanthanum oxide and 2 to 5 parts of yttrium oxide.

[0013] Through the above technical scheme, alumina, silica, magnesium oxide, lanthanum oxide and yttrium oxide in ceramic fibers provide high melting point and strength, enhance chemical stability, ensure that ceramic fibers are stable at high temperatures and not easily corroded by chemicals, silica also improves chemical stability and high-temperature performance, magnesium oxide increases toughness, making ceramic fibers more impact resistant, and can also adjust the thermal expansion coefficient to better match other materials, lanthanum oxide and yttrium oxide as rare earth oxides improve crystallization properties, making the crystal structure of ceramic fibers more uniform and dense, while greatly enhancing high-temperature stability, maintaining good mechanical and insulation properties at high temperatures, and may also optimize electrical properties and improve parameters such as insulation resistance. These components work together to make ceramic fibers a key component of mica insulation materials for battery cells, providing a strong guarantee for the safe and stable operation of batteries.

[0014] A method for preparing a battery cell mica insulating material is as follows:

[0015] S1: Select high-quality mica ore, and through crushing, grinding, screening and other processes, prepare mica flakes with a length of 5mm-10mm, a width of 2mm-6mm, and a thickness of 0.1mm-0.3mm. The crushing is done by a jaw crusher, the grinding is done by a ball mill, the grinding time is 2h-3h, and the screening is done by a 40-60 mesh screen;

[0016] S2: Mix polyether polyol and isocyanate in a ratio of 1:1.2 to 1:1.5, add 2% to 5% of the total mass of foaming agent and 0.5% to 1% of the total mass of catalyst, and control the density to 20kg / m through the foaming process. 3 ~30kg / m 3 , the pore diameter is 0.1mm~0.5mm, made into PU foam, the foaming temperature is 40℃~60℃, and the foaming time is 10 minutes~20 minutes;

[0017] S3: Using alumina, silica, magnesium oxide, lanthanum oxide and yttrium oxide as raw materials, first accurately weigh and evenly mix the raw materials according to the weight ratio of 40-50 parts of alumina, 25-35 parts of silica, 10-15 parts of magnesium oxide, 3-6 parts of lanthanum oxide and 2-5 parts of yttrium oxide, adopt the sol-gel method to prepare ceramic fiber, dissolve the mixed raw materials in a specific solvent to form a uniform solution, and then carry out gelation reaction at a gel temperature of 80°C to 100°C, and control the gel time to be 3h to 6h, so that the solution gradually changes into a gel state, and then heat-treat the gel to remove the solvent and other volatile components to obtain a ceramic precursor, and finally draw the ceramic precursor to prepare a ceramic fiber with a diameter of 3μm to 8μm and a length of 5mm to 10mm;

[0018] S4: mixing industrial-grade phosphoric acid, aluminum hydroxide, magnesium hydroxide, ammonium phosphate, ammonium polyphosphate and corresponding additives in a molar ratio of phosphoric acid: aluminum hydroxide: magnesium hydroxide: ammonium phosphate: ammonium polyphosphate: additive of 1:0.5:0.5:1:0.8:0.6, placing in a reactor, controlling the reactor temperature at 60°C to 80°C, stirring at a speed of 200r / min to 400r / min, and fully mixing, filtering, drying and other treatments of the mixed product to obtain a phosphate flame retardant;

[0019] S5: mixing an organic silicone resin, a curing agent, a filler and a coupling agent in a molar ratio of 1:0.3:0.4:0.2 in a reaction kettle, controlling the temperature at 80°C to 100°C, stirring at a speed of 300 r / min to 500 r / min, filtering to remove impurities after sufficient mixing, and drying at 100°C to 120°C to obtain an organic silicone resin adhesive;

[0020] S6: mixing silicon dioxide, aluminum oxide and calcium oxide uniformly according to weight ratio, heating to 1200°C to 1500°C to melt them, and then cooling, crushing and screening to obtain glass flakes, heating in a resistance furnace, the heating rate is 5°C / min to 10°C / min, cooling is done by air cooling, crushing is done by a hammer crusher, and screening is done by a 50-80 mesh screen;

[0021] S7: Using organic fiber as raw material, carbon fiber is prepared through high temperature treatment processes such as pre-oxidation, carbonization and graphitization, wherein the pre-oxidation temperature is 200°C to 300°C, the pre-oxidation time is 1h to 2h, the carbonization temperature is 800°C to 1000°C, the carbonization time is 1h to 2h, the graphitization temperature is 2500°C to 3000°C, and the graphitization time is 0.5h to 1h;

[0022] S8: synthesizing polyimide by polycondensation of pyromellitic dianhydride, the reaction being carried out under a nitrogen atmosphere, at a reaction temperature of 180 to 200° C., and for a reaction time of 4 to 6 hours;

[0023] S9: Using alumina as raw material, grinding and classifying to obtain alumina powder with particle size meeting the requirements, the grinding is carried out in a planetary ball mill, the grinding time is 3h to 5h, and the classification is carried out using a cyclone separator;

[0024] S10: selecting natural vermiculite ore, and obtaining vermiculite powder through crushing, grinding, screening and other processes, wherein the crushing is performed by a cone crusher, and the particle size after crushing is 5 mm to 10 mm, the grinding is performed by a Raymond mill, and the grinding time is 2 h to 3 h, and the screening is performed by a sieve of 40 mesh to 80 mesh;

[0025] S11: mixing melamine and cyanuric acid in a water solvent at a molar ratio of 1:1 to 1:1.2, reacting at 80° C. to 100° C. for 2 h to 3 h, filtering after the reaction, and drying at 120° C. to 150° C. for 4 h to 6 h to obtain melamine cyanurate;

[0026] S12: montmorillonite ore is mined, purified, modified, etc. to obtain montmorillonite that meets the requirements. The purification is carried out by washing with water and centrifuging. The modification is carried out by using hexadecyltrimethylammonium bromide as a modifier and reacting at 60°C to 80°C for 3h to 5h.

[0027] S13: The prepared mica flakes, ceramic fibers, phosphate flame retardants, silicone resin adhesives, glass flakes, carbon fibers, polyimide, alumina powder, vermiculite powder, melamine cyanurate and montmorillonite are mixed in parts by weight: 40-50 parts of mica flakes, 12-18 parts of ceramic fibers, 4-7 parts of phosphate flame retardants, 25-35 parts of silicone resin adhesives, 6-9 parts of glass flakes, 6-9 parts of carbon fibers, 10-13 parts of polyimide. 4-7 parts of aluminum oxide powder, 4-6 parts of vermiculite powder, 3-4 parts of melamine cyanurate, and 5-8 parts of montmorillonite are accurately weighed, the weighed materials are poured into a high-speed mixer, the mixer is started, and the mixture is first stirred at 1000 r / min-1500 r / min for 20 minutes-30 minutes, and then stirred at 500 r / min-800 r / min for 20 minutes-30 minutes to obtain a mica insulation material mixture for battery cells;

[0028] S14: placing the battery cell mica insulation material mixture into an aluminum alloy mold or a stainless steel mold, and pressing and molding it using a hydraulic press, wherein the pressing time is 30 minutes to 90 minutes, the pressing temperature is 50° C. to 80° C., the pressing pressure is 12 MPa to 18 MPa, and the cooling time is 30 minutes to 120 minutes to obtain material 1;

[0029] S15: Demolding to obtain material one, pasting PU foam on material one through silicone resin, and finally obtaining a battery cell mica insulating sheet.

[0030] Compared with the prior art, the present invention provides a battery core mica insulation material and a manufacturing method thereof, which has the following beneficial effects:

[0031] 1. The mica insulating material of the battery cell and its manufacturing method, wherein the mica sheet contained therein has good insulation performance and high temperature resistance, can ensure the normal operation of the battery, the PU foam can not only provide a certain buffering effect, but also its specific density and pore diameter can assist in enhancing the overall stability and flexibility of the insulating material, can protect the battery, the ceramic fiber has a suitable diameter and length, and is prepared by a variety of components in a precise ratio, which can greatly improve the thermal stability and mechanical strength of the insulating material, so that it can still maintain stable performance in a high temperature environment, and can withstand the pressure and vibration inside the battery, the phosphate flame retardant can effectively improve the flame retardant performance of the insulating material, reduce the risk of battery fire, and thus improve the safety of the battery, and the silicone resin adhesive has good high temperature resistance and corrosion resistance while ensuring the firm combination of various components;

[0032] 2. The glass flakes in the insulating material are made of silicon dioxide, aluminum oxide and calcium oxide in a specific proportion, which can enhance the hardness and wear resistance of the insulating material and also help to improve its insulation performance. Carbon fiber has high strength and high modulus, which further enhances the mechanical strength of the insulating material and makes it more durable. The addition of polyimide improves the high temperature resistance and chemical stability of the insulating material. Alumina powder can enhance the insulation and wear resistance of the insulating material. Vermiculite powder has good thermal insulation and hygroscopicity, which helps to control the temperature and humidity of the battery. Melamine cyanurate acts as a flame retardant and synergizes with phosphate flame retardants to further improve the flame retardant properties of the insulating material. After purification and modification, montmorillonite can enhance the adsorption performance and stability of the insulating material. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 The process of the present invention is shown in FIG. Figure 1 ;

[0034] Figure 2 The process of the present invention is shown in FIG. Figure 2 . DETAILED DESCRIPTION

[0035] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0036] Embodiment 1:

[0037] like Figure 1-2 As shown, a battery cell mica insulation material provided by the present invention is prepared from the following raw materials in parts by weight: 40 parts of mica sheets, 25 parts of PU foam, 12 parts of ceramic fibers, 4 parts of phosphate flame retardant, 25 parts of silicone resin adhesive, 6 parts of glass flakes, 6 parts of carbon fibers, 10 parts of polyimide, 4 parts of alumina powder, 4 parts of vermiculite powder, 3 parts of melamine cyanurate, and 5 parts of montmorillonite.

[0038] The advantage is that mica flakes, as one of the main components, have naturally high insulation properties. Their specific length, width and thickness can form an effective insulation layer in the battery cell to prevent current leakage, thereby improving the safety and stability of the battery. The silicone resin adhesive not only ensures the good combination of all components, but also has good insulation properties itself, further enhancing the insulation effect of the overall insulating material. After adding flame retardant ingredients such as phosphate flame retardants and melamine cyanurate, when an abnormal situation occurs in the battery, it can effectively prevent the spread of fire and reduce the risk of fire. The silica, alumina and calcium oxide in the glass flakes in a specific proportion can not only enhance the mechanical properties of the material, but also improve the flame retardant properties to a certain extent. When encountering high temperatures, the glass flakes can form an insulating layer to prevent heat transfer and slow down the combustion rate. The PU foam provides a certain flexibility and buffering performance for the insulating material within a specific density and pore diameter range, which can reduce the external force impact on the battery during use and prevent the insulating material from breaking. Crack, ceramic fiber is made of a variety of ingredients, and its specific diameter and length give it high strength and toughness. In insulating materials, ceramic fiber can play a reinforcing role and improve the material's tensile, bending and impact resistance. Carbon fiber has extremely high strength and stiffness, which can further enhance the mechanical properties of insulating materials, so that it can maintain stable performance even in harsh operating environments. Ingredients such as alumina micropowder and vermiculite powder have good thermal stability and can withstand the high temperature generated during the operation of the battery to maintain the stability of the performance of the insulating material. Alumina, silica, magnesium oxide and other ingredients in ceramic fibers have good stability at high temperatures and can effectively resist thermal stress to prevent the insulating material from being deformed or damaged due to high temperature. Polyimide has excellent high temperature resistance, corrosion resistance and insulation properties. Its addition can further improve the comprehensive performance of insulating materials and meet the needs of batteries under different working conditions. The addition of montmorillonite can improve the structural stability and adsorption properties of insulating materials, and improve the corrosion resistance and aging resistance of materials.

[0039] Specifically, the length of the mica sheet is 5 mm, the width is 2 mm, the thickness is 0.1 mm, and the density of the PU foam is 20 kg / m 3 , the pore diameter is 0.1mm, the diameter of the ceramic fiber is 3μm, and the length is 5mm.

[0040] The advantage is that the prepared battery cell mica insulation material has significant advantages in insulation performance, flame retardancy, mechanical properties, thermal stability, etc., and can provide reliable guarantee for the safe and stable operation of the battery.

[0041] Specifically, the glass flakes are prepared from silica, alumina and calcium oxide, and the weight ratio of silica, alumina and calcium oxide is 70 to 80 parts of silica, 10 to 20 parts of alumina and 5 to 15 parts of calcium oxide.

[0042] The advantage is that the glass flakes prepared from silicon dioxide, aluminum oxide and calcium oxide have many advantages. First, it has good insulation properties and can effectively prevent current conduction, thereby improving the overall insulation effect of the mica insulation material of the battery cell. Secondly, the glass flakes can resist the erosion of chemicals such as acids and alkalis, and can protect the battery cells from the influence of the external chemical environment. Thirdly, it improves its own hardness and strength, can withstand a certain external force impact, is not easy to break or damage, and enhances the reliability of the insulating material. In addition, the presence of aluminum oxide can reduce the thermal expansion coefficient of the glass, improve the heat resistance of the glass flakes, and enable it to better adapt to the temperature changes during the operation of the battery.

[0043] Specifically, the ceramic fiber is prepared from alumina, silica, magnesium oxide, lanthanum oxide and yttrium oxide, and the weight ratio of alumina, silica, magnesium oxide, lanthanum oxide and yttrium oxide is 40-50 parts of alumina, 25-35 parts of silica, 10-15 parts of magnesium oxide, 3-6 parts of lanthanum oxide and 2-5 parts of yttrium oxide.

[0044] The advantage is that alumina, silica, magnesium oxide, lanthanum oxide and yttrium oxide in ceramic fibers provide high melting point and strength, enhance chemical stability, ensure that ceramic fibers are stable at high temperatures and not easily corroded by chemicals, silica also improves chemical stability and high-temperature performance, magnesium oxide increases toughness, making ceramic fibers more impact resistant, and can also adjust the thermal expansion coefficient to better match other materials, lanthanum oxide and yttrium oxide as rare earth oxides improve crystallization properties, making the crystal structure of ceramic fibers more uniform and dense, while greatly enhancing high-temperature stability, maintaining good mechanical and insulation properties at high temperatures, and may also optimize electrical properties and improve parameters such as insulation resistance. These components work together to make ceramic fibers a key component of mica insulation materials for battery cells, providing strong guarantees for the safe and stable operation of batteries.

[0045] A method for preparing a battery cell mica insulating material is as follows:

[0046] S1: Select high-quality mica ore, and prepare mica flakes with a length of 5mm, a width of 2mm, and a thickness of 0.1mm through crushing, grinding, screening and other processes. The crushing is done by a jaw crusher, the grinding is done by a ball mill, the grinding time is 2h to 3h, and the screening is done by a 40-60 mesh screen;

[0047] S2: Mix polyether polyol and isocyanate in a ratio of 1:1.2 to 1:1.5, add 2% to 5% of the total mass of foaming agent and 0.5% to 1% of the total mass of catalyst, and control the density to 20kg / m through the foaming process. 3 , the pore diameter is 0.1mm, made into PU foam, the foaming temperature is 40℃~60℃, and the foaming time is 10 minutes~20 minutes;

[0048] S3: Using alumina, silica, magnesium oxide, lanthanum oxide and yttrium oxide as raw materials, first accurately weigh and evenly mix the raw materials according to the weight ratio of 40-50 parts of alumina, 25-35 parts of silica, 10-15 parts of magnesium oxide, 3-6 parts of lanthanum oxide and 2-5 parts of yttrium oxide, adopt the sol-gel method to prepare ceramic fiber, dissolve the mixed raw materials in a specific solvent to form a uniform solution, and then carry out gelation reaction at a gel temperature of 80°C to 100°C, and control the gel time to be 3h to 6h, so that the solution gradually changes into a gel state, and then heat-treat the gel to remove the solvent and other volatile components to obtain a ceramic precursor, and finally draw the ceramic precursor to prepare a ceramic fiber with a diameter of 3μm and a length of 5mm;

[0049] S4: mixing industrial-grade phosphoric acid, aluminum hydroxide, magnesium hydroxide, ammonium phosphate, ammonium polyphosphate and corresponding additives in a molar ratio of phosphoric acid: aluminum hydroxide: magnesium hydroxide: ammonium phosphate: ammonium polyphosphate: additive of 1:0.5:0.5:1:0.8:0.6, placing in a reactor, controlling the reactor temperature at 60°C to 80°C, stirring at a speed of 200r / min to 400r / min, and fully mixing, filtering, drying and other treatments of the mixed product to obtain a phosphate flame retardant;

[0050] S5: mixing an organic silicone resin, a curing agent, a filler and a coupling agent in a molar ratio of 1:0.3:0.4:0.2 in a reaction kettle, controlling the temperature at 80°C to 100°C, stirring at a speed of 300 r / min to 500 r / min, filtering to remove impurities after sufficient mixing, and drying at 100°C to 120°C to obtain an organic silicone resin adhesive;

[0051] S6: mixing silicon dioxide, aluminum oxide and calcium oxide uniformly according to weight ratio, heating to 1200°C to 1500°C to melt them, and then cooling, crushing and screening to obtain glass flakes, heating in a resistance furnace, the heating rate is 5°C / min to 10°C / min, cooling is done by air cooling, crushing is done by a hammer crusher, and screening is done by a 50-80 mesh screen;

[0052] S7: Using organic fiber as raw material, carbon fiber is prepared through high temperature treatment processes such as pre-oxidation, carbonization and graphitization, wherein the pre-oxidation temperature is 200°C to 300°C, the pre-oxidation time is 1h to 2h, the carbonization temperature is 800°C to 1000°C, the carbonization time is 1h to 2h, the graphitization temperature is 2500°C to 3000°C, and the graphitization time is 0.5h to 1h;

[0053] S8: synthesizing polyimide by polycondensation of pyromellitic dianhydride, the reaction being carried out under a nitrogen atmosphere, at a reaction temperature of 180 to 200° C., and for a reaction time of 4 to 6 hours;

[0054] S9: Using alumina as raw material, grinding and classifying to obtain alumina powder with particle size meeting the requirements, the grinding is carried out in a planetary ball mill, the grinding time is 3h to 5h, and the classification is carried out using a cyclone separator;

[0055] S10: selecting natural vermiculite ore, and obtaining vermiculite powder through crushing, grinding, screening and other processes, wherein the crushing is performed by a cone crusher, and the particle size after crushing is 5 mm to 10 mm, the grinding is performed by a Raymond mill, and the grinding time is 2 h to 3 h, and the screening is performed by a sieve of 40 mesh to 80 mesh;

[0056] S11: mixing melamine and cyanuric acid in a water solvent at a molar ratio of 1:1 to 1:1.2, reacting at 80° C. to 100° C. for 2 h to 3 h, filtering after the reaction, and drying at 120° C. to 150° C. for 4 h to 6 h to obtain melamine cyanurate;

[0057] S12: montmorillonite ore is mined, purified, modified, etc. to obtain montmorillonite that meets the requirements. The purification is carried out by washing with water and centrifuging. The modification is carried out by using hexadecyltrimethylammonium bromide as a modifier and reacting at 60°C to 80°C for 3h to 5h.

[0058] S13: The prepared mica flakes, ceramic fibers, phosphate flame retardants, silicone resin adhesives, glass flakes, carbon fibers, polyimide, alumina powder, vermiculite powder, melamine cyanurate and montmorillonite are mixed in parts by weight: 40-50 parts of mica flakes, 12-18 parts of ceramic fibers, 4-7 parts of phosphate flame retardants, 25-35 parts of silicone resin adhesives, 6-9 parts of glass flakes, 6-9 parts of carbon fibers, 10-13 parts of polyimide. 4-7 parts of aluminum oxide powder, 4-6 parts of vermiculite powder, 3-4 parts of melamine cyanurate, and 5-8 parts of montmorillonite are accurately weighed, the weighed materials are poured into a high-speed mixer, the mixer is started, and the mixture is first stirred at 1000 r / min-1500 r / min for 20 minutes-30 minutes, and then stirred at 500 r / min-800 r / min for 20 minutes-30 minutes to obtain a mica insulation material mixture for battery cells;

[0059] S14: placing the battery cell mica insulation material mixture into an aluminum alloy mold or a stainless steel mold, and pressing and molding it using a hydraulic press, wherein the pressing time is 30 minutes to 90 minutes, the pressing temperature is 50° C. to 80° C., the pressing pressure is 12 MPa to 18 MPa, and the cooling time is 30 minutes to 120 minutes to obtain material 1;

[0060] S15: Demolding to obtain material one, pasting PU foam on material one through silicone resin, and finally obtaining a battery cell mica insulating sheet.

[0061] Embodiment 2:

[0062] like Figure 1-2 As shown, a battery cell mica insulation material provided by the present invention is prepared from the following raw materials in parts by weight: 45 parts of mica sheets, 30 parts of PU foam, 15 parts of ceramic fibers, 6 parts of phosphate flame retardant, 30 parts of silicone resin adhesive, 8 parts of glass flakes, 7 parts of carbon fibers, 12 parts of polyimide, 5 parts of alumina powder, 5 parts of vermiculite powder, 3.5 parts of melamine cyanurate, and 6 parts of montmorillonite.

[0063] The advantage is that mica flakes, as one of the main components, have naturally high insulation properties. Their specific length, width and thickness can form an effective insulation layer in the battery cell to prevent current leakage, thereby improving the safety and stability of the battery. The silicone resin adhesive not only ensures the good combination of all components, but also has good insulation properties itself, further enhancing the insulation effect of the overall insulating material. After adding flame retardant ingredients such as phosphate flame retardants and melamine cyanurate, when an abnormal situation occurs in the battery, it can effectively prevent the spread of fire and reduce the risk of fire. The silica, alumina and calcium oxide in the glass flakes in a specific proportion can not only enhance the mechanical properties of the material, but also improve the flame retardant properties to a certain extent. When encountering high temperatures, the glass flakes can form an insulating layer to prevent heat transfer and slow down the combustion rate. The PU foam provides a certain flexibility and buffering performance for the insulating material within a specific density and pore diameter range, which can reduce the external force impact on the battery during use and prevent the insulating material from breaking. Crack, ceramic fiber is made of a variety of ingredients, and its specific diameter and length give it high strength and toughness. In insulating materials, ceramic fiber can play a reinforcing role and improve the material's tensile, bending and impact resistance. Carbon fiber has extremely high strength and stiffness, which can further enhance the mechanical properties of insulating materials, so that it can maintain stable performance even in harsh operating environments. Ingredients such as alumina micropowder and vermiculite powder have good thermal stability and can withstand the high temperature generated during the operation of the battery to maintain the stability of the performance of the insulating material. Alumina, silica, magnesium oxide and other ingredients in ceramic fibers have good stability at high temperatures and can effectively resist thermal stress to prevent the insulating material from being deformed or damaged due to high temperature. Polyimide has excellent high temperature resistance, corrosion resistance and insulation properties. Its addition can further improve the comprehensive performance of insulating materials and meet the needs of batteries under different working conditions. The addition of montmorillonite can improve the structural stability and adsorption properties of insulating materials, and improve the corrosion resistance and aging resistance of materials.

[0064] Specifically, the length of the mica sheet is 7 mm, the width is 3 mm, the thickness is 0.2 mm, and the density of the PU foam is 25 kg / m 3 , the pore diameter is 0.3mm, the diameter of the ceramic fiber is 5μm, and the length is 7mm.

[0065] The advantage is that the prepared battery cell mica insulation material has significant advantages in insulation performance, flame retardancy, mechanical properties, thermal stability, etc., and can provide reliable guarantee for the safe and stable operation of the battery.

[0066] Specifically, the glass flakes are prepared from silica, alumina and calcium oxide, and the weight ratio of silica, alumina and calcium oxide is 70 to 80 parts of silica, 10 to 20 parts of alumina and 5 to 15 parts of calcium oxide.

[0067] The advantage is that the glass flakes prepared from silicon dioxide, aluminum oxide and calcium oxide have many advantages. First, it has good insulation properties and can effectively prevent current conduction, thereby improving the overall insulation effect of the mica insulation material of the battery cell. Secondly, the glass flakes can resist the erosion of chemicals such as acids and alkalis, and can protect the battery cells from the influence of the external chemical environment. Thirdly, it improves its own hardness and strength, can withstand a certain external force impact, is not easy to break or damage, and enhances the reliability of the insulating material. In addition, the presence of aluminum oxide can reduce the thermal expansion coefficient of the glass, improve the heat resistance of the glass flakes, and enable it to better adapt to the temperature changes during the operation of the battery.

[0068] Specifically, the ceramic fiber is prepared from alumina, silica, magnesium oxide, lanthanum oxide and yttrium oxide, and the weight ratio of alumina, silica, magnesium oxide, lanthanum oxide and yttrium oxide is 40-50 parts of alumina, 25-35 parts of silica, 10-15 parts of magnesium oxide, 3-6 parts of lanthanum oxide and 2-5 parts of yttrium oxide.

[0069] The advantage is that alumina, silica, magnesium oxide, lanthanum oxide and yttrium oxide in ceramic fibers provide high melting point and strength, enhance chemical stability, ensure that ceramic fibers are stable at high temperatures and not easily corroded by chemicals, silica also improves chemical stability and high-temperature performance, magnesium oxide increases toughness, making ceramic fibers more impact resistant, and can also adjust the thermal expansion coefficient to better match other materials, lanthanum oxide and yttrium oxide as rare earth oxides improve crystallization properties, making the crystal structure of ceramic fibers more uniform and dense, while greatly enhancing high-temperature stability, maintaining good mechanical and insulation properties at high temperatures, and may also optimize electrical properties and improve parameters such as insulation resistance. These components work together to make ceramic fibers a key component of mica insulation materials for battery cells, providing strong guarantees for the safe and stable operation of batteries.

[0070] A method for preparing a battery cell mica insulating material is as follows:

[0071] S1: Select high-quality mica ore, and prepare mica flakes with a length of 7mm, a width of 3mm, and a thickness of 0.2mm through crushing, grinding, screening and other processes. The crushing is done by a jaw crusher, the grinding is done by a ball mill, the grinding time is 2h to 3h, and the screening is done by a sieve of 40-60 meshes;

[0072] S2: Mix polyether polyol and isocyanate in a ratio of 1:1.2 to 1:1.5, add 2% to 5% of the total mass of foaming agent and 0.5% to 1% of the total mass of catalyst, and control the density to 25kg / m through the foaming process. 3 , the pore diameter is 0.3mm, made into PU foam, the foaming temperature is 40℃~60℃, and the foaming time is 10 minutes~20 minutes;

[0073] S3: Using alumina, silica, magnesium oxide, lanthanum oxide and yttrium oxide as raw materials, first accurately weigh and evenly mix the raw materials according to the weight ratio of 40-50 parts of alumina, 25-35 parts of silica, 10-15 parts of magnesium oxide, 3-6 parts of lanthanum oxide and 2-5 parts of yttrium oxide, and adopt the sol-gel method to prepare ceramic fiber, dissolve the mixed raw materials in a specific solvent to form a uniform solution, and then carry out gelation reaction at a gel temperature of 80°C to 100°C, and control the gel time to be 3h to 6h, so that the solution gradually changes into a gel state, and then heat-treat the gel to remove the solvent and other volatile components to obtain a ceramic precursor, and finally draw the ceramic precursor to prepare a ceramic fiber with a diameter of 5μm and a length of 7mm;

[0074] S4: mixing industrial-grade phosphoric acid, aluminum hydroxide, magnesium hydroxide, ammonium phosphate, ammonium polyphosphate and corresponding additives in a molar ratio of phosphoric acid: aluminum hydroxide: magnesium hydroxide: ammonium phosphate: ammonium polyphosphate: additive of 1:0.5:0.5:1:0.8:0.6, placing in a reactor, controlling the reactor temperature at 60°C to 80°C, stirring at a speed of 200r / min to 400r / min, and fully mixing, filtering, drying and other treatments of the mixed product to obtain a phosphate flame retardant;

[0075] S5: mixing an organic silicone resin, a curing agent, a filler and a coupling agent in a molar ratio of 1:0.3:0.4:0.2 in a reaction kettle, controlling the temperature at 80°C to 100°C, stirring at a speed of 300 r / min to 500 r / min, filtering to remove impurities after sufficient mixing, and drying at 100°C to 120°C to obtain an organic silicone resin adhesive;

[0076] S6: mixing silicon dioxide, aluminum oxide and calcium oxide uniformly according to weight ratio, heating to 1200°C to 1500°C to melt them, and then cooling, crushing and screening to obtain glass flakes, heating in a resistance furnace, the heating rate is 5°C / min to 10°C / min, cooling is done by air cooling, crushing is done by a hammer crusher, and screening is done by a 50-80 mesh screen;

[0077] S7: Using organic fiber as raw material, carbon fiber is prepared through high temperature treatment processes such as pre-oxidation, carbonization and graphitization, wherein the pre-oxidation temperature is 200°C to 300°C, the pre-oxidation time is 1h to 2h, the carbonization temperature is 800°C to 1000°C, the carbonization time is 1h to 2h, the graphitization temperature is 2500°C to 3000°C, and the graphitization time is 0.5h to 1h;

[0078] S8: synthesizing polyimide by polycondensation of pyromellitic dianhydride, the reaction being carried out under a nitrogen atmosphere, at a reaction temperature of 180 to 200° C., and for a reaction time of 4 to 6 hours;

[0079] S9: Using alumina as raw material, grinding and classifying to obtain alumina powder with particle size meeting the requirements, the grinding is carried out in a planetary ball mill, the grinding time is 3h to 5h, and the classification is carried out using a cyclone separator;

[0080] S10: selecting natural vermiculite ore, and obtaining vermiculite powder through crushing, grinding, screening and other processes, wherein the crushing is performed by a cone crusher, and the particle size after crushing is 5 mm to 10 mm, the grinding is performed by a Raymond mill, and the grinding time is 2 h to 3 h, and the screening is performed by a sieve of 40 mesh to 80 mesh;

[0081] S11: mixing melamine and cyanuric acid in a water solvent at a molar ratio of 1:1 to 1:1.2, reacting at 80° C. to 100° C. for 2 h to 3 h, filtering after the reaction, and drying at 120° C. to 150° C. for 4 h to 6 h to obtain melamine cyanurate;

[0082] S12: montmorillonite ore is mined, purified, modified, etc. to obtain montmorillonite that meets the requirements. The purification is carried out by washing with water and centrifuging. The modification is carried out by using hexadecyltrimethylammonium bromide as a modifier and reacting at 60°C to 80°C for 3h to 5h.

[0083] S13: The prepared mica flakes, ceramic fibers, phosphate flame retardants, silicone resin adhesives, glass flakes, carbon fibers, polyimide, alumina powder, vermiculite powder, melamine cyanurate and montmorillonite are mixed in parts by weight: 40-50 parts of mica flakes, 12-18 parts of ceramic fibers, 4-7 parts of phosphate flame retardants, 25-35 parts of silicone resin adhesives, 6-9 parts of glass flakes, 6-9 parts of carbon fibers, 10-13 parts of polyimide. 4-7 parts of aluminum oxide powder, 4-6 parts of vermiculite powder, 3-4 parts of melamine cyanurate, and 5-8 parts of montmorillonite are accurately weighed, the weighed materials are poured into a high-speed mixer, the mixer is started, and the mixture is first stirred at 1000 r / min-1500 r / min for 20 minutes-30 minutes, and then stirred at 500 r / min-800 r / min for 20 minutes-30 minutes to obtain a mica insulation material mixture for battery cells;

[0084] S14: placing the battery cell mica insulation material mixture into an aluminum alloy mold or a stainless steel mold, and pressing and molding it using a hydraulic press, wherein the pressing time is 30 minutes to 90 minutes, the pressing temperature is 50° C. to 80° C., the pressing pressure is 12 MPa to 18 MPa, and the cooling time is 30 minutes to 120 minutes to obtain material 1;

[0085] S15: Demolding to obtain material one, pasting PU foam on material one through silicone resin, and finally obtaining a battery cell mica insulating sheet.

[0086] Embodiment three:

[0087] like Figure 1-2 As shown, a battery cell mica insulation material provided by the present invention is prepared from the following raw materials in parts by weight: 50 parts of mica sheets, 35 parts of PU foam, 18 parts of ceramic fibers, 7 parts of phosphate flame retardant, 35 parts of silicone resin adhesive, 9 parts of glass flakes, 9 parts of carbon fibers, 13 parts of polyimide, 7 parts of alumina powder, 6 parts of vermiculite powder, 4 parts of melamine cyanurate, and 8 parts of montmorillonite.

[0088] The advantage is that mica flakes, as one of the main components, have naturally high insulation properties. Their specific length, width and thickness can form an effective insulation layer in the battery cell to prevent current leakage, thereby improving the safety and stability of the battery. The silicone resin adhesive not only ensures the good combination of all components, but also has good insulation properties itself, further enhancing the insulation effect of the overall insulating material. After adding flame retardant ingredients such as phosphate flame retardants and melamine cyanurate, when an abnormal situation occurs in the battery, it can effectively prevent the spread of fire and reduce the risk of fire. The silica, alumina and calcium oxide in the glass flakes in a specific proportion can not only enhance the mechanical properties of the material, but also improve the flame retardant properties to a certain extent. When encountering high temperatures, the glass flakes can form an insulating layer to prevent heat transfer and slow down the combustion rate. The PU foam provides a certain flexibility and buffering performance for the insulating material within a specific density and pore diameter range, which can reduce the external force impact on the battery during use and prevent the insulating material from breaking. Crack, ceramic fiber is made of a variety of ingredients, and its specific diameter and length give it high strength and toughness. In insulating materials, ceramic fiber can play a reinforcing role and improve the material's tensile, bending and impact resistance. Carbon fiber has extremely high strength and stiffness, which can further enhance the mechanical properties of insulating materials, so that it can maintain stable performance even in harsh operating environments. Ingredients such as alumina micropowder and vermiculite powder have good thermal stability and can withstand the high temperature generated during the operation of the battery to maintain the stability of the performance of the insulating material. Alumina, silica, magnesium oxide and other ingredients in ceramic fibers have good stability at high temperatures and can effectively resist thermal stress to prevent the insulating material from being deformed or damaged due to high temperature. Polyimide has excellent high temperature resistance, corrosion resistance and insulation properties. Its addition can further improve the comprehensive performance of insulating materials and meet the needs of batteries under different working conditions. The addition of montmorillonite can improve the structural stability and adsorption properties of insulating materials, and improve the corrosion resistance and aging resistance of materials.

[0089] Specifically, the length of the mica sheet is 10 mm, the width is 6 mm, the thickness is 0.3 mm, and the density of the PU foam is 30 kg / m 3 , the pore diameter is 0.5mm, the diameter of the ceramic fiber is 8μm, and the length is 10mm.

[0090] The advantage is that the prepared battery cell mica insulation material has significant advantages in insulation performance, flame retardancy, mechanical properties, thermal stability, etc., and can provide reliable guarantee for the safe and stable operation of the battery.

[0091] Specifically, the glass flakes are prepared from silica, alumina and calcium oxide, and the weight ratio of silica, alumina and calcium oxide is 70 to 80 parts of silica, 10 to 20 parts of alumina and 5 to 15 parts of calcium oxide.

[0092] The advantage is that the glass flakes prepared from silicon dioxide, aluminum oxide and calcium oxide have many advantages. First, it has good insulation properties and can effectively prevent current conduction, thereby improving the overall insulation effect of the mica insulation material of the battery cell. Secondly, the glass flakes can resist the erosion of chemicals such as acids and alkalis, and can protect the battery cells from the influence of the external chemical environment. Thirdly, it improves its own hardness and strength, can withstand a certain external force impact, is not easy to break or damage, and enhances the reliability of the insulating material. In addition, the presence of aluminum oxide can reduce the thermal expansion coefficient of the glass, improve the heat resistance of the glass flakes, and enable it to better adapt to the temperature changes during the operation of the battery.

[0093] Specifically, the ceramic fiber is prepared from alumina, silica, magnesium oxide, lanthanum oxide and yttrium oxide, and the weight ratio of alumina, silica, magnesium oxide, lanthanum oxide and yttrium oxide is 40-50 parts of alumina, 25-35 parts of silica, 10-15 parts of magnesium oxide, 3-6 parts of lanthanum oxide and 2-5 parts of yttrium oxide.

[0094] The advantage is that alumina, silica, magnesium oxide, lanthanum oxide and yttrium oxide in ceramic fibers provide high melting point and strength, enhance chemical stability, ensure that ceramic fibers are stable at high temperatures and not easily corroded by chemicals, silica also improves chemical stability and high-temperature performance, magnesium oxide increases toughness, making ceramic fibers more impact resistant, and can also adjust the thermal expansion coefficient to better match other materials, lanthanum oxide and yttrium oxide as rare earth oxides improve crystallization properties, making the crystal structure of ceramic fibers more uniform and dense, while greatly enhancing high-temperature stability, maintaining good mechanical and insulation properties at high temperatures, and may also optimize electrical properties and improve parameters such as insulation resistance. These components work together to make ceramic fibers a key component of mica insulation materials for battery cells, providing strong guarantees for the safe and stable operation of batteries.

[0095] A method for preparing a battery cell mica insulating material is as follows:

[0096] S1: Select high-quality mica ore, and prepare mica flakes with a length of 10 mm, a width of 6 mm, and a thickness of 0.3 mm through processes such as crushing, grinding, and screening. The crushing is done by a jaw crusher, the grinding is done by a ball mill, the grinding time is 2h to 3h, and the screening is done by a sieve of 40 to 60 meshes;

[0097] S2: Mix polyether polyol and isocyanate in a ratio of 1:1.2 to 1:1.5, add 2% to 5% of the total mass of foaming agent and 0.5% to 1% of the total mass of catalyst, and control the density to 30kg / m through the foaming process. 3 , the pore diameter is 0.5mm, made into PU foam, the foaming temperature is 40℃~60℃, and the foaming time is 10 minutes~20 minutes;

[0098] S3: Using alumina, silica, magnesium oxide, lanthanum oxide and yttrium oxide as raw materials, first accurately weigh and evenly mix the raw materials according to the weight ratio of 40-50 parts of alumina, 25-35 parts of silica, 10-15 parts of magnesium oxide, 3-6 parts of lanthanum oxide and 2-5 parts of yttrium oxide, adopt the sol-gel method to prepare ceramic fiber, dissolve the mixed raw materials in a specific solvent to form a uniform solution, and then carry out gelation reaction at a gel temperature of 80°C to 100°C, and control the gel time to be 3h to 6h, so that the solution gradually changes into a gel state, and then heat-treat the gel to remove the solvent and other volatile components to obtain a ceramic precursor, and finally draw the ceramic precursor to prepare a ceramic fiber with a diameter of 8μm and a length of 10mm;

[0099] S4: mixing industrial-grade phosphoric acid, aluminum hydroxide, magnesium hydroxide, ammonium phosphate, ammonium polyphosphate and corresponding additives in a molar ratio of phosphoric acid: aluminum hydroxide: magnesium hydroxide: ammonium phosphate: ammonium polyphosphate: additive of 1:0.5:0.5:1:0.8:0.6, placing in a reactor, controlling the reactor temperature at 60°C to 80°C, stirring at a speed of 200r / min to 400r / min, and fully mixing, filtering, drying and other treatments of the mixed product to obtain a phosphate flame retardant;

[0100] S5: mixing an organic silicone resin, a curing agent, a filler and a coupling agent in a molar ratio of 1:0.3:0.4:0.2 in a reaction kettle, controlling the temperature at 80°C to 100°C, stirring at a speed of 300 r / min to 500 r / min, filtering to remove impurities after sufficient mixing, and drying at 100°C to 120°C to obtain an organic silicone resin adhesive;

[0101] S6: mixing silicon dioxide, aluminum oxide and calcium oxide uniformly according to weight ratio, heating to 1200°C to 1500°C to melt them, and then cooling, crushing and screening to obtain glass flakes, heating in a resistance furnace, the heating rate is 5°C / min to 10°C / min, cooling is done by air cooling, crushing is done by a hammer crusher, and screening is done by a 50-80 mesh screen;

[0102] S7: Using organic fiber as raw material, carbon fiber is prepared through high temperature treatment processes such as pre-oxidation, carbonization and graphitization, wherein the pre-oxidation temperature is 200°C to 300°C, the pre-oxidation time is 1h to 2h, the carbonization temperature is 800°C to 1000°C, the carbonization time is 1h to 2h, the graphitization temperature is 2500°C to 3000°C, and the graphitization time is 0.5h to 1h;

[0103] S8: synthesizing polyimide by polycondensation of pyromellitic dianhydride, the reaction being carried out under a nitrogen atmosphere, at a reaction temperature of 180 to 200° C., and for a reaction time of 4 to 6 hours;

[0104] S9: Using alumina as raw material, grinding and classifying to obtain alumina powder with particle size meeting the requirements, the grinding is carried out in a planetary ball mill, the grinding time is 3h to 5h, and the classification is carried out using a cyclone separator;

[0105] S10: selecting natural vermiculite ore, and obtaining vermiculite powder through crushing, grinding, screening and other processes, wherein the crushing is performed by a cone crusher, and the particle size after crushing is 5 mm to 10 mm, the grinding is performed by a Raymond mill, and the grinding time is 2 h to 3 h, and the screening is performed by a sieve of 40 mesh to 80 mesh;

[0106] S11: mixing melamine and cyanuric acid in a water solvent at a molar ratio of 1:1 to 1:1.2, reacting at 80° C. to 100° C. for 2 h to 3 h, filtering after the reaction, and drying at 120° C. to 150° C. for 4 h to 6 h to obtain melamine cyanurate;

[0107] S12: montmorillonite ore is mined, purified, modified, etc. to obtain montmorillonite that meets the requirements. The purification is carried out by washing with water and centrifuging. The modification is carried out by using hexadecyltrimethylammonium bromide as a modifier and reacting at 60°C to 80°C for 3h to 5h.

[0108] S13: The prepared mica flakes, ceramic fibers, phosphate flame retardants, silicone resin adhesives, glass flakes, carbon fibers, polyimide, alumina powder, vermiculite powder, melamine cyanurate and montmorillonite are mixed in parts by weight: 40-50 parts of mica flakes, 12-18 parts of ceramic fibers, 4-7 parts of phosphate flame retardants, 25-35 parts of silicone resin adhesives, 6-9 parts of glass flakes, 6-9 parts of carbon fibers, 10-13 parts of polyimide. 4-7 parts of aluminum oxide powder, 4-6 parts of vermiculite powder, 3-4 parts of melamine cyanurate, and 5-8 parts of montmorillonite are accurately weighed, the weighed materials are poured into a high-speed mixer, the mixer is started, and the mixture is first stirred at 1000 r / min-1500 r / min for 20 minutes-30 minutes, and then stirred at 500 r / min-800 r / min for 20 minutes-30 minutes to obtain a mica insulation material mixture for battery cells;

[0109] S14: placing the battery cell mica insulation material mixture into an aluminum alloy mold or a stainless steel mold, and pressing and molding it using a hydraulic press, wherein the pressing time is 30 minutes to 90 minutes, the pressing temperature is 50° C. to 80° C., the pressing pressure is 12 MPa to 18 MPa, and the cooling time is 30 minutes to 120 minutes to obtain material 1;

[0110] S15: Demolding to obtain material one, pasting PU foam on material one through silicone resin, and finally obtaining a battery cell mica insulating sheet.

[0111] In summary, when the components of the battery cell mica insulation material are 50 parts of mica sheets, 35 parts of PU foam, 18 parts of ceramic fiber, 7 parts of phosphate flame retardant, 35 parts of silicone resin adhesive, 9 parts of glass flakes, 9 parts of carbon fiber, 13 parts of polyimide, 7 parts of alumina powder, 6 parts of vermiculite powder, 4 parts of melamine cyanurate, 8 parts of montmorillonite, and the length of the mica sheet is 10 mm, the width is 6 mm, the thickness is 0.3 mm, and the density of the PU foam is 30 kg / m 3 When the pore diameter is 0.5 mm, the diameter of the ceramic fiber is 8 μm, and the length is 10 mm, the obtained battery cell mica insulation material has higher insulation performance, excellent flame retardant ability, good thermal stability, strong corrosion resistance and excellent anti-aging performance.

[0112] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A battery cell mica insulating material, characterized in that: The invention is prepared from the following raw materials in parts by weight: 40-50 parts of mica sheets, 25-35 parts of PU foams, 12-18 parts of ceramic fibers, 4-7 parts of phosphate flame retardants, 25-35 parts of silicone resin adhesives, 6-9 parts of glass flakes, 6-9 parts of carbon fibers, 10-13 parts of polyimide, 4-7 parts of alumina powder, 4-6 parts of vermiculite powder, 3-4 parts of melamine cyanurate and 5-8 parts of montmorillonite.

2. The battery core mica insulating material according to claim 1, characterized in that: The length of the mica sheet is 5 mm to 10 mm, the width is 2 mm to 6 mm, the thickness is 0.1 mm to 0.3 mm, and the density of the PU foam is 20 kg / m 3 ~30kg / m 3 The pore diameter is 0.1 mm to 0.5 mm, the diameter of the ceramic fiber is 3 μm to 8 μm, and the length is 5 mm to 10 mm.

3. The battery core mica insulating material according to claim 1, characterized in that: The glass flakes are prepared from silicon dioxide, aluminum oxide and calcium oxide, and the weight ratio of silicon dioxide, aluminum oxide and calcium oxide is 70 to 80 parts of silicon dioxide, 10 to 20 parts of aluminum oxide and 5 to 15 parts of calcium oxide.

4. The battery core mica insulating material according to claim 1, characterized in that: The ceramic fiber is prepared from alumina, silica, magnesium oxide, lanthanum oxide and yttrium oxide, wherein the weight ratio of the alumina, silica, magnesium oxide, lanthanum oxide and yttrium oxide is 40 to 50 parts of alumina, 25 to 35 parts of silica, 10 to 15 parts of magnesium oxide, 3 to 6 parts of lanthanum oxide and 2 to 5 parts of yttrium oxide.

5. A method for preparing a battery cell mica insulating material, characterized in that: A battery cell mica insulating material comprising: S1: Select high-quality mica ore, and through crushing, grinding, screening and other processes, prepare mica flakes with a length of 5mm-10mm, a width of 2mm-6mm, and a thickness of 0.1mm-0.3mm. The crushing is done by a jaw crusher, the grinding is done by a ball mill, the grinding time is 2h-3h, and the screening is done by a 40-60 mesh screen; S2: Mix polyether polyol and isocyanate in a ratio of 1:1.2 to 1:1.5, add 2% to 5% of the total mass of foaming agent and 0.5% to 1% of the total mass of catalyst, and control the density to 20kg / m through the foaming process. 3 ~30kg / m 3 , the pore diameter is 0.1mm~0.5mm, made into PU foam, the foaming temperature is 40℃~60℃, and the foaming time is 10 minutes~20 minutes; S3: Using alumina, silica, magnesium oxide, lanthanum oxide and yttrium oxide as raw materials, first accurately weigh and evenly mix the raw materials according to the weight ratio of 40-50 parts of alumina, 25-35 parts of silica, 10-15 parts of magnesium oxide, 3-6 parts of lanthanum oxide and 2-5 parts of yttrium oxide, adopt the sol-gel method to prepare ceramic fiber, dissolve the mixed raw materials in a specific solvent to form a uniform solution, and then carry out gelation reaction at a gel temperature of 80°C to 100°C, and control the gel time to be 3h to 6h, so that the solution gradually changes into a gel state, and then heat-treat the gel to remove the solvent and other volatile components to obtain a ceramic precursor, and finally draw the ceramic precursor to prepare a ceramic fiber with a diameter of 3μm to 8μm and a length of 5mm to 10mm; S4: mixing industrial-grade phosphoric acid, aluminum hydroxide, magnesium hydroxide, ammonium phosphate, ammonium polyphosphate and corresponding additives in a molar ratio of phosphoric acid: aluminum hydroxide: magnesium hydroxide: ammonium phosphate: ammonium polyphosphate: additive of 1:0.5:0.5:1:0.8:0.6, placing in a reactor, controlling the reactor temperature at 60°C to 80°C, stirring at a speed of 200r / min to 400r / min, and fully mixing, filtering, drying and other treatments of the mixed product to obtain a phosphate flame retardant; S5: mixing an organic silicone resin, a curing agent, a filler and a coupling agent in a molar ratio of 1:0.3:0.4:0.2 in a reaction kettle, controlling the temperature at 80°C to 100°C, stirring at a speed of 300 r / min to 500 r / min, filtering to remove impurities after sufficient mixing, and drying at 100°C to 120°C to obtain an organic silicone resin adhesive; S6: mixing silicon dioxide, aluminum oxide and calcium oxide uniformly according to weight ratio, heating to 1200°C to 1500°C to melt them, and then cooling, crushing and screening to obtain glass flakes, heating in a resistance furnace, the heating rate is 5°C / min to 10°C / min, cooling is done by air cooling, crushing is done by a hammer crusher, and screening is done by a 50-80 mesh screen; S7: Using organic fiber as raw material, carbon fiber is prepared through high temperature treatment processes such as pre-oxidation, carbonization and graphitization, wherein the pre-oxidation temperature is 200°C to 300°C, the pre-oxidation time is 1h to 2h, the carbonization temperature is 800°C to 1000°C, the carbonization time is 1h to 2h, the graphitization temperature is 2500°C to 3000°C, and the graphitization time is 0.5h to 1h; S8: synthesizing polyimide by polycondensation of pyromellitic dianhydride, the reaction being carried out under a nitrogen atmosphere, at a reaction temperature of 180 to 200° C., and for a reaction time of 4 to 6 hours; S9: Using alumina as raw material, grinding and classifying to obtain alumina powder with particle size meeting the requirements, the grinding is carried out in a planetary ball mill, the grinding time is 3h to 5h, and the classification is carried out using a cyclone separator; S10: selecting natural vermiculite ore, and obtaining vermiculite powder through crushing, grinding, screening and other processes, wherein the crushing is performed by a cone crusher, and the particle size after crushing is 5 mm to 10 mm, the grinding is performed by a Raymond mill, and the grinding time is 2 h to 3 h, and the screening is performed by a sieve of 40 mesh to 80 mesh; S11: mixing melamine and cyanuric acid in a water solvent at a molar ratio of 1:1 to 1:1.2, reacting at 80° C. to 100° C. for 2 h to 3 h, filtering after the reaction, and drying at 120° C. to 150° C. for 4 h to 6 h to obtain melamine cyanurate; S12: montmorillonite ore is mined, purified, modified, etc. to obtain montmorillonite that meets the requirements. The purification is carried out by washing with water and centrifuging. The modification is carried out by using hexadecyltrimethylammonium bromide as a modifier and reacting at 60°C to 80°C for 3h to 5h. S13: The prepared mica flakes, ceramic fibers, phosphate flame retardants, silicone resin adhesives, glass flakes, carbon fibers, polyimide, alumina powder, vermiculite powder, melamine cyanurate and montmorillonite are mixed in parts by weight: 40-50 parts of mica flakes, 12-18 parts of ceramic fibers, 4-7 parts of phosphate flame retardants, 25-35 parts of silicone resin adhesives, 6-9 parts of glass flakes, 6-9 parts of carbon fibers, 10-13 parts of polyimide. 4-7 parts of aluminum oxide powder, 4-6 parts of vermiculite powder, 3-4 parts of melamine cyanurate, and 5-8 parts of montmorillonite are accurately weighed, the weighed materials are poured into a high-speed mixer, the mixer is started, and the mixture is first stirred at 1000 r / min-1500 r / min for 20 minutes-30 minutes, and then stirred at 500 r / min-800 r / min for 20 minutes-30 minutes to obtain a mica insulation material mixture for battery cells; S14: placing the battery cell mica insulation material mixture into an aluminum alloy mold or a stainless steel mold, and pressing and molding it using a hydraulic press, wherein the pressing time is 30 minutes to 90 minutes, the pressing temperature is 50° C. to 80° C., the pressing pressure is 12 MPa to 18 MPa, and the cooling time is 30 minutes to 120 minutes to obtain material 1; S15: Demolding to obtain material one, pasting PU foam on material one through silicone resin, and finally obtaining a battery cell mica insulating sheet.