High-resistivity sintered neodymium-iron-boron magnet

By covering high-resistivity auxiliary alloys on the neodymium iron boron magnet and diffusing grain boundaries, a continuous and uniform praseodymium-rich thin layer is formed, which solves the problem of improving resistivity in the prior art that affects magnetic performance, and achieves high efficiency and low cost The resistivity and high-temperature performance of NdFeB magnets are improved.

CN119069247APending Publication Date: 2024-12-03ZHEJIANG KAIVEN MAGNETICS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411470817.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-21
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing methods of improving the resistivity of neodymium iron boron magnets will affect magnetic performance, or they may be complex in operation and not easy to mass production, and there is uneven coating of high-resistivity substances, which will affect the density of magnets.

Method used

The high resistivity auxiliary alloy Pr1-x-y-zAlxCuy(InGa)z is used to cover the surface of the NdFeB magnet matrix by magnetron sputtering, and grain boundary diffusion and tempering are carried out to form a continuous and uniform praseodymium-rich phase thin layer to improve crystallization boundary resistivity.

Benefits of technology

The resistivity and high-temperature performance of neodymium iron boron magnets are significantly improved. The maximum working temperature of the magnet can be increased by 20-50℃ without affecting the magnetic performance, avoiding the problem of performance degradation in traditional methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069247A_ABST
    Figure CN119069247A_ABST
Patent Text Reader

Abstract

The invention discloses a high-resistivity sintered neodymium-iron-boron magnet which is prepared according to the following method: sputtering a high-resistivity auxiliary alloy diffusion source on the surface of a neodymium-iron-boron magnet matrix, then performing grain boundary diffusion, cooling and tempering to obtain the high-resistivity sintered neodymium-iron-boron magnet, the component of the high-resistivity auxiliary alloy diffusion source is Pr < 1-x-y-z > Al < x > Cu < y > (InGa) < z >; wherein x is equal to 0.05 to 0.1, y is equal to 0.10 to 0.15, and z is equal to 0.10 to 0.15. The method of grain boundary diffusion after magnetron sputtering of the high-resistivity auxiliary alloy is adopted, the Pr content is increased, and the high-resistivity praseodymium-rich oxide phase continuously distributed on the grain boundary is formed by utilizing the characteristic that the Pr element is extremely oxygen-loving, so that the resistivity of the magnet is increased by 50% or above compared with that before treatment, and the performance of the magnet cannot be reduced; on the contrary, the intrinsic characteristics of the magnet are effectively improved, the high-temperature performance is remarkably improved, and great application value is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a high-resistivity sintered NdFeB magnet and a preparation method thereof. Background Art

[0002] Neodymium iron boron (RTB) rare earth permanent magnet is a permanent magnet material with excellent magnetic properties. Compared with other permanent magnet materials, it has the highest magnetic energy product and is widely used in modern industry. The high magnetic energy product of RTB rare earth magnets can effectively realize the miniaturization of equipment, so it has gradually replaced other permanent magnet materials in the field of electric motors.

[0003] When RTB magnets work in an alternating magnetic field, the alternating magnetic field will generate eddy currents in the magnets, which will induce Joule heat, and then cause the temperature of the magnets to rise during operation. Since the temperature coefficient of the magnetic properties of RTB magnets is negative, the magnetic properties will gradually decrease as the temperature of the magnets increases. Therefore, in engineering practice, certain methods need to be used to reduce the intensity of the induced eddy currents of the magnets and reduce the heating of the magnets.

[0004] Improving the resistivity of NdFeB magnets is an effective way to solve the eddy current effect generated during operation.

[0005] At present, the methods to improve the resistivity of NdFeB mainly include doping, coating with high resistivity materials, and adding high resistivity inorganic substances in stages.

[0006] However, there are still some problems in the existing solutions. For example, the introduction of dopants affects the grain boundary structure and reduces the magnetic properties of the magnet. Commonly used additives are high-resistivity materials such as oxides and fluorides. Although they can increase the resistivity, they introduce a large amount of non-magnetic materials, causing the magnetic properties of the magnet to deteriorate, including coercive force and magnetic energy product.

[0007] The segmented addition of high-resistivity materials greatly increases the resistivity of the magnet without reducing the magnetic properties, but the operation is complicated and not easy to mass produce; the coating of high-resistivity materials increases the resistivity of the magnet, but there is usually uneven coating, which affects the density of the magnet.

[0008] Therefore, it is necessary to develop a simple, efficient and low-cost method to prepare high resistivity sintered NdFeB magnets without affecting the magnetic properties. Summary of the invention

[0009] The purpose of the present invention is to provide a high resistivity sintered NdFeB magnet, which can suppress eddy current induction in an alternating magnetic field and improve the performance of the magnet.

[0010] The technical solution adopted by the present invention is: A high resistivity sintered NdFeB magnet is prepared by the following method: The high resistivity sintered NdFeB magnet is obtained by sputtering a high resistivity auxiliary alloy diffusion source on the surface of the NdFeB magnet matrix, then performing grain boundary diffusion, and then performing tempering treatment after cooling; The composition of the high resistivity auxiliary alloy diffusion source is: Pr 1-x-y-z Al x Cu y (InGa) z ; Among them, x=0.05~0.1, y=0.10~0.15, z=0.10~0.15; InGa represents one or both of In and Ga, the contents of In and Ga may be different, and the total content of In and Ga is x.

[0011] The preferred composition of the high resistivity auxiliary alloy diffusion source is Pr 1-x-y-z Al x Cu y Ga z .

[0012] Furthermore, the addition amount of the high resistivity auxiliary alloy diffusion source is 0.5-3% of the mass of the NdFeB magnet matrix, preferably 0.5-1.5%.

[0013] Furthermore, the high resistivity auxiliary alloy diffusion source is covered on the surface of the NdFeB magnet substrate by magnetron sputtering, and the NdFeB magnet substrate is a magnetic sheet with a thickness of 2-10 mm obtained by machining.

[0014] The surface of the NdFeB magnet substrate can be any one or more surfaces of the magnet. Preferably, the sputtering is performed on two surfaces of the NdFeB magnet substrate perpendicular to the orientation direction, but the method of the present invention is also applicable to sputtering the high resistivity auxiliary alloy diffusion source on other surfaces.

[0015] Furthermore, in the high resistivity auxiliary alloy diffusion source, the total mass content of low melting point elements such as Al, Cu, In and Ga is not less than 25wt%.

[0016] Furthermore, the melting point of the high resistivity auxiliary alloy diffusion source is 600-770°C.

[0017] The temperature of the grain boundary diffusion is 620-770° C., and the time is 3-10 hours.

[0018] The temperature of grain boundary diffusion is not lower than the melting point of the high resistivity auxiliary alloy diffusion source.

[0019] The tempering treatment temperature is 400-540° C., and the holding time is 2-4 h.

[0020] Grain boundary diffusion and tempering treatment are generally carried out under vacuum with an absolute pressure of less than 0.01 Pa.

[0021] Furthermore, the NdFeB magnet matrix may adopt a conventional magnet formula.

[0022] In a preferred embodiment, the composition of the NdFeB magnet matrix is ​​Re a M b (CoFe) bal B c The following components are preferably included in mass fraction: Re: 29-32wt%; Re is one or more of PrNd, Y, La, Ce, Ho, Gd, Dy, and Tb; PrNd refers to a commercially available national standard PrNd praseodymium-neodymium alloy metal having a Pr:Nd mass ratio of 25:75 or 20:80.

[0023] In Re, the total mass fraction of PrNd, Y, La, Ce, Ho, and Gd accounts for 27-30% of the magnet, that is, Re can contain no Dy or Tb; The total mass fraction of PrNd is more than 15% of the magnet; More preferably, Re contains one or two of La and Ce, and the total mass fraction of La and Ce is more than 7% of the magnet; Furthermore, the total content of Dy and Tb in Re is 0 to 3% of the magnet, and Re may not contain Dy or Tb.

[0024] M: 0.5-3wt%; M is one or more of Al, Cu, Ga, Zr, Nb, Ti, V, Cr, and Ni; B: 0.88-0.94wt%; The remainder is T and other unavoidable impurities, T is Fe and Co; the content of Co is 0.1~2% of the mass of the magnet.

[0025] In the present invention, it is preferred that the NdFeB magnet matrix contains a relatively low total amount of rare earth in the main phase, which is conducive to a greater role of the high resistivity auxiliary alloy.

[0026] The NdFeB magnet matrix can be prepared by conventional methods. Specifically, raw materials are taken according to the composition ratio, smelted, and spun to obtain SC sheets, which are then hydrogen crushed and air flow ground to obtain magnetic powder. The magnetic powder is prepared through orientation molding, isostatic pressing, vacuum sintering and heat treatment to obtain a NdFeB bulk magnet matrix, and then the magnetic sheets with a thickness of 2-10 mm are machined to serve as the NdFeB magnet matrix.

[0027] The high resistivity sintered NdFeB magnet prepared by the present invention has 7-11% volume fraction of praseodymium-rich phase, Pr6(FeM)14 (part of which is Pr6Fe13Ga phase), Pr5(InGa)3, and praseodymium-rich region between main phase crystals and in the corner region. A continuous and uniformly distributed 15nm praseodymium-rich phase thin layer is formed between main phase grains, which effectively isolates the main phase grains, prevents magnetic coupling of the main phase grains, and greatly improves the resistivity of the grain boundary.

[0028] The invention uses a high-resistivity auxiliary alloy diffusion source to perform magnetron sputtering and then grain boundary diffusion to obtain a high-resistivity sintered NdFeB magnet. Since the high-resistivity auxiliary alloy contains Pr, the Pr content in the high-resistivity sintered NdFeB magnet is increased by 4-30% compared with the Pr content in the NdFeB magnet matrix. The present invention utilizes the characteristic that the Pr element is more inclined to stay at the grain boundary, so that Pr and Cu, Al, In, and Ga diffused into the grain boundary together form a new grain boundary phase structure; and the Pr element is very oxygen-friendly, and it takes away the oxygen of the neodymium-rich phase in the magnet to form a praseodymium-rich praseodymium-based oxide phase (referred to as the praseodymium-rich phase), so that the main phase grains are effectively isolated by a continuous and uniformly distributed 15nm thick praseodymium-rich phase thin layer, which not only effectively prevents the magnetic coupling of the main phase grains, but also greatly improves the resistivity of the grain boundary. The resistivity of the magnet is increased by more than 50% compared with the neodymium iron boron magnet matrix before treatment, and the high-temperature performance of the magnet is significantly improved. After being installed in the motor, the maximum operating temperature can be increased by 20-50°C.

[0029] Moreover, compared with the NdFeB magnet matrix before treatment, the oxygen content of the prepared high resistivity sintered NdFeB magnet increases by no more than 200ppm, and the intrinsic coercive force of the magnet increases by more than 2KOe compared with the NdFeB magnet matrix before treatment.

[0030] The present invention adopts high resistivity auxiliary alloy Pr 1-x-y-z Al x Cu y (InGa) z The method of grain boundary diffusion after magnetron sputtering increases the Pr content and significantly improves the resistivity. It also avoids the impact of traditional additions of high-resistivity oxides on the performance of the magnet, effectively improving the intrinsic properties of the magnet. The high-temperature performance of high-resistivity sintered NdFeB magnets is significantly improved, which has great application value. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 Schematic diagram of the intergranular structure of high resistivity sintered NdFeB magnets.

[0032] Figure 2 This is a backscattered electron microscope photograph of the high resistivity sintered NdFeB magnet prepared in Example 1 and a composition analysis EDS analysis result diagram. DETAILED DESCRIPTION

[0033] The technical solution of the present invention is further described below in conjunction with specific embodiments, but the protection scope of the present invention is not limited thereto.

[0034] Preparation of main phase sintered NdFeB matrix magnet: Melting: weigh and mix the industrial pure metal raw materials according to the mass percentage of the sintered high resistivity auxiliary alloy and main phase alloy components, and use a vacuum rapid solidification melting furnace to rapidly quench the target raw materials into high resistivity auxiliary alloy ingots and main phase alloy flakes respectively; Main phase alloy hydrogen crushing: The main phase alloy flakes are crushed by oxygen-free hydrogen process to obtain main phase alloy coarse powder; Airflow milling of main phase alloy: The coarse powder of NdFeB main phase alloy is milled by nitrogen flow to obtain fine powder of NdFeB main phase alloy; additives such as antioxidants can be added.

[0035] Orientation molding: The main phase alloy powder is subjected to oxygen-free orientation molding under nitrogen protection and magnetic field to obtain NdFeB compacts; Sintering and tempering: After the NdFeB compact is pressurelessly sintered, it is cooled to obtain the main phase sintered NdFeB matrix magnet; Machining of substrate magnetic sheets: The main phase sintered NdFeB bulk magnet is machined to obtain magnetic sheets with a thickness of 2-10 mm, which serve as the sintered NdFeB substrate.

[0036] Preparation of high resistivity sintered NdFeB magnets: High resistivity auxiliary alloy smelting: weigh and mix the industrial pure metal raw materials according to the mass percentage of sintered NdFeB high resistivity auxiliary alloy, and cast the target raw materials into high resistivity auxiliary alloy ingots in a vacuum rapid solidification smelting furnace; Preparation of high resistivity auxiliary alloy target: The high resistivity sintered NdFeB auxiliary alloy ingot is forged to make a target of specified specifications.

[0037] Preparation of high resistivity sintered NdFeB magnets: magnetron sputtering is performed on the sintered NdFeB matrix magnet sheets, and the addition amount of high resistivity auxiliary alloy magnetron sputtering is 0.5-3%wt by mass percentage; Grain boundary diffusion and tempering: Grain boundary diffusion and tempering are carried out on the base magnetic sheet with high resistivity auxiliary alloy sputtered by magnetron to obtain high resistivity sintered NdFeB magnets.

[0038] Example 1 The preparation method is as follows: 1) Smelting of high resistivity auxiliary alloy: weighing and mixing the raw materials according to the mass percentage of high resistivity auxiliary alloy, smelting, and casting into high resistivity auxiliary alloy ingots; The composition mass percentage of the high resistivity auxiliary alloy in this embodiment is Pr 1-x-y-z Al x Cu y (InGa) z; Among them, Pr is 70wt%, Al is 5wt%, Cu is 10wt%, Ga is 15wt%, and In is 0%.

[0039] 2) Preparation of high resistivity auxiliary alloy target: Forge and machine the high resistivity sintered NdFeB auxiliary alloy ingot to make a target of specified specifications; 3) Preparation of NdFeB magnet matrix: Using the same formula as in Comparative Example 3, the mass percentage is (PrNd) a M b (CoFe) bal B c Make batching; The content of PrNd is a=30wt%, wherein PrNd is selected from a commercially available national standard praseodymium-neodymium alloy metal with a mass percentage ratio of Pr to Nd of 1:3, that is, a commercially available national standard PrNd praseodymium-neodymium alloy metal with a purity of 99%, that is, Pr is 7.425wt% and Nd is 22.275wt%; The content of M is b=0.73wt%, and M is Al, Cu, Ga, and Zr, with contents of 0.13wt%, 0.15wt%, 0.15wt%, and 0.3wt%, respectively.

[0040] The content of B is c=0.94wt%; the rest is CoFe, of which Co is 0.5wt%.

[0041] Melting: weigh and mix the industrial pure metal raw materials according to the alloy composition in mass percentage, and use a vacuum rapid solidification melting furnace to rapidly quench the target raw materials to obtain NdFeB alloy castings; Hydrogen crushing: The NdFeB alloy castings are crushed by hydrogen crushing furnace to obtain NdFeB coarse powder; Airflow milling: After the coarse powder is stirred and mixed, it is further ground with a fluidized bed airflow mill. No oxygen is added during the airflow milling to grind the coarse powder into fine NdFeB powder. Antioxidants are added to the obtained NdFeB fine powder and mixed evenly. Orientation molding: The alloy powder is oriented and molded in a magnetic field under nitrogen protection to obtain a compact; Sintering and tempering: After vacuum sintering and tempering, the pressed green sheet is cooled to obtain sintered NdFeB blanks with specifications of 55*45*35 squares.

[0042] The sintered NdFeB blank is a 55*45*35 square block. After machining, each blank magnet can be processed into 10 magnetic sheets with a size of 55*45*3mm. 4) For the sintered NdFeB magnet matrix magnetic sheet with a specification of 55*45*3, magnetron sputtering is performed using the high resistivity auxiliary alloy target material in step 2), and the addition amount of the high resistivity auxiliary alloy diffusion source is 0.5%wt of the mass of the NdFeB magnet matrix magnetic sheet; 5) Grain boundary diffusion and tempering: The 55*45*3 sintered NdFeB matrix magnet sheet with high resistivity auxiliary alloy that has been magnetron sputtered is subjected to grain boundary diffusion at 720°C for 8 hours. Then it is tempered at 500°C for 4 hours to obtain a high resistivity sintered NdFeB magnet.

[0043] 6) For the high resistivity sintered NdFeB magnet samples, the magnetic properties, magnet oxygen content, resistivity test, magnet composition test, installed overload aging and demagnetization test and other tests are carried out.

[0044] Example 2 The preparation method is as follows: 1) Smelting of high resistivity auxiliary alloy: weighing and mixing the raw materials according to the mass percentage of high resistivity auxiliary alloy, smelting, and casting into high resistivity auxiliary alloy ingots; The composition mass percentage of the high resistivity auxiliary alloy in this embodiment is Pr 1-x-y-z Al x Cu y (InGa) z ; Among them, Pr is 70wt%, Al is 5wt%, Cu is 10wt%, Ga is 10wt%, and In is 5%.

[0045] 2) Preparation of high resistivity auxiliary alloy target: Forge and machine the high resistivity sintered NdFeB auxiliary alloy ingot to make a target of specified specifications; 3) Preparation of NdFeB magnet matrix: Using the same formula as in Comparative Example 3, the mass percentage is (PrNd) a M b (CoFe) bal B c Make batching; The content of PrNd is a=30wt%, wherein PrNd is selected from a commercially available national standard praseodymium-neodymium alloy metal with a mass percentage ratio of Pr to Nd of 1:3, that is, a commercially available national standard PrNd praseodymium-neodymium alloy metal with a purity of 99%, that is, Pr is 7.425wt% and Nd is 22.275wt%; The content of M is b=0.73wt%, and M is Al, Cu, Ga, and Zr, with contents of 0.13wt%, 0.15wt%, 0.15wt%, and 0.3wt%, respectively.

[0046] The content of B is c=0.94wt%; the rest is CoFe, of which Co is 0.5wt%.

[0047] Melting: weigh and mix the industrial pure metal raw materials according to the alloy composition in mass percentage, and use a vacuum rapid solidification melting furnace to rapidly quench the target raw materials to obtain NdFeB alloy castings; Hydrogen crushing: The NdFeB alloy castings are crushed by hydrogen crushing furnace to obtain NdFeB coarse powder; Airflow milling: After the coarse powder is stirred and mixed, it is further ground with a fluidized bed airflow mill. No oxygen is added during the airflow milling to grind the coarse powder into fine NdFeB powder. Antioxidants are added to the obtained NdFeB fine powder and mixed evenly. Orientation molding: The alloy powder is oriented and molded in a magnetic field under nitrogen protection to obtain a compact; Sintering and tempering: After vacuum sintering and tempering, the pressed green sheet is cooled to obtain sintered NdFeB blanks with specifications of 55*45*35 squares.

[0048] The sintered NdFeB blank is a 55*45*35 square block. After machining, each blank magnet can be processed into 10 magnetic sheets with a size of 55*45*3mm. 4) For the sintered NdFeB magnet matrix magnetic sheet with a specification of 55*45*3, magnetron sputtering is performed using the high resistivity auxiliary alloy target material in step 2), and the addition amount of the high resistivity auxiliary alloy diffusion source is 0.5%wt of the mass of the NdFeB magnet matrix magnetic sheet; 5) Grain boundary diffusion and tempering: The 55*45*3 sintered NdFeB matrix magnet sheet with high resistivity auxiliary alloy that has been magnetron sputtered is subjected to grain boundary diffusion at 720°C for 8 hours. Then it is tempered at 500°C for 4 hours to obtain a high resistivity sintered NdFeB magnet.

[0049] 6) For the high resistivity sintered NdFeB magnet samples, the magnetic properties, magnet oxygen content, resistivity test, magnet composition test, installed overload aging and demagnetization test and other tests are carried out.

[0050] Comparative Example 1 The preparation method is as follows: 1) Smelting of high resistivity auxiliary alloy: weighing and mixing the raw materials according to the mass percentage of high resistivity auxiliary alloy, smelting, and casting into high resistivity auxiliary alloy ingots; The composition mass percentage of the high resistivity auxiliary alloy in this embodiment is Pr 1-x-y-z Al x Cu y (InGa) z ; Among them, Pr is 80wt%, Al is 10wt%, Cu is 10wt%, Ga is 0wt%, and In is 0%.

[0051] 2) Preparation of high resistivity auxiliary alloy target: Forge and machine the high resistivity sintered NdFeB auxiliary alloy ingot to make a target of specified specifications; 3) Preparation of NdFeB magnet matrix: Using the same formula as in Comparative Example 3, the mass percentage is (PrNd) a M b (CoFe) bal B c Make batching; The content of PrNd is a=30wt%, wherein PrNd is selected from a commercially available national standard praseodymium-neodymium alloy metal with a mass percentage ratio of Pr to Nd of 1:3, that is, a commercially available national standard PrNd praseodymium-neodymium alloy metal with a purity of 99%, that is, Pr is 7.425wt% and Nd is 22.275wt%; The content of M is b=0.73wt%, and M is Al, Cu, Ga, and Zr, with contents of 0.13wt%, 0.15wt%, 0.15wt%, and 0.3wt%, respectively.

[0052] The content of B is c=0.94wt%; the rest is CoFe, of which Co is 0.5wt%.

[0053] Melting: weigh and mix the industrial pure metal raw materials according to the alloy composition in mass percentage, and use a vacuum rapid solidification melting furnace to rapidly quench the target raw materials to obtain NdFeB alloy castings; Hydrogen crushing: The NdFeB alloy castings are crushed by hydrogen crushing furnace to obtain NdFeB coarse powder; Airflow milling: After the coarse powder is stirred and mixed, it is further ground with a fluidized bed airflow mill. No oxygen is added during the airflow milling to grind the coarse powder into fine NdFeB powder. Antioxidants are added to the obtained NdFeB fine powder and mixed evenly. Orientation molding: The alloy powder is oriented and molded in a magnetic field under nitrogen protection to obtain a compact; Sintering and tempering: After vacuum sintering and tempering, the pressed green sheet is cooled to obtain sintered NdFeB blanks with specifications of 55*45*35 squares.

[0054] The sintered NdFeB blank is a 55*45*35 square block. After machining, each blank magnet can be processed into 10 magnetic sheets with a size of 55*45*3mm. 4) For the sintered NdFeB magnet matrix magnetic sheet with a specification of 55*45*3, magnetron sputtering is performed using the high resistivity auxiliary alloy target material in step 2), and the addition amount of the high resistivity auxiliary alloy diffusion source is 0.5%wt of the mass of the NdFeB magnet matrix magnetic sheet; 5) Grain boundary diffusion and tempering: The 55*45*3 sintered NdFeB matrix magnet sheet with high resistivity auxiliary alloy that has been magnetron sputtered is subjected to grain boundary diffusion at 750°C for 8 hours. Then, it is tempered at 500°C for 4 hours to obtain a high resistivity sintered NdFeB magnet.

[0055] 6) For the high resistivity sintered NdFeB magnet samples, the magnetic properties, magnet oxygen content, resistivity test, magnet composition test, installed overload aging and demagnetization test and other tests are carried out.

[0056] Comparative Example 2 The preparation method is as follows: 1) Smelting of high resistivity auxiliary alloy: weighing and mixing the raw materials according to the mass percentage of high resistivity auxiliary alloy, smelting, and casting into high resistivity auxiliary alloy ingots; The composition mass percentage of the high resistivity auxiliary alloy in this embodiment is Pr 1-x-y-z Al x Cu y (InGa) z ; Among them, Pr is 85wt%, Al is 0wt%, Cu is 15wt%, Ga is 0wt%, and In is 0%.

[0057] 2) Preparation of high resistivity auxiliary alloy target: Forge and machine the high resistivity sintered NdFeB auxiliary alloy ingot to make a target of specified specifications; 3) Preparation of NdFeB magnet matrix: Using the same formula as in Comparative Example 3, the mass percentage is (PrNd) a M b (CoFe) bal B c Make batching; The content of PrNd is a=30wt%, wherein PrNd is selected from a commercially available national standard praseodymium-neodymium alloy metal with a mass percentage ratio of Pr to Nd of 1:3, that is, a commercially available national standard PrNd praseodymium-neodymium alloy metal with a purity of 99%, that is, Pr is 7.425wt% and Nd is 22.275wt%; The content of M is b=0.73wt%, and M is Al, Cu, Ga, and Zr, with contents of 0.13wt%, 0.15wt%, 0.15wt%, and 0.3wt%, respectively.

[0058] The content of B is c=0.94wt%; the rest is CoFe, of which Co is 0.5wt%.

[0059] Melting: weigh and mix the industrial pure metal raw materials according to the alloy composition in mass percentage, and use a vacuum rapid solidification melting furnace to rapidly quench the target raw materials to obtain NdFeB alloy castings; Hydrogen crushing: The NdFeB alloy castings are crushed by hydrogen crushing furnace to obtain NdFeB coarse powder; Airflow milling: After the coarse powder is stirred and mixed, it is further ground with a fluidized bed airflow mill. No oxygen is added during the airflow milling to grind the coarse powder into fine NdFeB powder. Antioxidants are added to the obtained NdFeB fine powder and mixed evenly. Orientation molding: The alloy powder is oriented and molded in a magnetic field under nitrogen protection to obtain a compact; Sintering and tempering: After vacuum sintering and tempering, the pressed green sheet is cooled to obtain sintered NdFeB blanks with specifications of 55*45*35 squares.

[0060] The sintered NdFeB blank is a 55*45*35 square block. After machining, each blank magnet can be processed into 10 magnetic sheets with a size of 55*45*3mm. 4) For the sintered NdFeB magnet matrix magnetic sheet with a specification of 55*45*3, magnetron sputtering is performed using the high resistivity auxiliary alloy target material in step 2), and the addition amount of the high resistivity auxiliary alloy diffusion source is 0.5%wt of the mass of the NdFeB magnet matrix magnetic sheet; 5) Grain boundary diffusion and tempering: The 55*45*3 sintered NdFeB matrix magnet sheet with high resistivity auxiliary alloy that has been magnetron sputtered is subjected to grain boundary diffusion at 750°C for 8 hours. Then, it is tempered at 500°C for 4 hours to obtain a high resistivity sintered NdFeB magnet.

[0061] 6) For the high resistivity sintered NdFeB magnet samples, the magnetic properties, magnet oxygen content, resistivity test, magnet composition test, installed overload aging and demagnetization test and other tests are carried out.

[0062] Comparative Example 3 1) PrNd by mass percentage a M b (CoFe) bal B c Make batching; The content of PrNd is a=30wt%, wherein PrNd is selected from a commercially available national standard praseodymium-neodymium alloy metal with a mass percentage ratio of Pr to Nd of 1:3, that is, a commercially available national standard PrNd praseodymium-neodymium alloy metal with a purity of 99%, that is, Pr is 7.425wt% and Nd is 22.275wt%; The content of M is b=0.73wt%, and M is Al, Cu, Ga, and Zr, with contents of 0.13wt%, 0.15wt%, 0.15wt%, and 0.3wt%, respectively.

[0063] The content of B is c=0.94wt%; the rest is CoFe, of which Co is 0.5wt%.

[0064] 2) Melting: weigh and mix the industrial pure metal raw materials according to the NdFeB alloy composition by mass percentage, and use a vacuum rapid solidification melting furnace to rapidly quench the target raw materials to obtain NdFeB alloy castings; 3) Hydrogen crushing: The NdFeB alloy castings are crushed by hydrogen in a hydrogen crushing furnace to obtain NdFeB coarse powder; 4) Airflow milling: After the coarse powder is stirred and mixed, it is further ground with a fluidized bed airflow mill. No oxygen is added during the airflow milling to grind the coarse powder into fine NdFeB powder. Antioxidants are added to the obtained NdFeB fine powder and mixed evenly. 5) Orientation molding: The alloy powder is oriented and molded in a magnetic field under nitrogen protection to obtain a compact; 6) Sintering and tempering: After vacuum sintering and tempering, the pressed green sheet is cooled to obtain a sintered NdFeB blank with a specification of 55*45*35.

[0065] 6) Process the blank into suitable samples and conduct tests on the magnetic properties, oxygen content, resistivity, composition, high temperature aging and demagnetization, and installed overload aging and demagnetization of the magnet.

[0066] A permanent magnet measuring instrument, a German ELTRA oxygen-hydrogen analyzer, a metal resistivity detector, an inductively coupled plasma mass spectrometer, a high temperature aging box, and a permanent magnet motor dynamometer were used to perform tests on the magnetic properties, oxygen content, resistivity, magnet composition, high temperature aging and demagnetization of the magnet, and high temperature overload aging and demagnetization of the installed machine. The test results of Example 1 and Comparative Example 3 are compared as shown in Table 1 below: Table 1 Compare project names Example 1 Comparative Example 3 The percentage change between Example 1 and Comparative Example 3 Pr(wt%) 7.775 7.425 ↑4.7% Nd(wt%) 22.275 22.275 - Al(wt%) 0.155 0.13 ↑19.2% Cu(wt%) 0.2 0.15 ↑33.3% Ga(wt%) 0.225 0.15 ↑50% In(wt%) 0 0 / Zr(wt%) 0.3 0.3 / Co(wt%) 0.5 0.5 / B(wt%) 0.94 0.94 / Br(KGs) 14.4 14.55 ↓1% Hcj(KOe) 17.75 15.7 ↑13.31% (BH)max(MGOe) 50.8 51.3 ↓1% Hk / Hcj(%) 99.5 97.8 ↑1.7% Oxygen content (ppm) 705 650 ↑8.5% Resistivity(uΩm) 2.25 1.46 ↑54.1% High temperature aging and demagnetization of magnets 100℃ open circuit for 2 hours, irreversible magnetic flux loss 1.2-3.5% 80℃ open circuit for 2 hours, irreversible loss of magnetic flux 3-5.5% / Installed high temperature overload aging demagnetization test After 150℃ closed circuit high current impact overload test, the irreversible loss of magnetic flux is 2.5-4.1% After 120℃ closed circuit high current impact overload test, the irreversible loss of magnetic flux is 4.2-7.7% / From the comparison in Table 1, it can be seen that in Example 1, high resistivity auxiliary alloy Pr is magnetron sputtered on a substrate having the same magnet composition as that of Comparative Example 3. 1-x-y-z Al x Cu y (InGa) z After that, grain boundary diffusion is carried out, and the resistivity of the obtained magnet is increased by more than 50%, which significantly improves the working performance of the magnet at high temperature, and the maximum working temperature can be increased by 20-50℃.

[0067] The magnet of Example 1 was subjected to backscatter electron microscopy and composition analysis EDS analysis and found that (such as Figure 2 As shown in the figure, the Pr element is more inclined to stay at the grain boundary through the diffusion of high resistivity auxiliary alloys at the grain boundary, so that Pr and Cu, Al, In, and Ga diffused into the grain boundary together form a new grain boundary phase; and the Pr element is very oxygen-friendly, which takes away the oxygen in the original magnet and the oxygen added during the grain boundary diffusion, forming a praseodymium-rich praseodymium-based oxide phase (referred to as praseodymium-rich phase), so that the main phase grains are effectively isolated by the continuous and uniformly distributed 15nm praseodymium-rich phase thin layer, which not only effectively prevents the magnetic coupling of the main phase grains, but also greatly improves the resistivity of the grain boundary. It not only avoids the influence of the traditional addition of high resistivity oxides on the performance of the magnet, but also effectively improves the intrinsic properties of the magnet.

[0068] A permanent magnet measuring instrument, a German ELTRA oxygen and hydrogen analyzer, a metal resistivity detector, an inductively coupled plasma mass spectrometer, a high temperature aging box, and a permanent magnet motor dynamometer are used to test the magnetic properties, oxygen content, resistivity, magnet composition, high temperature aging and demagnetization of magnets, and high temperature overload aging and demagnetization of installed machines. Examples 1 and 2 and Comparative Examples 1 and 2 all use the same NdFeB matrix magnet, with only the high resistivity auxiliary alloy composition being different. The test results of Examples 1 and 2 and Comparative Examples 1 and 2 are compared as shown in Table 2 below: Table 2 Compare project names Example 1 Example 2 Comparative Example 1 Comparative Example 2 Comparative Example 3 Pr(wt%) 7.775 7.775 7.825 7.85 7.425 Nd(wt%) 22.275 22.275 22.275 22.275 22.275 Al(wt%) 0.155 0.155 0.18 0.13 0.13 Cu(wt%) 0.2 0.2 0.2 0.225 0.15 Ga(wt%) 0.225 0.2 0.15 0.15 0.15 In(wt%) 0 0.025 0 0 0 Zr(wt%) 0.3 0.3 0.3 0.3 0.3 Co(wt%) 0.5 0.5 0.5 0.5 0.5 B(wt%) 0.94 0.94 0.94 0.94 0.94 Br(KGs) 14.4 14.41 14.51 14.52 14.55 Hcj(KOe) 17.75 17.15 16.65 16.85 15.7 (BH)max(MGOe) 50.8 50.9 51 51.2 51.3 Hk / Hcj(%) 99.5 99.5 98.5 99.3 97.8 Oxygen content (ppm) 705 720 740 732 650 Resistivity(uΩm) 2.25 2.23 2.26 2.28 1.46 High temperature aging and demagnetization of magnets 100℃ open circuit for 2 hours, irreversible flux loss 1.2-3.5% 100℃ open circuit for 2 hours, irreversible flux loss 2.7-4.2% 100℃ open circuit for 2 hours, irreversible magnetic flux loss 4.2-6.3% 100℃ open circuit for 2 hours, irreversible magnetic flux loss 4.1-5.5% 80℃ open circuit for 2 hours, irreversible loss of magnetic flux 3-5.5% Installed high temperature overload aging demagnetization test After 150℃ closed circuit high current impact high temperature overload test, the irreversible loss of magnetic flux is 2.5-4.1% After 140℃ closed circuit high current impact overload test, the irreversible loss of magnetic flux is 3.2-5.4% After 140℃ closed circuit high current impact high temperature overload test, the irreversible loss of magnetic flux is 5.2-7.8% After 140℃ closed circuit high current impact high temperature overload test, the irreversible loss of magnetic flux is 4.7-6.5% After 120℃ closed circuit high current impact overload test, the irreversible loss of magnetic flux is 4.2-7.7% From the comparison between Example 1 and Example 2, it can be seen that Example 2 adds In element, while Example 1 does not add In element. The resistivity improvement of Example 2 and Example 1 is similar, but the intrinsic coercivity improvement of Example 2 is lower. The high resistivity auxiliary alloy of Comparative Example 1 does not contain In and Ga, that is, z=0, which is not within the scope of the present invention. The total mass content of low melting point Al, Cu, In, and Ga elements is 20%, which is also lower than 25wt% defined in the present invention. The high resistivity auxiliary alloy of Comparative Example 2 does not contain Al, In, and Ga, that is, x=0, z=0, which is not within the scope of the present invention. The total mass content of low melting point Al, Cu, In, and Ga elements is 15%, which is also lower than 25wt% defined in the present invention. The base magnet components of Examples 1 and 2 are exactly the same as those of Comparative Examples 1, 2, and 3, except that the components of the high resistivity auxiliary alloy are different. From the above comparison results, it can be seen that on the same NdFeB matrix magnetic sheet, by diffusing high-resistivity auxiliary alloys of different components at the grain boundaries, that is, adjusting the components of Al, Cu, and Ga, the effect on the resistivity does not change much, and all have a relatively good effect of improving the resistivity, but the change in composition has a greater impact on the increase in the intrinsic coercivity, and the high-temperature performance of the magnet (aging demagnetization and overload aging demagnetization) is lower than that of Example 1. Under the same conditions, the diffusion temperature of the high-resistivity auxiliary alloy containing Ga can be lower, and the increase in intrinsic coercivity is also higher. If Ga is not contained in the high-resistivity auxiliary alloy, it is not conducive to lowering the melting point of the high-resistivity auxiliary alloy, so that the diffusion temperature of the high-resistivity auxiliary alloy is increased, and it is difficult to achieve low-temperature diffusion. It has little effect on the resistivity and intrinsic coercivity improvement of conventional sintered NdFeB magnets that do not contain high-abundance rare earths, and has no effect on the increase in the resistivity of sintered NdFeB magnets substituted with high-abundance rare earths, but it is not conducive to improving the intrinsic coercivity of sintered NdFeB magnets substituted with high-abundance rare earths. Therefore, the values ​​of x, y, and z need to be within the limited range of the present invention.

[0069] Example 3 The preparation method is as follows: 1) Smelting of high resistivity auxiliary alloy: weighing and mixing the raw materials according to the mass percentage of high resistivity auxiliary alloy, smelting, and casting into high resistivity auxiliary alloy ingots; The composition mass percentage of the high resistivity auxiliary alloy in this embodiment is Pr 1-x-y-z Al x Cu y (InGa) z ; Among them, Pr is 60wt%, Al is 10wt%, Cu is 15wt%, Ga is 15wt%, and In is 0%.

[0070] 2) Preparation of high resistivity auxiliary alloy target: Forge and machine the high resistivity sintered NdFeB auxiliary alloy ingot to make a target of specified specifications; 3) Preparation of NdFeB magnet matrix: using the same formula as in Comparative Example 4, Re by mass percentage a M b (CoFe) bal B c Make batching; The content of Re is a=31.8wt%, wherein Re is PrNd, Dy, and Ce, and the weight percentages are 23.3wt%, 1.5wt%, and 7wt% respectively, wherein PrNd is selected from a commercially available national standard praseodymium-neodymium alloy metal with a mass percentage ratio of Pr to Nd of 1:3, that is, a commercially available national standard PrNd praseodymium-neodymium alloy metal with a purity of 99%, that is, Pr is 5.767wt% and Nd is 17.533wt%; The content of M is b=1.2wt%, and M is Al, Cu, Ga, Ti, and Zr, with contents of 0.3wt%, 0.3wt%, 0.2wt%, 0.2wt%, and 0.2wt%, respectively.

[0071] The content of B is c=0.9wt%; the rest is CoFe, of which Co is 0.8wt%.

[0072] Melting: weigh and mix the industrial pure metal raw materials according to the alloy composition in mass percentage, and use a vacuum rapid solidification melting furnace to rapidly quench the target raw materials to obtain NdFeB alloy castings; Hydrogen crushing: The NdFeB alloy castings are crushed by hydrogen crushing furnace to obtain NdFeB coarse powder; Airflow milling: After the coarse powder is stirred and mixed, it is further ground with a fluidized bed airflow mill. No oxygen is added during the airflow milling to grind the coarse powder into fine NdFeB powder. Antioxidants are added to the obtained NdFeB fine powder and mixed evenly. Orientation molding: The alloy powder is oriented and molded in a magnetic field under nitrogen protection to obtain a compact; Sintering and tempering: After vacuum sintering and tempering, the pressed green sheet is cooled to obtain sintered NdFeB blanks with specifications of 55*45*35 squares.

[0073] The sintered NdFeB blank is a 55*45*35 square block. After machining, each blank magnet can be processed into 10 magnetic sheets with a size of 55*45*3mm. 4) For the sintered NdFeB magnet matrix magnetic sheet with a specification of 55*45*3, magnetron sputtering is performed using the high resistivity auxiliary alloy target material in step 2), and the addition amount of the high resistivity auxiliary alloy diffusion source is 0.5%wt of the mass of the NdFeB magnet matrix magnetic sheet; 5) Grain boundary diffusion and tempering: The 55*45*3 sintered NdFeB matrix magnet sheet with high resistivity auxiliary alloy that has been magnetron sputtered is subjected to grain boundary diffusion at 700℃ for 8 hours. Then it is tempered at 620℃ for 4 hours to obtain a high resistivity sintered NdFeB magnet.

[0074] 6) For the high resistivity sintered NdFeB magnet samples, the magnetic properties, magnet oxygen content, resistivity test, magnet composition test, installed overload aging and demagnetization test and other tests are carried out.

[0075] Comparative Example 4 1) Re by mass percentage a M b (CoFe) bal B c Make batching; The content of Re is a=31.8wt%, wherein Re is PrNd, Dy, and Ce, and the weight percentages are 23.3wt%, 1.5wt%, and 7wt% respectively, wherein PrNd is selected from a commercially available national standard praseodymium-neodymium alloy metal with a mass percentage ratio of Pr to Nd of 1:3, that is, a commercially available national standard PrNd praseodymium-neodymium alloy metal with a purity of 99%, that is, Pr is 5.767wt% and Nd is 17.533wt%; The content of M is b=1.2wt%, and M is Al, Cu, Ga, Ti, and Zr, with contents of 0.3wt%, 0.3wt%, 0.2wt%, 0.2wt%, and 0.2wt%, respectively.

[0076] The content of B is c=0.9wt%; the rest is CoFe, of which Co is 0.8wt%.

[0077] 2) Melting: weigh and mix the industrial pure metal raw materials according to the NdFeB alloy composition by mass percentage, and use a vacuum rapid solidification melting furnace to rapidly quench the target raw materials to obtain NdFeB alloy castings; 3) Hydrogen crushing: The NdFeB alloy castings are crushed by hydrogen in a hydrogen crushing furnace to obtain NdFeB coarse powder; 4) Airflow milling: After the coarse powder is stirred and mixed, it is further ground with a fluidized bed airflow mill. No oxygen is added during the airflow milling to grind the coarse powder into fine NdFeB powder. Antioxidants are added to the obtained NdFeB fine powder and mixed evenly. 5) Orientation molding: The alloy powder is oriented and molded in a magnetic field under nitrogen protection to obtain a compact; 6) Sintering and tempering: After vacuum sintering and tempering, the pressed green sheet is cooled to obtain a sintered NdFeB blank with a specification of 55*45*35.

[0078] 6) Process the blank into suitable samples and conduct tests on the magnetic properties, oxygen content, resistivity, composition, high temperature aging and demagnetization, and installed overload aging and demagnetization of the magnet.

[0079] A permanent magnet measuring instrument, a German ELTRA oxygen-hydrogen analyzer, a metal resistivity detector, an inductively coupled plasma mass spectrometer, a high temperature aging chamber, and a permanent magnet motor dynamometer were used to test the magnetic properties, oxygen content, resistivity, composition, high temperature aging and demagnetization of the magnet, and high temperature overload aging and demagnetization of the installed machine. The test results of Example 3 and Comparative Example 4 are compared as shown in Table 3 below: Table 3 Compare project names Example 3 Comparative Example 4 The percentage change between Example 3 and Comparative Example 4 Pr(wt%) 6.067 5.767 ↑5.2% Nd(wt%) 17.533 17.533 / Dy(wt%) 1.5 1.5 / Ce(wt%) 7 7 / Al(wt%) 0.35 0.3 ↑16.67% Cu(wt%) 0.375 0.3 ↑25% Ga(wt%) 0.275 0.2 ↑37.5% Ti(wt%) 0.2 0.2 / Zr(wt%) 0.2 0.2 / Co(wt%) 0.8 0.8 / B(wt%) 0.9 0.9 / Br(KGs) 12.55 12.7 ↓1.18% Hcj(KOe) 22.9 20.5 ↑11.7% (BH)max(MGOe) 38.9 39.3 ↓1% Hk / Hcj(%) 98.5 98 ↑0.5% Oxygen content (ppm) 725 680 ↑6.62% Resistivity(uΩm) 2.15 1.38 ↑55.8% High temperature aging and demagnetization of magnets 120℃ open circuit for 2 hours, irreversible magnetic flux loss 0.5-3.3% 100℃ open circuit for 2 hours, irreversible loss of magnetic flux 2-5.5% / Installed high temperature overload aging demagnetization test After 180℃ closed circuit high current impact overload test, the irreversible loss of magnetic flux is 1.5-4.7% After 150℃ closed circuit high current impact overload test, the irreversible loss of magnetic flux is 4.4-7.9% / From the comparison in Table 3, it can be seen that in Example 3, the high resistivity auxiliary alloy Pr is magnetron sputtered on a substrate having the same magnet composition as that of Comparative Example 4. 1-x-y-z Al x Cu y (InGa) z After that, grain boundary diffusion is carried out, and the resistivity of the obtained magnet is increased by more than 50%, which significantly improves the working performance of the magnet at high temperature, and the maximum working temperature can be increased by 20-50℃.

[0080] Comparative Example 5 1) Smelting of high resistivity auxiliary alloy: weighing and mixing the raw materials according to the mass percentage of high resistivity auxiliary alloy, smelting, and casting into high resistivity auxiliary alloy ingots; The composition mass percentage of the high resistivity auxiliary alloy in this embodiment is Pr 1-x-y-z Al x Cu y (InGa) z ; Among them, Pr is 70wt%, Al is 5wt%, Cu is 10wt%, Ga is 15wt%, and In is 0%.

[0081] 2) Preparation of high resistivity auxiliary alloy target: Forge and machine the high resistivity sintered NdFeB auxiliary alloy ingot to make a target of specified specifications; 3) Preparation of NdFeB magnet matrix: Using the same formula as in Comparative Example 3, the mass percentage is (PrNd) a M b (CoFe) bal B c Make batching; The content of PrNd is a=30wt%, wherein PrNd is selected from a commercially available national standard praseodymium-neodymium alloy metal with a mass percentage ratio of Pr to Nd of 1:3, that is, a commercially available national standard PrNd praseodymium-neodymium alloy metal with a purity of 99%, that is, Pr is 7.425wt% and Nd is 22.275wt%; The content of M is b=0.73wt%, and M is Al, Cu, Ga, and Zr, with contents of 0.13wt%, 0.15wt%, 0.15wt%, and 0.3wt%, respectively.

[0082] The content of B is c=0.94wt%; the rest is CoFe, of which Co is 0.5wt%.

[0083] Melting: weigh and mix the industrial pure metal raw materials according to the alloy composition in mass percentage, and use a vacuum rapid solidification melting furnace to rapidly quench the target raw materials to obtain NdFeB alloy castings; Hydrogen crushing: The NdFeB alloy castings are crushed by hydrogen crushing furnace to obtain NdFeB coarse powder; Airflow milling: After the coarse powder is stirred and mixed, it is further ground with a fluidized bed airflow mill. No oxygen is added during the airflow milling to grind the coarse powder into fine NdFeB powder. Antioxidants are added to the obtained NdFeB fine powder and mixed evenly. Orientation molding: The alloy powder is oriented and molded in a magnetic field under nitrogen protection to obtain a compact; Sintering and tempering: After vacuum sintering and tempering, the pressed green sheet is cooled to obtain sintered NdFeB blanks with specifications of 55*45*35 squares.

[0084] The sintered NdFeB blank is a 55*45*35 square block. After machining, each blank magnet can be processed into 10 magnetic sheets with a size of 55*45*3mm. 4) For the sintered NdFeB magnet matrix magnetic sheet with a specification of 55*45*3, magnetron sputtering is performed using the high resistivity auxiliary alloy target material in step 2), and the addition amount of the high resistivity auxiliary alloy diffusion source is 0.5%wt of the mass of the NdFeB magnet matrix magnetic sheet; 5) Grain boundary diffusion and tempering: The 55*45*3 sintered NdFeB matrix magnet sheet with high resistivity auxiliary alloy that has been magnetron sputtered is subjected to the commonly used 900℃ grain boundary diffusion for 8 hours. Then the tempering treatment is carried out at 500℃ for 4 hours to obtain a high resistivity sintered NdFeB magnet.

[0085] 6) For the high resistivity sintered NdFeB magnet samples, the magnetic properties, magnet oxygen content, resistivity test, magnet composition test, installed overload aging and demagnetization test and other tests are carried out.

[0086] Comparative Example 6 The preparation method is as follows: 1) Smelting of high resistivity auxiliary alloy: weighing and mixing the raw materials according to the mass percentage of high resistivity auxiliary alloy, smelting, and casting into high resistivity auxiliary alloy ingots; The composition mass percentage of the high resistivity auxiliary alloy in this embodiment is Pr 1-x-y-z Al x Cu y (InGa) z ; Among them, Pr is 60wt%, Al is 10wt%, Cu is 15wt%, Ga is 15wt%, and In is 0%.

[0087] Preparation of high resistivity auxiliary alloy target: Forge and machine the high resistivity sintered NdFeB auxiliary alloy ingot to make a target of specified specifications; 3) Preparation of NdFeB magnet matrix: using the same formula as in Comparative Example 4, Re by mass percentage a M b (CoFe) bal B c Make batching; The content of Re is a=31.8wt%, wherein Re is PrNd, Dy, and Ce, and the weight percentages are 23.3wt%, 1.5wt%, and 7wt% respectively, wherein PrNd is selected from a commercially available national standard praseodymium-neodymium alloy metal with a mass percentage ratio of Pr to Nd of 1:3, that is, a commercially available national standard PrNd praseodymium-neodymium alloy metal with a purity of 99%, that is, Pr is 5.767wt% and Nd is 17.533wt%; The content of M is b=1.2wt%, and M is Al, Cu, Ga, Ti, and Zr, with contents of 0.3wt%, 0.3wt%, 0.2wt%, 0.2wt%, and 0.2wt%, respectively.

[0088] The content of B is c=0.9wt%; the rest is CoFe, of which Co is 0.8wt%.

[0089] Melting: weigh and mix the industrial pure metal raw materials according to the alloy composition in mass percentage, and use a vacuum rapid solidification melting furnace to rapidly quench the target raw materials to obtain NdFeB alloy castings; Hydrogen crushing: The NdFeB alloy castings are crushed by hydrogen crushing furnace to obtain NdFeB coarse powder; Airflow milling: After the coarse powder is stirred and mixed, it is further ground with a fluidized bed airflow mill. No oxygen is added during the airflow milling to grind the coarse powder into fine NdFeB powder. Antioxidants are added to the obtained NdFeB fine powder and mixed evenly. Orientation molding: The alloy powder is oriented and molded in a magnetic field under nitrogen protection to obtain a compact; Sintering and tempering: After vacuum sintering and tempering, the pressed green sheet is cooled to obtain sintered NdFeB blanks with specifications of 55*45*35 squares.

[0090] The sintered NdFeB blank is a 55*45*35 square block. After machining, each blank magnet can be processed into 10 magnetic sheets with a size of 55*45*3mm. 4) For the sintered NdFeB magnet matrix magnetic sheet with a specification of 55*45*3, magnetron sputtering is performed using the high resistivity auxiliary alloy target material in step 2), and the addition amount of the high resistivity auxiliary alloy diffusion source is 0.5%wt of the mass of the NdFeB magnet matrix magnetic sheet; 5) Grain boundary diffusion and tempering: The 55*45*3 sintered NdFeB matrix magnet sheet with high resistivity auxiliary alloy that has been magnetron sputtered is subjected to grain boundary diffusion at 900℃ for 8 hours. Then it is tempered at 620℃ for 4 hours to obtain a high resistivity sintered NdFeB magnet.

[0091] 6) For the high resistivity sintered NdFeB magnet samples, the magnetic properties, magnet oxygen content, resistivity test, magnet composition test, installed overload aging and demagnetization test and other tests are carried out.

[0092] A permanent magnet measuring instrument, a German ELTRA oxygen-hydrogen analyzer, a metal resistivity detector, an inductively coupled plasma mass spectrometer, a high temperature aging box, and a permanent magnet motor dynamometer are used to respectively carry out the magnetic properties, oxygen content, resistivity test, magnet composition test, high temperature aging demagnetization test, and installed high temperature overload aging demagnetization test of the magnet. The test results of Example 1 and Comparative Example 5, and Example 3 and Comparative Example 6 are compared as shown in Table 4: Table 4 Compare project names Example 1 Comparative Example 5 Example 3 Comparative Example 6 Pr(wt%) 7.775 7.775 6.067 6.067 Nd(wt%) 22.275 22.275 17.533 17.533 Dy(wt%) 0 0 1.5 1.5 Ce(wt%) 0 0 7 7 Al(wt%) 0.155 0.155 0.35 0.35 Cu(wt%) 0.2 0.2 0.375 0.375 Ga(wt%) 0.225 0.225 0.275 0.275 In(wt%) 0 0 0 0 Ti(wt%) 0 0 0.2 0.2 Zr(wt%) 0.3 0.3 0.2 0.2 Co(wt%) 0.5 0.5 0.8 0.8 B(wt%) 0.94 0.94 0.9 0.9 Br(KGs) 14.4 14.4 12.55 12.54 Hcj(KOe) 17.75 16.95 22.9 21.2 (BH)max(MGOe) 50.8 50.75 38.9 38.95 Hk / Hcj(%) 99.5 98.5 98.5 97 Oxygen content (ppm) 705 750 725 770 Resistivity(uΩm) 2.25 1.95 2.15 1.87 High temperature aging and demagnetization of magnets 100℃ open circuit for 2 hours, irreversible flux loss 1.2-3.5% 100℃ open circuit for 2 hours, irreversible magnetic flux loss 7.7-10.2% 120℃ open circuit for 2 hours, irreversible magnetic flux loss 0.5-3.3% 120℃ open circuit for 2 hours, irreversible magnetic flux loss 9.1-10.5% Installed high temperature overload aging demagnetization test After 150℃ closed circuit high current impact high temperature overload test, the irreversible loss of magnetic flux is 2.5-4.1% After 150℃ closed circuit high current impact high temperature overload test, the irreversible loss of magnetic flux is 8.5-10.9% After 180℃ closed circuit high current impact overload test, the irreversible loss of magnetic flux is 1.8-4.7% After 180℃ closed circuit high current impact high temperature overload test, the irreversible loss of magnetic flux is 12.1-15.5% From the comparison of the feed ratio and the results in Table 4, it can be seen that the magnet matrix composition and the high resistivity auxiliary alloy of the sintered NdFeB matrix of Example 1 and Comparative Example 5 are exactly the same. Due to the low melting point of the high resistivity auxiliary alloy, there is no difference in the element content after low temperature diffusion and high temperature diffusion. While Example 1 uses a lower diffusion temperature of 720°C, and Comparative Example 5 uses a traditional higher diffusion temperature of 900°C. From the comparison data, it can be seen that the use of the low temperature diffusion process of the present invention to perform grain boundary diffusion of the high resistivity auxiliary alloy can obtain better resistivity, intrinsic coercivity, high temperature aging demagnetization of magnets, and installed high temperature overload aging demagnetization test performance.

[0093] From the comparison in Table 4, it can be seen that the magnet composition of the sintered NdFeB matrix of Example 3 and Comparative Example 6 is exactly the same, and the sintered NdFeB matrix magnet uses Ce to replace PrNd by 23%, while Example 3 uses a lower diffusion temperature of 700°C, and Comparative Example 6 uses a traditional higher diffusion temperature of 900°C. From the comparative data, low-temperature diffusion of the high-resistivity auxiliary alloy described in the present invention can obtain better resistivity, intrinsic coercive force, high-temperature aging demagnetization of the magnet, and installed high-temperature overload aging demagnetization tests.

[0094] And it can be analyzed from the data that the resistivity, intrinsic coercive force, high-temperature aging demagnetization of magnets, and installed high-temperature overload aging demagnetization tests of high-cerium NdFeB magnets are improved more significantly by low-temperature grain boundary diffusion at a temperature far lower than the traditional diffusion temperature. After analysis, it is believed that the present invention adopts a lower diffusion temperature to avoid the change in the phase structure of the cerium iron boron magnet caused by the traditional higher diffusion temperature. The high resistivity auxiliary alloy of the present invention has a lower melting point than the traditional diffusion source. By utilizing its low-temperature diffusion property, it can effectively avoid the phase change caused by the diffusion of the cerium iron boron magnet, which is beneficial to improve the resistivity and intrinsic coercive force of the cerium iron boron magnet.

Claims

1. A high resistivity sintered NdFeB magnet, Features The high resistivity sintered NdFeB magnet is prepared by the following method: The high resistivity sintered NdFeB magnet is obtained by sputtering a high resistivity auxiliary alloy diffusion source on the surface of the NdFeB magnet matrix, then performing grain boundary diffusion, and then performing tempering treatment after cooling; The composition of the high resistivity auxiliary alloy diffusion source is: Fr. 1-x-y-z the x With y (InGa) z ; Among them, x=0.05~0.1, y=0.10~0.15, z=0.10~0.

15.

2. The high resistivity sintered NdFeB magnet according to claim 1, Features The addition amount of the high resistivity auxiliary alloy diffusion source is 0.5-3% of the mass of the NdFeB magnet matrix.

3. The high resistivity sintered NdFeB magnet according to claim 1, Features The high resistivity auxiliary alloy diffusion source is covered on the surface of the NdFeB magnet substrate by magnetron sputtering. The NdFeB magnet substrate is a magnetic sheet with a thickness of 2-10 mm obtained by machining.

4. The high resistivity sintered NdFeB magnet according to claim 1, Features In the high resistivity auxiliary alloy diffusion source, the total mass content of low melting point elements such as Al, Cu, In and Ga is not less than 25wt%.

5. The high resistivity sintered NdFeB magnet according to claim 1, Features The melting point of the high resistivity auxiliary alloy diffusion source is 600-770°C.

6. The high resistivity sintered NdFeB magnet according to claim 1, Features The temperature of the grain boundary diffusion is 620-770° C., and the time is 3-10 hours.

7. The high resistivity sintered NdFeB magnet according to claim 1, Features The Pr content in high resistivity sintered NdFeB magnets is 4~30% higher than that in the NdFeB magnet matrix.

8. The high resistivity sintered NdFeB magnet according to claim 1, Features The resistivity of high resistivity sintered NdFeB magnets is more than 50% higher than that of NdFeB magnet matrix. After being installed in the motor, the maximum operating temperature is increased by 20-50℃.

9. The high resistivity sintered NdFeB magnet according to claim 1, Features The oxygen content of the high resistivity sintered NdFeB magnet increases by no more than 200ppm compared with the NdFeB magnet matrix before treatment, and the intrinsic coercive force of the high resistivity sintered NdFeB magnet increases by more than 2KOe compared with the NdFeB magnet matrix before treatment.

10. The high resistivity sintered NdFeB magnet according to claim 1, Features The high resistivity sintered NdFeB magnet has praseodymium-rich phase, Pr6(FeM)14 phase, part of Pr6Fe13Ga phase, Pr5(InGa)3 and praseodymium-rich region with a volume fraction of 7-11% between main phase crystals and corner regions.