Novel flip chip welding process

By performing substrate plasma cleaning, setting bumps and ultrasonic welding in the flip welding process, combining specific solder paste and flux, the problems of complex connection between chips and substrates in the existing technology are solved, and efficient chip welding is achieved and industrial production.

CN119069371APending Publication Date: 2024-12-03NANO OPTOELECTRONICS (TAIYUAN) RESEARCH INSTITUTE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411197838.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing flip welding process is complex in the process of connecting chips to substrates and poor connection point reliability, which affects the packaging quality and output of the chips.

Method used

The new flip chip welding process is adopted, including substrate plasma cleaning, bump setting, ultrasonic welding and glue filling, and the use of specific components of solder paste and flux, combined with ultrasonic welding technology to ensure the reliability of the connection point.

Benefits of technology

It improves the assembly efficiency and connection reliability of chips and substrates, saves production time, is suitable for industrial production, and significantly improves the quality and quality of chip welding.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of semiconductor packaging, in particular to a novel flip chip welding process. Comprising the following steps: S1, taking a to-be-treated substrate, and carrying out plasma cleaning on the substrate to obtain a pretreated substrate; s2, salient points are arranged on the substrate obtained through pretreatment; s3, the chip is reversely attached to the substrate, ultrasonic welding and filling are carried out, and welding of the flip chip is completed; the welding process provided by the invention not only has better assembly efficiency, but also can save time, effectively improve the yield and is more beneficial to industrial production of flip-chip welding chips, and the provided soldering paste and soldering flux are combined with an ultrasonic welding mode, so that reliable connection of connection points in the packaging process of the chips and the substrate is ensured, and the production efficiency of the flip-chip welding chips is improved. And the quality is effectively ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of semiconductor packaging, in particular to a novel flip chip welding process. Background Art

[0002] Flip chip welding technology connects two materials in the vertical direction through metal or alloy bumps. In addition to fixing the two materials, it also requires that electrical signals can be transmitted between the two.

[0003] The existing flip-chip soldering is mainly done on the aluminum layer of the chip, using electroplating and other processes to make copper pillars and solder caps of a certain thickness, then applying flux, flip-chip mounting, and reflow to achieve the connection between the chip and the substrate. The above process is relatively complicated for the chip processing process, and the reliability of the connection point during the chip and substrate packaging process is poor.

[0004] Based on this, the present invention provides a new flip chip welding process to solve the above-mentioned technical problems! Summary of the invention

[0005] The purpose of the present invention is to provide a novel flip chip welding process. The provided welding process not only has good assembly efficiency, but also can save time, so that the output is effectively improved, which is more conducive to the industrial production of flip chip welding chips. The provided solder paste and flux, combined with ultrasonic welding method, ensure the reliable connection of the connection points during the chip and substrate packaging process, effectively ensuring its quality.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] The present invention provides a novel flip chip welding process, comprising the following steps:

[0008] S1, taking a substrate to be processed, and plasma cleaning the substrate to obtain a pre-processed substrate;

[0009] S2, setting bumps on the pre-treated substrate;

[0010] S3, attaching the chip to the substrate by flip-chip, ultrasonic welding, and filling to complete the welding of the flip-chip.

[0011] The present invention is further configured as follows: in step S1, the plasma cleaning process is as follows:

[0012] Place the substrate in a plasma cleaning device and evacuate the substrate to a vacuum degree of 35 to 80 Pa;

[0013] Then, a plasma cleaning working gas is injected, and the substrate is cleaned at a substrate moving speed of 8 to 10 m / min;

[0014] The injection flow rate of the working gas is 3 to 6 L / min.

[0015] The present invention is further configured as follows: the working gas is selected from any one of nitrogen and argon.

[0016] The present invention is further configured as follows: in step S2, the process of setting the bumps on the substrate obtained by the pretreatment is as follows:

[0017] A substrate pad is arranged on the substrate, and then a copper column is prefabricated on the substrate pad;

[0018] Solder paste is printed on the resulting copper pillars, and flux is printed on the solder paste to complete the setting of the bumps.

[0019] The present invention is further configured as follows: the solder paste is composed of the following raw material components in percentage by mass: 1.2-1.4% Ag, 0.5-0.8% Cu, 0.05-0.1% Ni, and the remainder Sn;

[0020] The preparation process of the solder paste is as follows:

[0021] Accurately weigh Ag, Cu, Ni and Sn, and mix the Ag, Cu, Ni and Sn powders by ball milling;

[0022] Then put it into a quartz tube and seal it in vacuum. After high-temperature smelting, keep it warm for 100 to 120 minutes, and then cool it to room temperature before discharging it.

[0023] The product obtained by discharging the material is placed in a muffle furnace for remelting, and after melting, it is taken out and oil-cooled;

[0024] Among them, the vacuum degree of the vacuum tube is 0.5~1.1×10 -4 Pa, the smelting temperature is 800~1000℃.

[0025] The present invention is further configured as follows: the soldering flux is composed of the following raw materials in parts by weight: 30 to 40 parts of solvent, 3 to 6 parts of zinc chloride, 3 to 5 parts of hydrogenated rosin, 2 to 4 parts of dodecyl hydroxystearic acid, 4 to 7 parts of sodium dodecylbenzene sulfonate and 2 to 5 parts of methylbenzotriazole;

[0026] The preparation process of the soldering flux is as follows:

[0027] The solvent, zinc chloride, hydrogenated rosin, dodecyl stearic acid, sodium dodecylbenzene sulfonate and methyl benzotriazole are accurately weighed and placed in a production kettle for heating and dissolution to obtain a soldering flux.

[0028] The present invention is further configured as follows: the solvent is a mixture of diethylene glycol butyl ether and ethylene glycol diethyl ether in a mass ratio of 1:0.2-0.4.

[0029] The present invention is further configured as follows: in step S3, the ultrasonic power of the ultrasonic welding is 0.7-1.5 W, the welding time is 100-300 ms, and the welding temperature is 60-200°C.

[0030] The present invention is further configured as follows: in the step S3, the filling is to fill glue between the chip and the substrate after the welding is solidified.

[0031] Compared with the prior art, the present invention has the following beneficial effects:

[0032] The novel flip chip welding process provided by the present invention is to obtain a pre-treated substrate by plasma cleaning the substrate, then set bumps on the pre-treated substrate, and finally flip the chip onto the substrate, ultrasonically weld, and fill to complete the welding of the flip chip; the provided welding process not only has good assembly efficiency, but also can save time, so that the output is effectively improved, which is more conducive to the industrial production of flip chip welding chips, and the provided solder paste and flux, combined with the ultrasonic welding method, ensure the reliable connection of the connection points during the chip and substrate packaging process, and effectively ensure its quality. The novel flip chip welding process provided by the present invention has a broader market prospect and is more suitable for promotion. DETAILED DESCRIPTION

[0033] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0034] Example 1

[0035] This embodiment provides a novel flip chip welding process, comprising the following steps:

[0036] S1. Take a substrate to be processed and perform plasma cleaning on the substrate to obtain a pre-processed substrate.

[0037] The process of plasma cleaning is as follows:

[0038] Place the substrate in a plasma cleaning device and evacuate the substrate to a vacuum degree of 35 Pa;

[0039] Then, a plasma cleaning working gas is injected and the substrate is cleaned at a substrate moving speed of 8 m / min;

[0040] The injection flow rate of the working gas is 3 L / min.

[0041] Furthermore, nitrogen is selected as the working gas.

[0042] S2, setting bumps on the pre-treated substrate.

[0043] The process of setting the bumps on the pre-treated substrate is as follows:

[0044] A substrate pad is arranged on the substrate, and then a copper column is prefabricated on the substrate pad;

[0045] Solder paste is printed on the resulting copper pillars, and flux is printed on the solder paste to complete the setting of the bumps.

[0046] Further, the solder paste is composed of the following raw material components in mass percentage: 1.2% Ag, 0.5% Cu, 0.05% Ni, and the balance Sn;

[0047] The preparation process of solder paste is as follows:

[0048] Accurately weigh Ag, Cu, Ni and Sn, and mix the Ag, Cu, Ni and Sn powders by ball milling;

[0049] Then put it into a quartz tube and seal it in vacuum. After high-temperature smelting, keep it warm for 100 to 120 minutes, and then cool it to room temperature before discharging it.

[0050] The product obtained by discharging the material is placed in a muffle furnace for remelting, and after melting, it is taken out and oil-cooled;

[0051] The vacuum degree of the vacuum tube is 0.5×10 -4 Pa, the smelting temperature is 800℃.

[0052] In addition, the soldering flux is composed of the following raw materials in parts by weight: 30 to 40 parts of solvent, 3 to 6 parts of zinc chloride, 3 parts of hydrogenated rosin, 2 parts of dodecyl hydroxystearic acid, 4 parts of sodium dodecylbenzene sulfonate and 2 parts of methyl benzotriazole;

[0053] The preparation process of flux is as follows:

[0054] The solvent, zinc chloride, hydrogenated rosin, dodecyl stearic acid, sodium dodecylbenzene sulfonate and methyl benzotriazole are accurately weighed and placed in a production kettle for heating and dissolution to obtain a soldering flux.

[0055] The solvent is a mixture of diethylene glycol butyl ether and ethylene glycol diethyl ether in a mass ratio of 1:0.2.

[0056] S3, attaching the chip to the substrate by flip-chip, ultrasonic welding, and filling to complete the welding of the flip-chip.

[0057] The ultrasonic power of ultrasonic welding is 0.7W, the welding time is 100ms, and the welding temperature is 60°C.

[0058] Filling is to fill glue between the chip and the substrate after the soldering is solidified.

[0059] In this embodiment, it should be noted that the glue used is nitrile phenolic polyurethane glue NCP.

[0060] Example 2

[0061] This embodiment provides a novel flip chip welding process, comprising the following steps:

[0062] S1. Take a substrate to be processed and perform plasma cleaning on the substrate to obtain a pre-processed substrate.

[0063] The process of plasma cleaning is as follows:

[0064] Place the substrate in a plasma cleaning device and evacuate the device to a vacuum degree of 37 Pa;

[0065] Then, a plasma cleaning working gas is injected and the substrate is cleaned at a substrate moving speed of 9 m / min;

[0066] The injection flow rate of the working gas is 4 L / min.

[0067] Furthermore, argon is selected as the working gas.

[0068] S2, setting bumps on the pre-treated substrate.

[0069] The process of setting the bumps on the pre-treated substrate is as follows:

[0070] A substrate pad is arranged on the substrate, and then a copper column is prefabricated on the substrate pad;

[0071] Solder paste is printed on the resulting copper pillars, and flux is printed on the solder paste to complete the setting of the bumps.

[0072] Further, the solder paste is composed of the following raw material components in mass percentage: 1.3% Ag, 0.6% Cu, 0.06% Ni, and the balance Sn;

[0073] The preparation process of solder paste is as follows:

[0074] Accurately weigh Ag, Cu, Ni and Sn, and mix the Ag, Cu, Ni and Sn powders by ball milling;

[0075] Then put it into a quartz tube and seal it in vacuum. After high-temperature smelting, keep it warm for 100 to 120 minutes, and then cool it to room temperature before discharging it.

[0076] The product obtained by discharging the material is placed in a muffle furnace for remelting, and after melting, it is taken out and oil-cooled;

[0077] The vacuum degree of the vacuum tube is 0.6×10 -4 Pa, the smelting temperature is 810℃.

[0078] In addition, the soldering flux is composed of the following raw materials in parts by weight: 32 parts of solvent, 4 parts of zinc chloride, 4 parts of hydrogenated rosin, 3 parts of dodecyl hydroxystearic acid, 5 parts of sodium dodecylbenzene sulfonate and 3 parts of methyl benzotriazole;

[0079] The preparation process of flux is as follows:

[0080] The solvent, zinc chloride, hydrogenated rosin, dodecyl stearic acid, sodium dodecylbenzene sulfonate and methyl benzotriazole are accurately weighed and placed in a production kettle for heating and dissolution to obtain a soldering flux.

[0081] The solvent is a mixture of diethylene glycol butyl ether and ethylene glycol diethyl ether in a mass ratio of 1:0.3.

[0082] S3, attaching the chip to the substrate by flip-chip, ultrasonic welding, and filling to complete the welding of the flip-chip.

[0083] Among them, the ultrasonic power of ultrasonic welding is 0.8W, the welding time is 110ms, and the welding temperature is 62°C.

[0084] Filling is to fill glue between the chip and the substrate after the soldering is solidified.

[0085] In this embodiment, it should be noted that the glue used is nitrile phenolic polyurethane glue NCP.

[0086] Example 3

[0087] This embodiment provides a novel flip chip welding process, comprising the following steps:

[0088] S1. Take a substrate to be processed and perform plasma cleaning on the substrate to obtain a pre-processed substrate.

[0089] The process of plasma cleaning is as follows:

[0090] Place the substrate in a plasma cleaning device and evacuate the substrate to a vacuum degree of 55 Pa;

[0091] Then, a plasma cleaning working gas is injected and the substrate is cleaned at a substrate moving speed of 9 m / min;

[0092] The injection flow rate of the working gas is 5 L / min.

[0093] Furthermore, nitrogen is selected as the working gas.

[0094] S2, setting bumps on the pre-treated substrate.

[0095] The process of setting the bumps on the pre-treated substrate is as follows:

[0096] A substrate pad is arranged on the substrate, and then a copper column is prefabricated on the substrate pad;

[0097] Solder paste is printed on the resulting copper pillars, and flux is printed on the solder paste to complete the setting of the bumps.

[0098] Further, the solder paste is composed of the following raw material components in mass percentage: 1.3% Ag, 0.6% Cu, 0.07% Ni, and the balance Sn;

[0099] The preparation process of solder paste is as follows:

[0100] Accurately weigh Ag, Cu, Ni and Sn, and mix the Ag, Cu, Ni and Sn powders by ball milling;

[0101] Then put it into a quartz tube and seal it in vacuum. After high-temperature smelting, keep it warm for 110 minutes and cool it to room temperature before discharging.

[0102] The product obtained by discharging the material is placed in a muffle furnace for remelting, and after melting, it is taken out and oil-cooled;

[0103] The vacuum degree of the vacuum tube is 0.8×10 -4 Pa, the smelting temperature is 900℃.

[0104] In addition, the soldering flux is composed of the following raw materials in parts by weight: 35 parts of solvent, 5 parts of zinc chloride, 4 parts of hydrogenated rosin, 3 parts of dodecyl hydroxystearic acid, 5 parts of sodium dodecylbenzene sulfonate and 4 parts of methyl benzotriazole;

[0105] The preparation process of flux is as follows:

[0106] The solvent, zinc chloride, hydrogenated rosin, dodecyl stearic acid, sodium dodecylbenzene sulfonate and methyl benzotriazole are accurately weighed and placed in a production kettle for heating and dissolution to obtain a soldering flux.

[0107] The solvent is a mixture of diethylene glycol butyl ether and ethylene glycol diethyl ether in a mass ratio of 1:0.3.

[0108] S3, attaching the chip to the substrate by flip-chip, ultrasonic welding, and filling to complete the welding of the flip-chip.

[0109] The ultrasonic power of ultrasonic welding is 1.1W, the welding time is 200ms, and the welding temperature is 130°C.

[0110] Filling is to fill glue between the chip and the substrate after the soldering is solidified.

[0111] In this embodiment, it should be noted that the glue used is nitrile phenolic polyurethane glue NCP.

[0112] Example 4

[0113] This embodiment provides a novel flip chip welding process, comprising the following steps:

[0114] S1. Take a substrate to be processed and perform plasma cleaning on the substrate to obtain a pre-processed substrate.

[0115] The process of plasma cleaning is as follows:

[0116] Place the substrate in a plasma cleaning device and evacuate the device to a vacuum degree of 78 Pa;

[0117] Then, a plasma cleaning working gas is injected and the substrate is cleaned at a substrate moving speed of 9 m / min;

[0118] The injection flow rate of the working gas is 5 L / min.

[0119] Furthermore, nitrogen is selected as the working gas.

[0120] S2, setting bumps on the pre-treated substrate.

[0121] The process of setting the bumps on the pre-treated substrate is as follows:

[0122] A substrate pad is arranged on the substrate, and then a copper column is prefabricated on the substrate pad;

[0123] Solder paste is printed on the resulting copper pillars, and flux is printed on the solder paste to complete the setting of the bumps.

[0124] Further, the solder paste is composed of the following raw material components in mass percentage: 1.3% Ag, 0.7% Cu, 0.09% Ni, and the balance Sn;

[0125] The preparation process of solder paste is as follows:

[0126] Accurately weigh Ag, Cu, Ni and Sn, and mix the Ag, Cu, Ni and Sn powders by ball milling;

[0127] Then put it into a quartz tube and seal it in vacuum. After high-temperature smelting, keep it warm for 118 minutes and discharge it after cooling to room temperature.

[0128] The product obtained by discharging the material is placed in a muffle furnace for remelting, and after melting, it is taken out and oil-cooled;

[0129] The vacuum degree of the vacuum tube is 1.0×10 -4 Pa, the smelting temperature is 950℃.

[0130] In addition, the soldering flux is composed of the following raw materials in parts by weight: 38 parts of solvent, 5 parts of zinc chloride, 4 parts of hydrogenated rosin, 3 parts of dodecyl hydroxystearic acid, 6 parts of sodium dodecylbenzene sulfonate and 4 parts of methylbenzotriazole;

[0131] The preparation process of flux is as follows:

[0132] The solvent, zinc chloride, hydrogenated rosin, dodecyl stearic acid, sodium dodecylbenzene sulfonate and methyl benzotriazole are accurately weighed and placed in a production kettle for heating and dissolution to obtain a soldering flux.

[0133] The solvent is a mixture of diethylene glycol butyl ether and ethylene glycol diethyl ether in a mass ratio of 1:0.3.

[0134] S3, attaching the chip to the substrate by flip-chip, ultrasonic welding, and filling to complete the welding of the flip-chip.

[0135] Among them, the ultrasonic power of ultrasonic welding is 1.4W, the welding time is 280ms, and the welding temperature is 190℃.

[0136] Filling is to fill glue between the chip and the substrate after the soldering is solidified.

[0137] In this embodiment, it should be noted that the glue used is nitrile phenolic polyurethane glue NCP.

[0138] Example 5

[0139] This embodiment provides a novel flip chip welding process, comprising the following steps:

[0140] S1. Take a substrate to be processed and perform plasma cleaning on the substrate to obtain a pre-processed substrate.

[0141] The process of plasma cleaning is as follows:

[0142] Place the substrate in a plasma cleaning device and evacuate the substrate to a vacuum degree of 80 Pa;

[0143] Then, a plasma cleaning working gas is injected and the substrate is cleaned at a substrate moving speed of 10 m / min;

[0144] The injection flow rate of the working gas is 6 L / min.

[0145] Furthermore, nitrogen is selected as the working gas.

[0146] S2, setting bumps on the pre-treated substrate.

[0147] The process of setting the bumps on the pre-treated substrate is as follows:

[0148] A substrate pad is arranged on the substrate, and then a copper column is prefabricated on the substrate pad;

[0149] Solder paste is printed on the resulting copper pillars, and flux is printed on the solder paste to complete the setting of the bumps.

[0150] Further, the solder paste is composed of the following raw material components in mass percentage: 1.4% Ag, 0.8% Cu, 0.1% Ni, and the balance Sn;

[0151] The preparation process of solder paste is as follows:

[0152] Accurately weigh Ag, Cu, Ni and Sn, and mix the Ag, Cu, Ni and Sn powders by ball milling;

[0153] Then put it into a quartz tube and seal it in vacuum. After high-temperature smelting, keep it warm for 100 to 120 minutes, and then cool it to room temperature before discharging it.

[0154] The product obtained by discharging the material is placed in a muffle furnace for remelting, and after melting, it is taken out and oil-cooled;

[0155] The vacuum degree of the vacuum tube is 1.1×10 -4 Pa, the smelting temperature is 1000℃.

[0156] In addition, the soldering flux is composed of the following raw materials in parts by weight: 40 parts of solvent, 6 parts of zinc chloride, 5 parts of hydrogenated rosin, 4 parts of dodecyl hydroxystearic acid, 7 parts of sodium dodecylbenzene sulfonate and 5 parts of methyl benzotriazole;

[0157] The preparation process of flux is as follows:

[0158] The solvent, zinc chloride, hydrogenated rosin, dodecyl stearic acid, sodium dodecylbenzene sulfonate and methyl benzotriazole are accurately weighed and placed in a production kettle for heating and dissolution to obtain a soldering flux.

[0159] The solvent is a mixture of diethylene glycol butyl ether and ethylene glycol diethyl ether in a mass ratio of 1:0.4.

[0160] S3, attaching the chip to the substrate by flip-chip, ultrasonic welding, and filling to complete the welding of the flip-chip.

[0161] Among them, the ultrasonic power of ultrasonic welding is 1.5W, the welding time is 300ms, and the welding temperature is 200℃.

[0162] Filling is to fill glue between the chip and the substrate after the soldering is solidified.

[0163] In this embodiment, it should be noted that the glue used is nitrile phenolic polyurethane glue NCP.

[0164] The novel flip chip welding process provided by the present invention not only has good assembly efficiency, but also can save time, so that the output is effectively improved, which is more conducive to the industrial production of flip chip welding chips, and the provided solder paste and flux, combined with the ultrasonic welding method, ensure the reliable connection of the connection points during the chip and substrate packaging process, and effectively guarantee its quality. This shows that the novel flip chip welding process provided by the present invention has a broader market prospect and is more suitable for promotion.

[0165] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0166] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A novel flip chip welding process, characterized in that: The following steps are involved: S1, taking a substrate to be processed, and plasma cleaning the substrate to obtain a pre-processed substrate; S2, setting bumps on the pre-treated substrate; S3, attaching the chip to the substrate by flip-chip, ultrasonic welding, and filling to complete the welding of the flip-chip.

2. A novel flip chip welding process according to claim 1, characterized in that: In step S1, the plasma cleaning process is as follows: Place the substrate in a plasma cleaning device and evacuate the substrate to a vacuum degree of 35 to 80 Pa; Then, a plasma cleaning working gas is injected, and the substrate is cleaned under the condition of a substrate moving speed of 8 to 10 m / min; The injection flow rate of the working gas is 3 to 6 L / min.

3. A novel flip chip welding process according to claim 2, characterized in that: The working gas is selected from any one of nitrogen and argon.

4. A novel flip chip welding process according to claim 1, characterized in that: In step S2, the process of setting bumps on the pre-treated substrate is as follows: A substrate pad is arranged on the substrate, and then a copper column is prefabricated on the substrate pad; Solder paste is printed on the resulting copper pillars, and flux is printed on the solder paste to complete the setting of the bumps.

5. A novel flip chip welding process according to claim 4, characterized in that: The solder paste is composed of the following raw material components in percentage by mass: 1.2-1.4% Ag, 0.5-0.8% Cu, 0.05-0.1% Ni, and the balance Sn; The preparation process of the solder paste is as follows: Accurately weigh Ag, Cu, Ni and Sn, and mix the Ag, Cu, Ni and Sn powders by ball milling; Then put it into a quartz tube and seal it in vacuum. After high-temperature smelting, keep it warm for 100 to 120 minutes, and then discharge it after cooling to room temperature. The product obtained by discharging the material is placed in a muffle furnace for remelting, and after melting, it is taken out and oil-cooled; The vacuum degree of the vacuum tube is 0.5~1.1×10 -4 Pa, the smelting temperature is 800~1000℃.

6. A novel flip chip welding process according to claim 4, characterized in that: The soldering flux is composed of the following raw materials in parts by weight: 30 to 40 parts of solvent, 3 to 6 parts of zinc chloride, 3 to 5 parts of hydrogenated rosin, 2 to 4 parts of dodecyl hydroxystearic acid, 4 to 7 parts of sodium dodecylbenzene sulfonate and 2 to 5 parts of methylbenzotriazole; The preparation process of the soldering flux is as follows: The solvent, zinc chloride, hydrogenated rosin, dodecyl stearic acid, sodium dodecylbenzene sulfonate and methyl benzotriazole are accurately weighed and placed in a production kettle for heating and dissolution to obtain a soldering flux.

7. A novel flip chip welding process according to claim 6, characterized in that: The solvent is prepared by mixing diethylene glycol butyl ether and ethylene glycol diethyl ether in a mass ratio of 1:0.2-0.

4.

8. A novel flip chip welding process according to claim 1, characterized in that: In the step S3, the ultrasonic power of the ultrasonic welding is 0.7-1.5W, the welding time is 100-300ms, and the welding temperature is 60-200°C.