Graphene wafer transferring and packaging method and application thereof

By forming an antimony trioxide encapsulation layer on the surface of the graphene wafer and using an adhesive layer to assist the transfer, the problems of polymer residues and water and oxygen adsorption in graphene transfer are solved, and high integrity and cleanliness of graphene are achieved degree transfer improves its performance and stability.

CN119069381APending Publication Date: 2024-12-03BEIJING GRAPHENE INST +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310632341.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-30
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

In the existing graphene transfer method, the strong interaction between polymer polymer and graphene is difficult to remove, resulting in the residual surface of graphene affecting its structure and performance. The shear stress during the cleaning process may cause damage, which in turn causes carrier scattering and reduces the device. performance.

Method used

Antimony trioxide is used as the transfer medium, and the encapsulation layer is formed on the surface of the graphene wafer by vacuum thermal deposition. During the transfer process, the adhesive layer and the support substrate are used to assist the transfer, and the support substrate is separated from the heat treatment to form the encapsulation layer. /graphene/target substrate composite structure to avoid organic molecules residues and water and oxygen adsorption.

Benefits of technology

Realizes lossless, clean transfer and packaging of graphene, reduces carrier scattering, improves graphene performance and working stability, is compatible with the packaging technology of large-area graphene wafers, and reduces interface scattering and device roughness. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069381A_ABST
    Figure CN119069381A_ABST
Patent Text Reader

Abstract

The invention relates to a graphene wafer transfer method. The method comprises the following steps: forming a packaging layer on the surface of a graphene wafer directly growing on a growth substrate; spin-coating adhesive glue on the packaging layer to form an adhesive glue layer, and attaching a viscous supporting substrate to obtain a supporting substrate / packaging layer / graphene wafer / growth substrate composite structure; separating the supporting substrate / packaging layer / graphene wafer from the growth substrate to obtain a supporting substrate / packaging layer / graphene wafer composite structure; the supporting substrate / packaging layer / graphene wafer composite structure is attached to a target substrate; performing heat treatment to separate the supporting substrate from the packaging layer to obtain a packaging layer / graphene wafer / target substrate composite structure; wherein the packaging layer is an antimony trioxide layer. According to the method for transferring the graphene wafer through the packaging material, lossless, clean and large-area transferring and packaging of the graphene wafer are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of carbon materials, and in particular relates to the transfer, packaging and application of graphene wafers. Background Art

[0002] Graphene has excellent physical and chemical properties due to its unique structure. It has great application potential in the fields of electronic devices, transparent conductive films, composite materials, etc., and has attracted extensive attention and research. Especially in the field of electronic communications, graphene has become a highly competitive electronic material in the post-silicon CMOS era due to its extremely high carrier mobility, submicron-scale ballistic transmission, and ultra-high frequency operation response. Graphene films are mainly prepared by chemical vapor deposition, which can grow large-size, high-quality, and controllable-number-of-layer graphene films on the surface of transition metals, especially copper substrates. In order to realize the practical application of graphene, it is usually necessary to transfer it from the growth substrate to the target substrate. Therefore, transfer technology has become an important factor limiting the excellent performance of graphene. It is crucial to develop large-area, high-integrity, high-cleanliness, low-defect density, low-cost, and green graphene transfer technology.

[0003] At present, most graphene transfer methods rely on high molecular polymers such as polymethyl methacrylate (PMMA) as transfer media, and based on this, a support layer is designed to assist in completing graphene transfer. However, these high molecular polymers have strong interactions with graphene and are difficult to remove. The organic molecules remaining on the graphene surface will greatly affect the intrinsic structure and physical properties of graphene. Secondly, during the cleaning process, the shear stress caused by the surface tension of the liquid will also cause damage to the graphene. After the transfer, the graphene surface exposed to the air is prone to adsorb water and oxygen molecules. Charge transfer will occur between these adsorbates in the air and graphene, which will cause scattering of graphene carriers, resulting in a decrease in the performance of graphene devices. Summary of the invention

[0004] In order to solve the above problems, the present invention provides a graphene wafer transfer and packaging method and a structure and application obtained by the method.

[0005] The invention provides a method for transferring a graphene wafer, comprising: forming a packaging layer on the surface of a graphene wafer directly grown on a growth substrate; spin-coating an adhesive on the packaging layer to form an adhesive layer, and then laminating a support substrate with an adhesiveness to obtain a support substrate / packaging layer / graphene wafer / growth substrate composite structure; separating the support substrate / packaging layer / graphene wafer from the growth substrate to obtain a support substrate / packaging layer / graphene wafer composite structure; laminating the support substrate / packaging layer / graphene wafer composite structure to a target substrate; and separating the support substrate and the packaging layer by heat treatment to obtain a packaging layer / graphene wafer / target substrate composite structure; wherein the packaging layer is an antimony trioxide layer.

[0006] According to one embodiment of the present invention, the encapsulation layer is formed on the surface of the graphene wafer by vacuum thermal evaporation, and the evaporation condition is a vacuum degree of 10 -5 -10 -7 Torr, evaporation rate 0.01-2nm / s.

[0007] According to another embodiment of the present invention, the thickness of the encapsulation layer is greater than or equal to 3 nm; preferably, less than or equal to 20 μm.

[0008] According to another embodiment of the present invention, the adhesive is polyvinyl alcohol, polymethyl methacrylate, polycarbonate, preferably polyvinyl alcohol.

[0009] According to another embodiment of the present invention, the adhesive layer is formed by spin coating a solution containing polyvinyl alcohol on the surface of the encapsulation layer and then baking. The spin coating speed is 500-8000rpm, and the spin coating time is 30s-5min. The baking temperature is 50-200℃, and the baking time is 1-5min. Preferably, the mass concentration of the polyvinyl alcohol in the solution is 0.1-20%; the solvent of the solution is water or ethanol.

[0010] According to another embodiment of the present invention, the adhesive support substrate is a thermal release tape, a UV film or a silicone film, preferably a thermal release tape. The lamination method is roll lamination or vacuum lamination.

[0011] According to another embodiment of the present invention, the target substrate is a silicon wafer or sapphire, preferably a silicon wafer. The support substrate / encapsulation layer / graphene wafer composite structure is bonded to the target substrate by roll bonding or vacuum bonding.

[0012] According to another embodiment of the present invention, the support substrate / encapsulation layer / graphene wafer is separated from the growth substrate by mechanical peeling. Preferably, the mechanical peeling is manual or mechanical device assisted peeling, and the peeling speed is 0.1-5 cm / s.

[0013] According to another embodiment of the present invention, the thermal release tape is detached by placing the supporting substrate / encapsulation layer / graphene wafer / target substrate composite structure into a vacuum drying oven for heating, the heating temperature is 100-200° C., and the time is 20-60 min.

[0014] According to another embodiment of the present invention, the encapsulation layer / graphene wafer / target substrate composite structure is immersed in an adhesive solvent to remove residual organic molecular impurities. Preferably, the adhesive solvent is water or ethanol, the immersion temperature is 20-80°C, and the time is 1-10 minutes.

[0015] The present invention also provides a graphene wafer packaging structure, comprising a graphene wafer and an antimony trioxide packaging layer packaged on the surface of the graphene wafer.

[0016] According to an embodiment of the present invention, the thickness of the encapsulation layer is greater than or equal to 3 nm; preferably, less than or equal to 20 μm.

[0017] The present invention further provides a method for packaging a graphene wafer, comprising: forming a packaging layer on the surface of a graphene wafer directly grown on a growth substrate; wherein the packaging layer is an antimony trioxide layer.

[0018] According to one embodiment of the present invention, the encapsulation layer is formed on the surface of the graphene wafer by vacuum thermal evaporation, and the evaporation condition is a vacuum degree of 10 -5 -10 -7 Torr, and the evaporation rate is 0.01-2nm / s.

[0019] The present invention further provides a semiconductor device, comprising the above-mentioned graphene wafer packaging structure.

[0020] The present invention uses a method for transferring a graphene wafer using a packaging material to achieve lossless, clean transfer and packaging of the graphene wafer. Antimony trioxide, a packaging material that has a strong interaction with graphene, is used as a transfer medium to reduce the influence of organic molecules on the structure and properties of the graphene wafer during the transfer process, thereby avoiding damage and doping of the graphene. Furthermore, the transfer medium is formed into a thin film on the surface of the graphene wafer by thermal evaporation, and the graphene can achieve conformal contact with the transfer medium, avoiding water and oxygen doping, and improving the integrity during the transfer process. After the transfer, the graphene wafer is still protected by the packaging layer, avoiding the adsorption of impurity molecules such as water and oxygen in the environment on the graphene surface, reducing the carrier scattering caused by the adsorbate, and improving the performance and working stability of the subsequent application of the graphene. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 The graphene wafer transferred to the silicon wafer in Example 1 and Comparative Example 1 is a real photo and an optical microscope photo

[0022] Figure 2 1 and 2 are atomic force microscope images of the graphene wafers in Example 1 and Comparative Example 1.

[0023] Figure 3 It is the Raman characterization peak position statistical image of the graphene wafer in Example 1 and Comparative Example 1.

[0024] Figure 4 It is the Raman characterization 2D half-peak width statistical image of the graphene wafer in Example 1 and Comparative Example 1.

[0025] Figure 5 This is a real photo of the graphene wafer transferred to the sapphire substrate in Example 3.

[0026] Figure 6 This is an optical photograph of the micro-nano structure prepared in Example 4.

[0027] Fig. 7A and Figure 7B The carrier mobility test curves of the micro-nano devices prepared in Example 4 and Comparative Example 2 are shown respectively. DETAILED DESCRIPTION

[0028] The present invention is described in detail below in conjunction with specific implementation modes.

[0029] The transfer method of the graphene wafer of the present invention comprises: forming a packaging layer on the surface of the graphene wafer directly grown on the growth substrate; spin-coating an adhesive on the packaging layer to form an adhesive layer, and then laminating a support substrate with an adhesiveness to obtain a support substrate / packaging layer / graphene wafer / growth substrate composite structure; separating the support substrate / packaging layer / graphene wafer from the growth substrate to obtain a support substrate / packaging layer / graphene wafer composite structure; laminating the support substrate / packaging layer / graphene wafer composite structure to a target substrate; and separating the support substrate and the packaging layer by heat treatment to obtain a packaging layer / graphene wafer / target substrate composite structure; wherein the packaging layer is an antimony trioxide layer (Sb2O3).

[0030] The method for transferring a graphene wafer of the present invention can also be used to encapsulate a graphene wafer. That is, the method for encapsulating a graphene wafer comprises: forming an encapsulation layer on the surface of a graphene wafer directly grown on a growth substrate; wherein the encapsulation layer is an antimony trioxide layer. A graphene wafer encapsulation structure is obtained by the encapsulation method, the structure comprising a graphene wafer and an antimony trioxide encapsulation layer encapsulated on the surface thereof. The encapsulation structure can be used in semiconductor devices.

[0031] The graphene wafer transfer and packaging method of the present invention solves the influence of air adsorbents on the upper surface of graphene, such as water and oxygen molecules, on the scattering of graphene carriers while completing the lossless and clean transfer of graphene. The present invention develops an effective packaging technology compatible with silicon-based large-area graphene wafers, and uses a packaging layer material that can effectively block water and oxygen, thereby effectively inhibiting the adsorption of water and oxygen on the graphene surface. And explore interface packaging technology that is compatible with the transfer process. During the transfer process, it is usually necessary to introduce a transfer medium to assist in supporting the graphene, and to achieve conformal contact between the transfer medium and the graphene, so as to reduce the damage caused during the transfer process. The present invention uses the transfer medium itself as the packaging layer material of large-area graphene, selects a transfer medium with excellent water and oxygen barrier properties and easy to spread on the graphene surface to form conformal contact, and encapsulates and protects the graphene while assisting in the transfer of graphene.

[0032] The transfer and packaging method of the present invention uses antimony trioxide (Sb2O3) as a transfer packaging medium. The antimony oxide Sb2O3 selected in the present method is an inorganic molecular crystal, and its crystal structure is a cubic system or an orthorhombic system. The chemical bonds of Sb2O3 are all saturated, and there are no dangling bonds on the surface of the film formed by it. Moreover, a wafer-level film can be prepared by a standard thermal evaporation deposition process, and the required temperature is relatively low (186°C). Sb2O3 has a strong interaction force with graphene, and can be directly used as a transfer medium to transfer graphene. In addition, the band gap of cubic system Sb2O3 is 4.06eV, and the dielectric constant is 11.5, which also meets the requirements as a dielectric material. It can be combined with the top gate process of graphene devices to develop large-area graphene packaging technology, and it can be used as a packaging layer and a gate dielectric layer to inhibit the adsorption of water and oxygen, and introduce a top gate structure to effectively regulate the graphene carrier concentration. At the same time, compared with commonly used materials such as HfO2, it reduces the roughness of the top gate dielectric layer, the density of charge traps and scattering centers, reduces interface scattering, and improves the carrier mobility and device stability of graphene. Of course, orthorhombic Sb2O3 is a semiconductor material that can also realize the transfer and packaging of graphene.

[0033] In an optional embodiment, antimony trioxide is covered on the surface of the graphene wafer by thermal evaporation. Sb2O3 evaporated on a growth substrate such as a Cu wafer has a strong interaction force with graphene, and graphene can be directly mechanically peeled off from the growth substrate, and then transferred to a silicon substrate to continue to be retained as an encapsulation layer to protect graphene. Graphene will not be damaged by pollution and the like throughout the process, avoiding the influence of water, oxygen and other charged impurities remaining at the graphene interface on the quality of graphene. Sb2O3 is used as a transfer medium to complete the transfer and encapsulation of graphene. The Sb2O3 on the upper surface of the graphene is used as an encapsulation layer to avoid graphene contamination and doping, and can also be used as a top gate to accurately control the graphene Fermi level. At the same time, since the method does not use an organic solvent between the graphene and the encapsulation medium, the residual pollutants on the graphene surface can be greatly reduced, and the cleanliness of the graphene after the transfer is greatly improved. The method of the present invention can achieve large-area clean and complete graphene wafer transfer. It is compatible with batch transfer of 2, 4, 6, 8, and 12-inch graphene wafers. The transfer method of the present invention is applicable to any growth substrate for growing graphene wafers, including but not limited to copper / sapphire, copper-nickel alloy / sapphire, copper-cobalt alloy / sapphire, etc. The growth method of graphene wafers is not limited to chemical vapor deposition.

[0034] The evaporation conditions are vacuum for about 10 -5 -10 -7 Torr, evaporation temperature is about 150-200℃, and evaporation rate is 0.01-1nm / s. The slower the evaporation rate, the more uniform the antimony trioxide film obtained. Evaporation of antimony trioxide with a thickness of 3nm-20μm can transfer the graphene wafer completely. Those skilled in the art can select an appropriate evaporation thickness according to the actual use of the packaging structure, such as but not limited to 3nm, 10nm, 20nm, 30nm, 40nm, 50nm, 60nm, 70nm, 80nm, 90nm, 100nm, 150nm, 200nm, 500nm, 1μm, 5μm, 10μm, 15μm, 20μm, etc.

[0035] After the antimony trioxide is evaporated to transfer the encapsulation medium layer, an adhesive is spin-coated on the encapsulation layer, and then a sticky support substrate is bonded. The adhesive is polyvinyl alcohol, polymethyl methacrylate, etc., preferably polyvinyl alcohol. The mass concentration of polyvinyl alcohol in the solution is 1-10%; the solvent of the solution is water or ethanol. The polyvinyl alcohol layer is formed by spin-coating a solution containing polyvinyl alcohol on the surface of the encapsulation layer and then baking it. The spin coating speed is 500-8000rpm, and the spin coating time is 30s-5min. The baking temperature is 50-200℃, and the baking time is 1-5min. Then bond the support substrate, which is a thermal release tape, UV film or silicone resin film, preferably a thermal release tape. Bond the support substrate to the encapsulation layer / graphene wafer / growth substrate by roller bonding, vacuum bonding, etc. to reduce bubbles generated by bonding.

[0036] The support substrate / encapsulation layer / graphene wafer can be separated from the growth substrate by mechanical stripping. Mechanical stripping is manual or mechanical device assisted stripping, and the stripping speed is 0.1-5cm / s. Slower speed can improve the integrity of graphene. Those skilled in the art can select appropriate stripping speed according to actual needs, such as but not limited to 0.1cm / s, 0.2cm / s, 0.3cm / s, 0.4cm / s, 0.5cm / s, 0.6cm / s, 0.7cm / s, 0.8cm / s, 0.9cm / s, 1cm / s, 2cm / s, 3cm / s, 4cm / s, 5cm / s, etc.

[0037] The mechanically peeled support substrate / encapsulation layer / graphene wafer composite structure is bonded to the transfer target substrate, the target substrate is a silicon wafer or sapphire, preferably a silicon wafer. The support substrate / encapsulation layer / graphene wafer composite structure is bonded to the target substrate by roller bonding or vacuum bonding.

[0038] Afterwards, the support substrate is removed. For example, the support substrate / encapsulation layer / graphene wafer / target substrate composite structure can be placed in a vacuum drying oven and heated to remove the thermal release tape, the heating temperature is 100-200°C, the time is 20-60 minutes, the thermal release tape loses its stickiness, and the support substrate is removed.

[0039] Finally, the remaining adhesive layer is removed. The encapsulation layer / graphene wafer / target substrate composite structure can be immersed in an adhesive solvent to remove residual organic molecular impurities. The adhesive polyvinyl alcohol solvent can be water or ethanol, and the immersion temperature is 20-80°C and the time is 1-10 minutes.

[0040] The present invention is further described below by specific examples. However, these examples are merely exemplary and do not constitute any limitation to the protection scope of the present invention.

[0041] In the following examples and comparative examples, the reagents, materials and instruments used are all commercially available unless otherwise specified.

[0042] Example 1

[0043] The common commercial inorganic molecule antimony trioxide was deposited onto the surface of 4-inch graphene wafer / copper / sapphire wafer by thermal evaporation. Vacuum degree 5×10 -7 Torr, rate 0.03nm / s, thickness 50nm. Then spin-coat a polyvinyl alcohol solution (mass fraction 5%, solvent is water) at a speed of 4000rpm for 60s. After spin coating, place it on a hot plate and bake it at 80°C for 3min. Then use roller pressing to bond the thermal release tape (TRT) to the surface of polyvinyl alcohol to form a thermal release tape / polyvinyl alcohol / antimony trioxide / graphene / copper / sapphire composite structure. It is then fixed on a carrier, and a mechanical peeling (1cm / s) device is used to slowly peel off the thermal release tape / polyvinyl alcohol / antimony trioxide / graphene from the copper surface. The copper / sapphire growth substrate is cleaned with deionized water and ethanol, and then dried with nitrogen and placed in a wafer box for recovery. After that, a roller press is used to bond it to a silicon wafer. The resulting thermal release tape / polyvinyl alcohol / antimony trioxide / graphene / silicon wafer is placed in an oven, heated at 120°C for 30min, and then the edge of the silicon wafer is fixed with a clamp to peel off the supporting substrate. The antimony trioxide / graphene / silicon wafer structure was immersed in deionized water for 30 minutes to remove the residual polyvinyl alcohol adhesive, the surface was cleaned with deionized water, and dried with nitrogen to finally obtain a 4-inch graphene wafer transferred to the silicon wafer.

[0044] Example 2

[0045] The thickness of the antimony trioxide encapsulation layer formed by thermal evaporation of antimony trioxide onto the surface of the 6-inch graphene wafer / copper / sapphire wafer is 3 nm. The other steps are the same as those in Example 1, and finally a 6-inch graphene wafer transferred to a silicon wafer is obtained.

[0046] Example 3

[0047] The common commercial inorganic molecule antimony trioxide was deposited onto the surface of 4-inch graphene wafer / copper / sapphire wafer by thermal evaporation. Vacuum degree 5×10 -7Torr, rate 0.03nm / s, thickness 30nm. Then spin-coat a polyvinyl alcohol solution (mass fraction 5%, solvent is water) at a speed of 4000rpm for 60s. After spin coating, place it on a hot plate and bake it at 80°C for 3min. Then use a roller to bond the thermal release tape (TRT) to the surface of polyvinyl alcohol to form a thermal release tape / polyvinyl alcohol / antimony trioxide / graphene / copper / sapphire composite structure. It is then fixed on a carrier, and a mechanical peeling (1cm / s) device is used to slowly peel off the thermal release tape / polyvinyl alcohol / antimony trioxide / graphene from the copper surface, cut out 2cm*2cm, and the copper / sapphire growth substrate is cleaned with deionized water and ethanol, and then blown dry with nitrogen and placed in a wafer box for recovery. Afterwards, a roller press is used to bond it to the sapphire. The obtained thermal release tape / polyvinyl alcohol / antimony trioxide / graphene / sapphire was put into an oven and heated at 120°C for 30 minutes. The thermal release tape fell off, and the antimony trioxide / graphene / sapphire structure was immersed in deionized water for 30 minutes to remove the residual polyvinyl alcohol residue. The surface was washed with deionized water and blown dry with nitrogen to finally obtain a graphene wafer transferred to a 2-inch sapphire.

[0048] Comparative Example 1

[0049] Use a coating machine to spin-coat PMMA solution (950PMMA A4) on the surface of a 4-inch graphene wafer at a speed of 5000rpm for 60s. After spin coating, place it on a hot plate and bake it at a temperature of 130℃ for 3min. Then use a roller press to bond the thermal release tape (TRT) to the PMMA surface to form a TRT / PMMA / graphene / copper / sapphire composite structure. It is then fixed on a carrier and immersed in a sodium hydroxide solution with a concentration of 1mol / L. The negative electrode of the DC power supply is connected to the copper part of the composite structure, and the positive electrode is connected to a platinum sheet. During bubbling, the DC power supply applies a voltage of 6V for 5min. The TRT / PMMA / graphene wafer composite structure is then peeled off from the copper / sapphire using a wafer clamp and washed in deionized water for 3 times, 15min each time. The surface of the copper / sapphire growth substrate is cleaned with deionized water and ethanol, and then blown dry with nitrogen and recycled in a wafer box. After the cleaned TRT / PMMA / graphene wafer composite structure is naturally dried for 3 hours, it is bonded to the silicon wafer at 100°C using a roller press. The obtained TRT / PMMA / graphene wafer / silicon wafer is placed in an oven and heated at 120°C for 60 minutes to release the TRT and remove it. The obtained PMMA / graphene wafer / silicon wafer is placed on a hot plate and baked at 180°C for 3 hours. Then it is placed in a mixed solution of acetone and isopropanol in a ratio of 3:2 for degumming, soaked 3 times, 10 minutes each time, and stirred with a magnetic bar. Finally, it is blown dry with nitrogen to obtain a 4-inch graphene wafer transferred to the silicon wafer.

[0050] Figure 1 a and b are respectively a physical photo and an optical microscope photo of the graphene wafer transferred onto the silicon wafer in Example 1; c and d are respectively a physical photo and an optical microscope photo of the graphene wafer transferred onto the silicon wafer in Comparative Example 1. Figure 1 It can be observed that the graphene wafer in Example 1 has significantly higher integrity and cleanliness than that in Comparative Example 1.

[0051] Figure 2 Figures a and b are atomic force microscope images of graphene wafers of comparative example 1 and embodiment 1, respectively. The atomic force microscope (AFM) image results show that the surface contaminants remaining on the graphene wafer in embodiment 1 are significantly less than those in comparative example 1, and its surface roughness is lower and smoother. The AFM results show that the average roughness of the transferred packaging medium / graphene / target substrate composite structure is only 0.27nm, which is comparable to that of a silicon substrate.

[0052] Figure 3 The Raman spectra of the Sb2O3 encapsulated graphene after transfer in Example 1 and the transfer structure in Comparative Example 1 show that the Raman peak position statistics of Example 1 indicate that the transfer method of the present invention has less doping on graphene, and the transfer process has less impact on the quality of graphene.

[0053] Figure 4 The statistical results of the Raman spectra of Sb2O3 encapsulated graphene (a) after transfer in Example 1 and Comparative Example 1 (b) characterize the half-peak width of the 2D peak. The half-peak width of the 2D peak is related to the carrier mobility of graphene. The narrower the half-peak width, the higher the carrier mobility. The structure of the graphene upper surface encapsulated with antimony trioxide has a Raman 2D peak half-peak width of 27 cm -1 , compared with the graphene Raman 2D peak half-peak width (28.8 cm) transferred to the silicon wafer without encapsulation layer in comparative example 1 -1 ), indicating that Sb2O3 encapsulation reduces the doping and contamination of graphene and significantly improves the quality of graphene.

[0054] The integrity and cleanliness of the transferred graphene wafer in Example 2 are similar to those in Example 1, and are significantly better than those in Comparative Example 1.

[0055] Figure 5 A photograph of a graphene wafer transferred to a sapphire substrate prepared in Example 3 is shown. From the figure, it can be seen that the transferred graphene wafer is intact and clean.

[0056] This proves that the integrity and cleanliness of the graphene transferred by the method of the present invention are higher than those of the graphene obtained by the traditional PMMA transfer method.

[0057] Example 4

[0058] After mechanical peeling in Example 1, a roller press was used to bond to the gold-embedded silicon wafer, and the obtained thermal release tape / polyvinyl alcohol / antimony trioxide / graphene / gold-embedded silicon wafer was placed in an oven, heated at 120°C for 30 minutes, and then the edge of the silicon wafer was fixed with a clamp to peel off the supporting substrate. The antimony trioxide / graphene / gold-embedded silicon wafer structure was soaked in deionized water for 30 minutes to remove the residual polyvinyl alcohol residue, the surface was washed with deionized water, and dried with nitrogen to obtain a semiconductor device, and the micro-nano device was processed by electron beam exposure, electrode evaporation, etc.

[0059] Comparative Example 2

[0060] A micro-nano device was formed using the mechanically peeled structure of Comparative Example 1 in the same manner as Example 4.

[0061] Figure 6 The optical photograph of the micro-nano structure prepared in Example 4 is shown. As can be seen from the figure, the central blue part is graphene carrying antimony oxide.

[0062] The carrier mobility of the micro-nano devices prepared in Example 3 and Comparative Example 2 was tested. The test results are as follows: Fig. 7A and Figure 7B As shown. Fig. 7A The mobility of the device prepared in Example 4 can be calculated to be 12000 cm 2 / (V·s). Figure 7B The mobility of the device prepared in Comparative Example 2 can be calculated to be 7000 cm 2 / (V·s). This proves that the mobility of the graphene device encapsulated by the method of the present invention is higher. Based on the mechanical peeling of Example 2, the self-flowing electron mobility test results of the micro-nano device prepared in the same manner as Example 4 are similar to those of Example 4, and are significantly higher than the mobility of the device in Comparative Example 2.

[0063] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A method for transferring a graphene wafer, characterized in that: include: forming an encapsulation layer on the surface of a graphene wafer grown directly on a growth substrate; Spin coating an adhesive on the encapsulation layer to form an adhesive layer, and then laminating an adhesive support substrate to obtain a support substrate / encapsulation layer / graphene wafer / growth substrate composite structure; Separating the supporting substrate / packaging layer / graphene wafer from the growth substrate to obtain a supporting substrate / packaging layer / graphene wafer composite structure; Laminating the support substrate / encapsulation layer / graphene wafer composite structure to a target substrate; Thermally treating and separating the support substrate and the packaging layer to obtain a packaging layer / graphene wafer / target substrate composite structure; Wherein, the encapsulation layer is an antimony trioxide layer.

2. The method for transferring a graphene wafer according to claim 1, characterized in that: The encapsulation layer is formed on the surface of the graphene wafer by vacuum thermal evaporation, and the evaporation condition is a vacuum degree of 10 -5 -10 -7 Torr, evaporation rate 0.01-2nm / s.

3. The method for transferring a graphene wafer according to claim 1, wherein: The thickness of the encapsulation layer is greater than or equal to 3 nm; preferably, less than or equal to 20 μm.

4. The method for transferring a graphene wafer according to claim 1, characterized in that: The adhesive is polyvinyl alcohol, polymethyl methacrylate, polycarbonate, preferably polyvinyl alcohol; Preferably, the adhesive layer is formed by spin coating a solution containing polyvinyl alcohol on the surface of the encapsulation layer and then baking; the spin coating speed is 500-8000 rpm, the spin coating time is 30s-5min; the baking temperature is 50-200°C, and the baking time is 1-5min; preferably, the mass concentration of the polyvinyl alcohol in the solution is 0.1-20%; the solvent of the solution is water or ethanol; Preferably, the adhesive support substrate is a thermal release tape, a UV film or a silicone film, preferably a thermal release tape; the lamination method is roll lamination or vacuum lamination; Preferably, the target substrate is a silicon wafer or sapphire, preferably a silicon wafer; and the support substrate / encapsulation layer / graphene wafer composite structure is bonded to the target substrate by roll bonding or vacuum bonding.

5. The method for transferring a graphene wafer according to claim 1, characterized in that: Separating the support substrate / encapsulation layer / graphene wafer from the growth substrate by mechanical peeling; Preferably, the mechanical stripping is manual or mechanical device assisted stripping, and the stripping speed is 0.1-5 cm / s; Preferably, the thermal release tape is detached by placing the support substrate / encapsulation layer / graphene wafer / target substrate composite structure into a vacuum drying oven for heating, the heating temperature is 100-200° C., and the time is 20-60 min; Preferably, the encapsulation layer / graphene wafer / target substrate composite structure is immersed in an adhesive solvent to remove residual organic molecular impurities; preferably, the adhesive solvent is water or ethanol, the immersion temperature is 20-80° C., and the time is 1-10 min.

6. A graphene wafer packaging structure, characterized in that: The invention comprises a graphene wafer and an antimony trioxide encapsulation layer encapsulated on the surface of the graphene wafer.

7. The graphene wafer packaging structure according to claim 6, characterized in that: The thickness of the encapsulation layer is greater than or equal to 3 nm; preferably, less than or equal to 20 μm.

8. A method for packaging a graphene wafer, characterized in that: include: forming an encapsulation layer on the surface of a graphene wafer grown directly on a growth substrate; Wherein, the encapsulation layer is an antimony trioxide layer.

9. The method for packaging a graphene wafer according to claim 8, characterized in that: The encapsulation layer is formed on the surface of the graphene wafer by vacuum thermal evaporation, and the evaporation condition is a vacuum degree of 10 -5 -10 -7 Torr, and the evaporation rate is 0.01-2nm / s.

10. A semiconductor device, characterized in that: Comprising the graphene wafer packaging structure as described in claim 6 or 7.