Semiconductor structure and preparation method thereof, and memory
By using ohmic contact and heat treatment to form a conductive layer in the semiconductor structure, the contact resistance between the source and drain electrode and the channel material is reduced, the problem of current reduction during microscopic shrinkage is solved, and a higher open-state current is achieved.
Patent Information
- Application Number
- CN202310636680.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-31
- Publication Date
- 2024-12-03
AI Technical Summary
During the miniaturization of a semiconductor device, the contact area between the source and drain electrode and the semiconductor material decreases, resulting in an increase in contact resistance, affecting the open-state current of the device, and thus limiting further reduction of the device size.
A semiconductor structure is designed in which the channel layer forms ohmic contact with the first conductive layer through the second conductive layer, the channel layer forms ohmic contact with the third conductive layer through the fourth conductive layer, and the initial electrode part is oxidized to form conductive by heat treatment. layer, thereby reducing contact resistance between the source and drain electrode and channel material.
Without increasing the device size, the open-state current of the semiconductor device is significantly increased, solving the problem of increasing contact resistance.
Smart Images

Figure CN119069516A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of semiconductor technology. Specifically, the present application relates to a semiconductor structure and a preparation method thereof, and a memory. Background Art
[0002] With the development and progress of technology, semiconductor devices are constantly moving towards miniaturization and high integration. As the basic unit of storage technology, the miniaturization of transistors can further realize the miniaturization of storage units and improve the density of storage units.
[0003] However, in the process of miniaturization, it is necessary to ensure device performance (such as on-state current). The reduction in size of semiconductor devices can easily lead to a reduction in the contact area between the source and drain of the transistor and the semiconductor material, an increase in contact resistance, and a significant reduction in the on-state current of the semiconductor device, affecting the operating speed of the semiconductor device; and in order to reduce the contact resistance between the source and drain and the semiconductor material and ensure sufficient on-state current, it is difficult to reduce the contact area between the source and drain and the semiconductor material, which has become a problem that limits the miniaturization of semiconductor devices. Summary of the invention
[0004] In view of the shortcomings of the existing methods, the present application proposes a semiconductor structure and a preparation method thereof, and a memory, which can increase the on-state current of the device without increasing the size of the device.
[0005] In a first aspect, an embodiment of the present application provides a semiconductor structure, including:
[0006] substrate;
[0007] A channel layer is disposed on one side of the substrate, and at least a portion of the channel layer extends in a direction perpendicular to the substrate;
[0008] A first electrode is located on a side of the channel layer facing the substrate, and the channel layer is in contact with the first electrode;
[0009] A second electrode is arranged on one side of the substrate and surrounds the outer periphery of the channel layer. The channel layer contacts the second electrode. The extension direction of the second electrode forms an angle with the extension direction of the first electrode. The second electrode is insulated from the first electrode.
[0010] in:
[0011] The first electrode includes a first conductive layer and a second conductive layer, and the first conductive layer and the second conductive layer are arranged in sequence along the direction from the substrate to the channel layer, and the channel layer forms an ohmic contact with the first conductive layer through the second conductive layer; and / or,
[0012] The second electrode includes a third conductive layer and a fourth conductive layer. The third conductive layer is located on a side of the fourth conductive layer away from the channel layer. The channel layer forms an ohmic contact with the third conductive layer through the fourth conductive layer.
[0013] In some optional embodiments of the present application, the material of the channel layer includes an oxide semiconductor material;
[0014] The material of the first conductive layer is aluminum, and the material of the second conductive layer is aluminum oxide; and / or,
[0015] The material of the third conductive layer is aluminum, and the material of the fourth conductive layer is aluminum oxide.
[0016] In some optional embodiments of the present application, the substrate has a first groove, the opening of the first groove faces the side where the channel layer is located, and the first groove extends along a first direction parallel to the substrate;
[0017] The first conductive layer and the second conductive layer are both disposed in the first groove, and the second conductive layer is located on a side of the first conductive layer facing an opening of the first groove.
[0018] In some optional embodiments of the present application, the semiconductor structure further includes an insulating layer, which is disposed on one side of the substrate and covers a portion of the first conductive layer, and the second electrode is located on a side of the insulating layer away from the substrate;
[0019] The semiconductor structure has a first through hole penetrating the second electrode and the insulating layer, the first through hole exposes the second conductive layer, and the channel layer at least covers the inner wall of the first through hole, so that the channel layer contacts the second electrode and the second conductive layer respectively.
[0020] In some optional embodiments of the present application, the insulating layer has a second groove, the opening of the second groove faces the side of the insulating layer away from the substrate, the second groove extends along a second direction parallel to the substrate, the second electrode is arranged in the second groove, and the orthographic projection of the first through hole on the substrate overlaps with the orthographic projection of the second groove on the substrate; and / or,
[0021] The fourth conductive layer of the second electrode is arranged around the periphery of the first through hole, and the third conductive layer of the second electrode is located on a side of the fourth conductive layer away from the first through hole.
[0022] In some optional embodiments of the present application, the semiconductor structure further includes an insulating layer, which is disposed on one side of the substrate and covers a portion of the first electrode, and the second electrode is located on a side of the insulating layer away from the substrate;
[0023] The semiconductor structure has a first through hole, and the fourth conductive layer is arranged around the periphery of the first through hole. The first through hole penetrates the insulating layer and exposes the first electrode. The channel layer at least covers the inner wall of the first through hole, so that the channel layer contacts the fourth conductive layer and the first electrode respectively, and the third conductive layer is located on the side of the fourth conductive layer away from the first through hole.
[0024] In some optional embodiments of the present application, the semiconductor structure further includes:
[0025] A first dielectric layer is arranged on a side of the second electrode away from the substrate and covers the second electrode and the insulating layer, wherein the first through hole penetrates the first dielectric layer and extends in a direction perpendicular to the substrate;
[0026] A gate dielectric layer is disposed on a side of the channel layer away from the substrate, and at least a portion of the gate dielectric layer is located in the first through hole;
[0027] The gate is arranged on a side of the gate dielectric layer away from the substrate and fills the first through hole.
[0028] In a second aspect, an embodiment of the present application provides a memory, comprising: the above-mentioned semiconductor structure.
[0029] In a third aspect, an embodiment of the present application provides a method for preparing a semiconductor structure, comprising:
[0030] Providing a substrate and manufacturing a first initial electrode, wherein the first initial electrode is located on one side of the substrate;
[0031] A second initial electrode is formed on one side of the substrate, wherein the extension direction of the second initial electrode is arranged at an angle with the extension direction of the first initial electrode, and the second initial electrode is insulated from the first initial electrode;
[0032] Making a first through hole penetrating the second initial electrode, wherein the first through hole extends in a direction perpendicular to the substrate, and the first through hole exposes the first initial electrode;
[0033] Manufacturing a channel layer, the channel layer at least covering the inner wall of the first through hole, so that the first initial electrode is located on the side of the channel layer facing the substrate, the second initial electrode is arranged around the outer periphery of the channel layer, and the channel layer is in contact with the first initial electrode and the second initial electrode respectively; and
[0034] A heat treatment is performed to oxidize a portion of the first initial electrode in contact with the channel layer, and a portion of the first initial electrode that is not oxidized forms a first conductive layer, and a portion that is oxidized forms a second conductive layer. The first conductive layer and the second conductive layer form a first electrode, and the channel layer forms an ohmic contact with the first conductive layer through the second conductive layer; and / or, a portion of the second initial electrode in contact with the channel layer is oxidized, and a portion of the second initial electrode that is not oxidized forms a third conductive layer, and a portion that is oxidized forms a fourth conductive layer. The third conductive layer and the fourth conductive layer form a second electrode, and the channel layer forms an ohmic contact with the third conductive layer through the fourth conductive layer.
[0035] In some optional embodiments of the present application, a substrate is provided, and a first initial electrode is manufactured, including:
[0036] providing an initial substrate;
[0037] A first groove is formed on an initial substrate, wherein the first groove extends along a first direction, and the initial substrate having the first groove formed thereon forms a substrate;
[0038] Depositing aluminum material in the first groove to form a first initial electrode layer, wherein the first initial electrode layer fills the first groove;
[0039] The first initial electrode layer is planarized, and the planarized first initial electrode layer forms a first initial electrode.
[0040] In some optional embodiments of the present application, manufacturing the second initial electrode includes:
[0041] Forming an initial insulating layer on one side of the substrate, wherein the initial insulating layer covers the first initial electrode;
[0042] A second groove is formed on the initial insulating layer, the second groove extends along a second direction, and the initial insulating layer having the second groove is formed into an insulating layer;
[0043] Depositing aluminum material in the second groove to form a second initial electrode layer, the second initial electrode layer fills the second groove, and the orthographic projection of the second initial electrode layer on the substrate has an overlapping area with the orthographic projection of the first initial electrode layer on the substrate;
[0044] The second initial electrode layer is planarized, and the planarized second initial electrode layer forms a second initial electrode.
[0045] In some optional embodiments of the present application, before forming the first through hole, the method for preparing the semiconductor structure further includes:
[0046] Forming a first dielectric layer on a side of the insulating layer away from the substrate, wherein the first dielectric layer covers at least a portion of the second initial electrode;
[0047] Making a first through hole, comprising:
[0048] Graphic processing is performed to form a first through hole that sequentially penetrates the first dielectric layer, the second initial electrode and the insulating layer, wherein the orthographic projection of the first through hole on the substrate is located in the overlapping area, and the first through hole exposes the first initial electrode.
[0049] In some optional embodiments of the present application, fabricating a channel layer includes:
[0050] depositing an oxide semiconductor material in the first through hole to form a channel layer;
[0051] Heat treatment is performed, including:
[0052] By annealing, the portion of the first initial electrode in contact with the channel layer is spontaneously oxidized to form an aluminum oxide film, the portion of the first initial electrode that is not oxidized forms the first conductive layer, and the aluminum oxide film formed by oxidation forms the second conductive layer; and / or,
[0053] The portion of the second initial electrode in contact with the channel layer is spontaneously oxidized to form an aluminum oxide film, the portion of the second initial electrode that is not oxidized forms a third conductive layer, and the aluminum oxide film formed by oxidation forms a fourth conductive layer.
[0054] In some optional embodiments of the present application, after the heat treatment, the method for preparing the semiconductor structure further includes:
[0055] A gate dielectric layer is formed on a side of the channel layer away from the substrate, wherein at least a portion of the gate dielectric layer is located in the first through hole;
[0056] A gate is formed on a side of the gate dielectric layer away from the substrate, and at least a portion of the gate is located in the first through hole.
[0057] The beneficial technical effects brought about by the technical solution provided by the embodiment of the present application include:
[0058] In the embodiment of the present application, the channel layer forms an ohmic contact with the first conductive layer through the second conductive layer, and the channel layer forms an ohmic contact with the third conductive layer through the fourth conductive layer. The technical solution of the present application can effectively reduce the contact resistance between the source and drain and the channel material without increasing the size of the device, thereby significantly improving the on-state current of the semiconductor device.
[0059] Additional aspects and advantages of the present application will be partially given in the following description, which will become apparent from the following description, or will be understood through the practice of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0060] The above and / or additional aspects and advantages of the present application will become apparent and easily understood from the following description of the embodiments in conjunction with the accompanying drawings, in which:
[0061] Figure 1 A schematic diagram of a process for preparing a semiconductor structure provided in an embodiment of the present application;
[0062] Figures 2 to 13 A schematic diagram of a semiconductor structure preparation method according to an embodiment of the present invention at different stages ( Figure 6 Shows Figure 5 AA section view, Figures 7 to 13 Shows Figure 6 (Schematic diagram of the structure of B when it is in different processes).
[0063] Reference numerals:
[0064] 100-semiconductor structure; 10-substrate; 11-first groove; 20-channel layer; 30-first electrode; 31-first conductive layer; 32-second conductive layer; 33-first initial electrode; 40-second electrode; 41-third conductive layer; 42-fourth conductive layer; 43-second initial electrode; 50-insulating layer; 51-second groove; 52-initial insulating layer; 60-first through hole; 70-first dielectric layer; 80-gate dielectric layer; 90-gate; 110-second dielectric layer; 111-second through hole; 120-connection structure. DETAILED DESCRIPTION
[0065] The embodiments of the present application are described below in conjunction with the drawings in the present application. It should be understood that the implementation methods described below in conjunction with the drawings are exemplary descriptions for explaining the technical solutions of the embodiments of the present application and do not constitute a limitation on the technical solutions of the embodiments of the present application.
[0066] It will be understood by those skilled in the art that, unless specifically stated, the singular forms "one", "an", "said" and "the" used herein may also include plural forms. It should be further understood that the term "comprising" used in the specification of the present application refers to the presence of the features, integers, steps, operations, elements and / or components, but does not exclude the implementation of other features, information, data, steps, operations, elements, components and / or combinations thereof supported by the present technical field. It should be understood that when we refer to an element as being "connected" or "coupled" to another element, the element may be directly connected or coupled to the other element, or may refer to the connection relationship between the element and the other element established through an intermediate element. In addition, the "connection" or "coupling" used herein may include wireless connection or wireless coupling. The term "and / or" used herein refers to at least one of the items defined by the term, for example, "A and / or B" may be implemented as "A", or as "B", or as "A and B".
[0067] In order to make the objectives, technical solutions and advantages of the present application clearer, the implementation methods of the present application will be further described in detail below with reference to the accompanying drawings.
[0068] First, several terms involved in this application are introduced and explained:
[0069] Ohmic contact: When metal and semiconductor are in contact, they can form a non-rectifying contact, that is, an ohmic contact, which does not produce significant additional impedance and does not significantly change the equilibrium carrier concentration inside the semiconductor. Electrically speaking, the contact resistance of an ideal ohmic contact should be very small compared to the semiconductor sample or device. When current flows through, the voltage drop on the ohmic contact should be much smaller than the voltage drop of the sample or device itself.
[0070] Schottky contact: refers to a metal-semiconductor contact with rectification characteristics. When metal and semiconductor materials come into contact, the energy band of the semiconductor bends at the interface to form a Schottky barrier. The existence of the barrier leads to a large interface resistance. The corresponding is the ohmic contact, where the barrier at the interface is very small or there is no contact barrier.
[0071] The following is an explanation of the relevant technologies:
[0072] The source, drain and channel materials generally form Schottky contacts, and there is a large resistance at the contact interface. This characteristic determines that the contact area between the source, drain and channel materials is difficult to reduce, which becomes a problem that limits the miniaturization of semiconductor devices. This problem still exists in vertical channel semiconductor devices.
[0073] The traditional solution is to increase the area of the source and drain metal, and in vertical channel semiconductor devices, the solution is to increase the thickness of the source and drain metal layer to increase the contact area between the source and drain and the channel material, thereby reducing resistance. However, this solution is not practical due to limitations such as stress and etching process, and increasing the area or thickness is not conducive to achieving the miniaturization of semiconductor devices.
[0074] The semiconductor structure and its preparation method, memory, and electronic device provided in the present application are intended to solve at least one of the above technical problems in the prior art.
[0075] The following is a detailed description of the technical solution of the present application and how the technical solution of the present application solves the above technical problems with specific embodiments. It should be noted that the following implementations can refer to, draw on or combine with each other, and the same terms, similar features and similar implementation steps in different implementations will not be described repeatedly.
[0076] A schematic diagram of a method for preparing a semiconductor structure provided in an embodiment of the present application is as follows: Figure 1 As shown, a schematic diagram of the structure of a semiconductor structure preparation method provided in an embodiment of the present application at different processes is shown in FIG. Figures 2 to 13 As shown, a schematic diagram of a semiconductor structure provided in an embodiment of the present application is shown in Figures 10 to 13As shown, it includes: a substrate 10, a channel layer 20, a first electrode 30 and a second electrode 40, the channel layer 20 is arranged on one side of the substrate 10, and at least a portion of the channel layer 20 extends in a direction perpendicular to the substrate 10; the first electrode 30 is located on the side of the channel layer 20 facing the substrate 10, and the channel layer 20 is in contact with the first electrode 30; the second electrode 40 is arranged on one side of the substrate 10 and is arranged around the periphery of the channel layer 20, the channel layer 20 is in contact with the second electrode 40, the extension direction of the second electrode 40 is arranged at an angle to the extension direction of the first electrode 30, and the second electrode 40 is insulated from the first electrode 30. Wherein: the first electrode 30 includes a first conductive layer 31 and a second conductive layer 32, and the first conductive layer 31 and the second conductive layer 32 are arranged in sequence along the direction pointing from the substrate 10 to the channel layer 20, and the channel layer 20 forms an ohmic contact with the first conductive layer 31 through the second conductive layer 32; the second electrode 40 includes a third conductive layer 41 and a fourth conductive layer 42, and the third conductive layer 41 is located on a side of the fourth conductive layer 42 away from the channel layer 20, and the channel layer 20 forms an ohmic contact with the third conductive layer 41 through the fourth conductive layer 42.
[0077] In the embodiment of the present application, the substrate 10 supports the channel layer 20, the first electrode 30 and the second electrode 40. At least part of the channel layer 20 extends in a direction perpendicular to the substrate 10 to form a vertical channel, which can reduce the horizontal dimension of the semiconductor structure 100 in a direction parallel to the substrate 10 and provide a higher channel current; the first electrode 30 is located on the side of the channel layer 20 facing the substrate 10, and the second electrode 40 is arranged around the periphery of the channel layer 20. The semiconductor structure 100 is a ring channel type semiconductor device structure, and the channel layer 20 is in contact with the first electrode 30 and the second electrode 40 respectively. The first electrode 30 can be one of the source and the drain of the semiconductor structure 100, and the second electrode 40 can be the other of the source and the drain of the semiconductor structure 100. The part of the channel layer 20 located between the first electrode 30 and the second electrode 40 in the power-on state forms a channel. There is a channel between the source and the drain of the transistor, and the current can flow through the drain, the channel and the source. In the embodiment of the present application, a portion of the structure of the channel layer 20 forms a vertical channel, that is, the transmission direction of carriers in the channel is perpendicular to the substrate 10 .
[0078] Studies have shown that the aluminum-aluminum oxide-oxide semiconductor material (such as IGZO) heterojunction is an ohmic contact. In the embodiment of the present application, the material of the channel layer 20 includes an oxide semiconductor material, the material of the first conductive layer 31 is aluminum, the material of the second conductive layer 32 is aluminum oxide, the material of the third conductive layer 41 is aluminum, and the material of the fourth conductive layer 42 is aluminum oxide, so that the channel layer 20 forms an ohmic contact with the first conductive layer 31 through the second conductive layer 32, and the channel layer 20 forms an ohmic contact with the third conductive layer 41 through the fourth conductive layer 42. Compared with the technology of forming a Schottky contact between the source and drain and the channel material, the technical solution of the present application can greatly reduce the contact resistance between the source and drain and the channel material, thereby significantly improving the on-state current of the semiconductor device.
[0079] Based on the structure of a ring-channel semiconductor device, the technical solution of the present application can effectively reduce the contact resistance between the source, drain and channel material without increasing the size of the device, thereby increasing the on-state current of the semiconductor device by at least one order of magnitude.
[0080] Of course, in some optional embodiments of the present application, according to actual needs, only the first electrode 30 includes the first conductive layer 31 and the second conductive layer 32, and the first conductive layer 31 and the second conductive layer 32 are arranged in sequence along the direction pointing from the substrate 10 to the channel layer 20, and the channel layer 20 forms an ohmic contact with the first conductive layer 31 through the second conductive layer 32. At this time, the structure and materials of the second electrode 40 can adopt conventional technologies in the field. For example, the material of the second electrode 40 can be aluminum or other materials; or, only the second electrode 40 includes the third conductive layer 41 and the fourth conductive layer 42, and the third conductive layer 41 is located on the side of the fourth conductive layer 42 away from the channel layer 20, and the channel layer 20 forms an ohmic contact with the third conductive layer 41 through the fourth conductive layer 42. At this time, the structure and materials of the first electrode 30 can adopt conventional technologies in the field. For example, the material of the first electrode 30 can be aluminum or other materials.
[0081] In some optional embodiments of the present application, the first electrode 30 may also serve as a bit line, and the second electrode 40 may also serve as a word line.
[0082] In some optional embodiments of the present application, such as Figure 4 , Figures 10 to 13As shown, the substrate 10 has a first groove 11, the opening of the first groove 11 faces the side where the channel layer 20 is located, and the first groove 11 extends along a first direction parallel to the substrate 10. The first electrode 30 is arranged in the first groove 11, and the first electrode 30 extends along the first direction. Compared with the technology of arranging the first electrode on one side of the substrate, resulting in a larger size in the direction perpendicular to the substrate (for example, approximately equal to the sum of the thickness of the substrate and the size of the first electrode in the direction perpendicular to the substrate), in the present application, the first electrode 30 is arranged in the first groove 11 of the substrate 10 (the size in the direction perpendicular to the substrate 10 is less than the sum of the thickness of the substrate and the size of the first electrode in the direction perpendicular to the substrate), which is conducive to reducing the size of the semiconductor structure 100 in the direction perpendicular to the substrate 10.
[0083] In some optional embodiments of the present application, such as Figures 10 to 13 As shown, the first electrode 30 includes a first conductive layer 31 and a second conductive layer 32. The first conductive layer 31 forms an ohmic contact with the channel layer 20 through the second conductive layer 32, which can reduce the contact resistance between the source and drain and the channel material, and significantly improve the on-state current of the semiconductor device. The first conductive layer 31 and the second conductive layer 32 are both arranged in the first groove 11. The first groove 11 is used to accommodate the first conductive layer 31 and the second conductive layer 32, and the second conductive layer 32 is located on the opening side of the first conductive layer 31 facing the first groove 11, so that the second conductive layer 32 is in contact with the channel layer 20. The first conductive layer 31 and the second conductive layer 32 both extend along the first direction. Optionally, the material of the first conductive layer 31 is aluminum, and the material of the second conductive layer 32 is aluminum oxide.
[0084] In some optional embodiments of the present application, such as Figures 10 to 13 As shown, the semiconductor structure 100 further includes an insulating layer 50, which is disposed on one side of the substrate 10 and covers a portion of the first electrode 30, and the second electrode 40 is located on a side of the insulating layer 50 away from the substrate 10, so that the first electrode 30 and the second electrode 40 are insulated. Optionally, the material of the insulating layer 50 is silicon oxide. The semiconductor structure 100 has a first through hole 60 that penetrates the second electrode 40 and the insulating layer 50, and the first through hole 60 exposes the first electrode 30. The channel layer 20 at least covers the inner wall of the first through hole 60, so that the channel layer 20 is in contact with the first electrode 30 and the second electrode 40, respectively.
[0085] In some optional embodiments of the present application, such as Figures 10 to 13 As shown, the first electrode 30 includes a first conductive layer 31 and a second conductive layer 32 , the insulating layer 50 covers a portion of the first conductive layer 31 , the first through hole 60 exposes the second conductive layer 32 , and the channel layer 20 contacts the second conductive layer 32 .
[0086] In some optional embodiments of the present application, such as Figures 10 to 13As shown, the second electrode 40 includes a third conductive layer 41 and a fourth conductive layer 42. The third conductive layer 41 is in ohmic contact with the channel layer 20 through the fourth conductive layer 42, which can reduce the contact resistance between the source and drain and the channel material, and significantly improve the on-state current of the semiconductor device. The fourth conductive layer 42 is arranged around the periphery of the first through hole 60, and the third conductive layer 41 is located on the side of the fourth conductive layer 42 away from the first through hole 60, that is, the fourth conductive layer 42 is located on the side of the third conductive layer 41 facing the first through hole 60, so that the fourth conductive layer 42 is in contact with the channel layer 20. Optionally, the material of the third conductive layer 41 is aluminum, and the material of the fourth conductive layer 42 is aluminum oxide.
[0087] In some optional embodiments of the present application, such as Figures 10 to 13 As shown, along the second direction (along Fig.10 In the left-right direction, the third conductive layer 41 is located on a side of the fourth conductive layer 42 away from the first through hole 60 .
[0088] In some optional embodiments of the present application, such as Figures 4 to 8 As shown, the insulating layer 50 has a second groove 51, the opening of the second groove 51 is toward the side of the insulating layer 50 away from the substrate 10, the second groove 51 extends along a second direction parallel to the substrate 10, the first direction and the second direction are set at an angle, the second electrode 40 is set in the second groove 51, the second groove 51 is used to accommodate the second electrode 40, the second electrode 40 extends along the second direction, and the orthographic projection of the first through hole 60 on the substrate 10 overlaps with the orthographic projection of the second groove 51 on the substrate 10, so that the first through hole 60 passes through the second electrode 40.
[0089] Of course, in some optional embodiments of the present application, according to actual needs, only the first electrode 30 includes the first conductive layer 31 and the second conductive layer 32. In this case, the insulating layer 50 covers part of the first conductive layer 31, the first through hole 60 exposes the second conductive layer 32, and the channel layer 20 contacts the second conductive layer 32 and the second electrode 40 respectively; or, only the second electrode 40 includes the third conductive layer 41 and the fourth conductive layer 42. In this case, the insulating layer 50 covers part of the first electrode 30, the first through hole 60 exposes the first electrode 30, and the channel layer 20 contacts the first electrode 30 and the fourth conductive layer 42 respectively.
[0090] In some optional embodiments of the present application, such as Figures 10 to 13As shown, the semiconductor structure 100 further includes: a first dielectric layer 70, a gate dielectric layer 80 and a gate 90. The first dielectric layer 70 is arranged on a side of the second electrode 40 away from the substrate 10 and covers the second electrode 40 and the insulating layer 50. The first dielectric layer 70 is used to insulate and separate the second electrode 40 and the gate 90. The first through hole 60 penetrates the first dielectric layer 70, and the first through hole 60 extends in a direction perpendicular to the substrate 10. The gate dielectric layer 80 is arranged on a side of the channel layer 20 away from the substrate 10, and at least a portion of the gate dielectric layer 80 is located in the first through hole 60. The gate dielectric layer 80 is used to insulate and isolate the channel layer 20 and the gate 90. The gate 90 is arranged on a side of the gate dielectric layer 80 away from the substrate 10 and fills the first through hole 60. The gate 90 can control the semiconductor structure 100 (for example, the semiconductor structure 100 can be a transistor) to be turned on or off.
[0091] Optionally, the material of the first dielectric layer 70 includes but is not limited to silicon oxide. The material of the gate dielectric layer 80 includes but is not limited to silicon oxide, silicon nitride or silicon oxynitride, or a high dielectric constant material such as hafnium oxide. The material of the gate 90 includes but is not limited to titanium or tungsten.
[0092] In the embodiments of the present application, the semiconductor structure relates to the field of semiconductor devices, and the semiconductor structure may be a transistor structure, and specifically, may be an improved vertical channel transistor device structure.
[0093] Based on the same inventive concept, the present application embodiment provides a method for preparing a semiconductor structure. The process diagram of the method for preparing a semiconductor structure is as follows: Figure 1 As shown, the structural schematic diagram of the semiconductor structure in different processes in the preparation method is as follows Figures 2 to 13 As shown, the method for preparing the semiconductor structure includes:
[0094] S101, providing a substrate 10, and manufacturing a first initial electrode 33, wherein the first initial electrode 33 is located on one side of the substrate 10;
[0095] S102, manufacturing a second initial electrode 43 on one side of the substrate 10, wherein the extension direction of the second initial electrode 43 is arranged at an angle with the extension direction of the first initial electrode 33, and the second initial electrode 43 is insulated from the first initial electrode 33;
[0096] S103, making a first through hole 60 penetrating the second initial electrode 43, the first through hole 60 extending in a direction perpendicular to the substrate 10, and the first through hole 60 exposing the first initial electrode 33;
[0097] S104, manufacturing the channel layer 20, such as Figure 8As shown, the channel layer 20 at least covers the inner wall of the first through hole 60, so that the first initial electrode 33 is located on the side of the channel layer 20 facing the substrate 10, and the second initial electrode 43 is arranged around the outer periphery of the channel layer 20, so that the channel layer 20 is in contact with the first initial electrode 33 and the second initial electrode 43 respectively; optionally, the channel layer 20 can be formed by a deposition method;
[0098] S105, performing heat treatment to oxidize the portion of the first initial electrode 33 in contact with the channel layer 20, the portion of the first initial electrode 33 that is not oxidized forms the first conductive layer 31, the portion that is oxidized forms the second conductive layer 32, the first conductive layer 31 and the second conductive layer 32 form the first electrode 30, and the channel layer 20 forms an ohmic contact with the first conductive layer 31 through the second conductive layer 32; and oxidize the portion of the second initial electrode 43 in contact with the channel layer 20, the portion of the second initial electrode 43 that is not oxidized forms the third conductive layer 41, the portion that is oxidized forms the fourth conductive layer 42, the third conductive layer 41 and the fourth conductive layer 42 form the second electrode 40, and the channel layer 20 forms an ohmic contact with the third conductive layer 41 through the fourth conductive layer 42, as shown in FIG. Fig. 9 shown.
[0099] In the embodiments of the present application, the method for preparing a semiconductor structure can be used to manufacture the semiconductor structure in any embodiment of the present application.
[0100] In the embodiment of the present application, the substrate 10 supports the channel layer 20, the first electrode 30 and the second electrode 40. At least part of the channel layer 20 extends in a direction perpendicular to the substrate 10 to form a vertical channel, which can reduce the horizontal dimension of the semiconductor structure 100 in a direction parallel to the substrate 10 and provide a higher channel current; the first electrode 30 is located on the side of the channel layer 20 facing the substrate 10, and the second electrode 40 is arranged around the periphery of the channel layer 20. The semiconductor structure 100 is a ring channel type semiconductor device structure, and the channel layer 20 is in contact with the first electrode 30 and the second electrode 40 respectively. The first electrode 30 can be one of the source and the drain of the semiconductor structure 100, and the second electrode 40 can be the other of the source and the drain of the semiconductor structure 100. The part of the channel layer 20 located between the first electrode 30 and the second electrode 40 in the power-on state forms a channel. There is a channel between the source and the drain of the transistor, and the current can flow through the drain, the channel and the source. In the embodiment of the present application, a portion of the structure of the channel layer 20 forms a vertical channel, that is, the transmission direction of carriers in the channel is perpendicular to the substrate 10 .
[0101] In the embodiment of the present application, through heat treatment, the portion of the first initial electrode 33 in contact with the channel layer 20 is oxidized to form the second conductive layer 32, and the portion of the second initial electrode 43 in contact with the channel layer 20 is oxidized to form the fourth conductive layer 42. No additional patterning process is required, and the horizontal size of the semiconductor device (the size in the direction parallel to the substrate 10) will not be increased.
[0102] The technical solution of the present application is based on the structure of a ring-channel semiconductor device. Without adding an additional graphic process or increasing the size of the device, it is possible to form a channel layer 20 made of an oxide semiconductor material, a first conductive layer 31 made of aluminum, a second conductive layer 32 made of aluminum oxide, a third conductive layer 41 made of aluminum, and a fourth conductive layer 42 made of aluminum oxide, so that the channel layer 20 forms an ohmic contact with the first conductive layer 31 through the second conductive layer 32, and the channel layer 20 forms an ohmic contact with the third conductive layer 41 through the fourth conductive layer 42, which can greatly reduce the contact resistance between the source and drain and the channel material, thereby significantly improving the on-state current of the semiconductor device (for example, increasing the on-state current of the semiconductor device by at least one order of magnitude).
[0103] Of course, in some optional embodiments of the present application, the method for preparing the semiconductor structure may also include, according to actual needs:
[0104] S105, performing heat treatment to oxidize only the portion of the first initial electrode 33 that contacts the channel layer 20, the portion of the first initial electrode 33 that is not oxidized forms the first conductive layer 31, the portion that is oxidized forms the second conductive layer 32, the first conductive layer 31 and the second conductive layer 32 form the first electrode 30, the channel layer 20 forms an ohmic contact with the first conductive layer 31 through the second conductive layer 32, at this time, the second initial electrode 43 forms the second electrode 40; or, oxidize only the portion of the second initial electrode 43 that contacts the channel layer 20, the portion of the second initial electrode 43 that is not oxidized forms the third conductive layer 41, the portion that is oxidized forms the fourth conductive layer 42, the third conductive layer 41 and the fourth conductive layer 42 form the second electrode 40, the channel layer 20 forms an ohmic contact with the third conductive layer 41 through the fourth conductive layer 42, at this time, the first initial electrode 33 forms the first electrode 30.
[0105] In some optional embodiments of the present application, such as Figure 2 As shown, a substrate 10 is provided, and a first initial electrode 33 is made of aluminum material, including:
[0106] Providing an initial substrate; optionally, the material of the initial substrate is an insulating material;
[0107] A first groove 11 is formed on an initial substrate, the first groove 11 extends along a first direction, and the initial substrate with the first groove 11 forms a substrate 10; specifically, the opening of the first groove 11 faces one side of the initial substrate; optionally, the first groove 11 can be formed on the initial substrate by a patterning process, optionally, the shape and position of the first groove 11 to be formed on the initial substrate can be defined by a photolithography process, and then the first groove 11 can be etched on the initial substrate by a dry etching process; optionally, the substrate 10 is an insulating substrate;
[0108] Aluminum material is deposited in the first groove 11 to form a first initial electrode layer, and the first initial electrode layer fills the first groove 11; optionally, the aluminum material can be deposited by a deposition method such as chemical vapor deposition (CVD);
[0109] The first initial electrode layer is planarized so that the surface of the first initial electrode layer away from the first groove 11 is flush with the surface of the substrate 10, and the planarized first initial electrode layer forms the first initial electrode 33. Optionally, the planarization can be performed by chemical mechanical polishing (CMP).
[0110] In some optional embodiments of the present application, the first groove 11 may be formed on the initial substrate by direct etching, and the first groove 11 may be formed on the initial substrate and aluminum material may be deposited to form the first initial electrode layer by Damascus process.
[0111] In some optional embodiments of the present application, such as Figure 3 and Figure 4 As shown, manufacturing the second initial electrode 43 includes:
[0112] An initial insulating layer 52 is formed on one side of the substrate 10, and the initial insulating layer 52 covers the first initial electrode 33; optionally, the material of the initial insulating layer 52 can be any insulating medium, such as silicon oxide, silicon nitride, aluminum oxide, etc., and the initial insulating layer 52 can be formed by deposition, and the deposition method includes but is not limited to CVD, physical vapor deposition (Physical Vapor Deposition, referred to as PVD), atomic layer deposition (Atomic Layer Deposition, referred to as ALD) and other methods;
[0113] A second groove 51 is formed on the initial insulating layer 52, and the second groove 51 extends along the second direction. The initial insulating layer 52 with the second groove 51 forms an insulating layer 50, wherein both the first direction and the second direction are formed at an angle with the substrate 10. Specifically, the opening of the second groove 51 faces the side of the initial insulating layer 52 away from the substrate 10. The length of the channel to be formed can be defined according to the thickness of the insulating layer 50.
[0114] In some optional embodiments of the present application, such as Figure 4 As shown, manufacturing the second initial electrode 43 also includes:
[0115] Aluminum material is deposited in the second groove 51 to form a second initial electrode layer, the second initial electrode layer fills the second groove 51, and the orthographic projection of the second initial electrode layer on the substrate 10 has an overlapping area with the orthographic projection of the first initial electrode layer on the substrate 10;
[0116] The second initial electrode layer is planarized so that the surface of the second initial electrode layer away from the second groove 51 is flush with the surface of the insulating layer 50 away from the substrate 10 . The planarized second initial electrode layer forms the second initial electrode 43 .
[0117] It should be noted that, in the embodiment of the present application, the steps of opening a second groove, depositing aluminum material to form a second initial electrode layer, and flattening the second initial electrode layer can adopt the same or similar process method as the above-mentioned steps of opening a first groove, depositing aluminum material to form a first initial electrode layer, and flattening the first initial electrode layer, and will not be repeated here.
[0118] In some optional embodiments of the present application, such as Figure 5 and Figure 6 As shown, before forming the first through hole 60, the method for preparing the semiconductor structure further includes:
[0119] A first dielectric layer 70 is formed on a side of the insulating layer 50 away from the substrate 10 , and the first dielectric layer 70 covers at least a portion of the second initial electrode 43 .
[0120] In some optional embodiments of the present application, such as Figure 7 As shown, making the first through hole 60 includes:
[0121] A patterning process is performed to form a first through hole 60 that sequentially penetrates the first dielectric layer 70, the second initial electrode 43, and the insulating layer 50. The orthographic projection of the first through hole 60 on the substrate 10 is located in the overlapping region, and the first through hole 60 exposes the first initial electrode 33. Optionally, the shape and position of the first through hole 60 to be formed can be defined by a photolithography process, and then the first through hole 60 is formed by an etching process.
[0122] In some optional embodiments of the present application, fabricating the channel layer includes:
[0123] An oxide semiconductor material is deposited in the first through hole 60 to form a channel layer 20 ; optionally, the material of the channel layer 20 may be indium gallium zinc oxide (IGZO), indium tin oxide (ITO), indium tungsten oxide (IWO), or the like.
[0124] In some optional embodiments of the present application, the heat treatment comprises:
[0125] By annealing, the portion of the first initial electrode 33 in contact with the channel layer 20 is spontaneously oxidized to form an aluminum oxide film, the portion of the first initial electrode 33 that is not oxidized forms the first conductive layer 31, and the aluminum oxide film formed by oxidation forms the second conductive layer 32; and / or,
[0126] Through the annealing process, the portion of the second initial electrode 43 in contact with the channel layer 20 is spontaneously oxidized to form an aluminum oxide film, the portion of the second initial electrode 43 that is not oxidized forms the third conductive layer 41, and the oxidized aluminum oxide film forms the fourth conductive layer 42.
[0127] In some optional embodiments of the present application, the semiconductor structure in the manufacturing process can be heat-treated by an annealing process, so that the first initial electrode 33 made of aluminum material and the channel layer 20 made of a material including an oxide semiconductor material are spontaneously oxidized to form a very thin aluminum oxide film, and the second initial electrode 43 made of aluminum material and the channel layer 20 made of a material including an oxide semiconductor material are spontaneously oxidized to form a very thin aluminum oxide film. Studies have shown that the aluminum-aluminum oxide-oxide semiconductor material (such as IGZO) heterojunction is an ohmic contact, so that the channel layer 20 forms an ohmic contact with the first conductive layer 31 through the second conductive layer 32, and the channel layer 20 forms an ohmic contact with the third conductive layer 41 through the fourth conductive layer 42. As a result, the contact resistance between the channel layer 20 and the first electrode 30 and between the channel layer 20 and the second electrode 40 is low, which is conducive to the input and output of current, thereby achieving the purpose of increasing the on-state current of the device by at least one order of magnitude without increasing the size of the device.
[0128] In some optional embodiments of the present application, the semiconductor structure in the manufacturing process can be locally annealed by an annealing process. For example, the semiconductor structure in the manufacturing process can be locally annealed by a selective laser annealing process, and the local annealing area at least covers the portion of the first initial electrode 33 that contacts the channel layer 20, or at least covers the portion of the second initial electrode 43 that contacts the channel layer 20, and does not completely cover the entire semiconductor structure in the manufacturing process, so as to achieve local annealing of the portion of the first initial electrode 33 that contacts the channel layer 20, so that the portion of the first initial electrode 33 that contacts the channel layer 20 is oxidized, or to achieve local annealing of the portion of the second initial electrode 43 that contacts the channel layer 20, so that the portion of the second initial electrode 43 that contacts the channel layer 20 is oxidized.
[0129] In some optional embodiments of the present application, such as Fig.10 As shown, after the heat treatment, the method for preparing the semiconductor structure further includes:
[0130] A gate dielectric layer 80 is formed on a side of the channel layer 20 away from the substrate 10 , and at least a portion of the gate dielectric layer 80 is located in the first through hole 60 ;
[0131] A gate 90 is formed on a side of the gate dielectric layer 80 away from the substrate 10 , and at least a portion of the gate 90 is located in the first through hole 60 , so as to form a semiconductor structure with a vertical channel. Specifically, the gate 90 fills the first through hole 60 .
[0132] In some optional embodiments of the present application, such as Figures 11 to 13 As shown, after manufacturing the gate 90, the method for preparing the semiconductor structure further includes:
[0133] The channel layer 20, the gate dielectric layer 80 and the gate 90 located on the side of the first dielectric layer 70 away from the substrate 10 are patterned by a patterning process to remove at least a portion of the channel layer 20, the gate dielectric layer 80 and the gate 90 extending in a direction parallel to the substrate 10;
[0134] A second dielectric layer 110 is formed on a side of the first dielectric layer 70 away from the substrate 10 , and the second dielectric layer 110 covers the channel layer 20 , the gate dielectric layer 80 and the gate 90 ;
[0135] The second dielectric layer 110 is patterned to form a second through hole 111 penetrating the second dielectric layer 110 , wherein the second through hole 111 exposes the gate 90 ;
[0136] A conductive material is deposited on the side of the second dielectric layer 110 away from the substrate 10 to form a connection structure 120. The connection structure 120 fills the second through hole 111 and is electrically connected to the gate 90. The connection structure 120 is used as a connection line at each end for electrically connecting to an external structure. Optionally, the material of the connection structure 120 can be a metal material, the connection structure 120 can be a lead or a wire, and the external structure can be a component such as a capacitor. Optionally, the second through hole 111 can be formed by an etching process, or the second through hole 111 and the connection structure 120 can be formed by a Damascus process.
[0137] In the embodiments of the present application, the method for preparing a semiconductor structure belongs to the field of semiconductor device preparation, and particularly relates to a preparation process for a transistor structure.
[0138] It should be noted that the "patterning process" mentioned in the embodiments of the present application includes processes such as depositing a film layer, coating a photoresist, mask exposure, development, etching, and stripping a photoresist, which is a mature preparation process in the relevant technology. The "photolithography process" mentioned in the embodiments of the present application includes processes such as coating a film layer, mask exposure, and development, which is a mature preparation process in the relevant technology. Among them, deposition can adopt known processes such as sputtering, evaporation, and chemical vapor deposition, coating can adopt known coating processes, and etching can adopt known methods, which are not specifically limited here.
[0139] In the description of the embodiments of the present application, it should be understood that a "layer" refers to a thin film made by depositing or coating a certain material on a substrate. If the thin film does not require a composition process or a photolithography process during the entire production process, the thin film can also be called a layer. If the thin film still requires a composition process or a photolithography process during the entire production process, it can be called a thin film before the composition process and can be called a layer after the composition process. The "layer" after the composition process or the photolithography process contains at least one "pattern".
[0140] Based on the same inventive concept, an embodiment of the present application provides a memory, which includes: the semiconductor structure 100 mentioned above.
[0141] In some optional embodiments of the present application, the memory includes a plurality of semiconductor structures 100, among which a plurality of semiconductor structures 100 are arranged in an array in a direction parallel to the substrate 10, and optionally, at least two semiconductor structures 100 arranged in a first direction may share one of the bit line and the word line, and at least two semiconductor structures 100 arranged in a second direction may share the other of the bit line and the word line; and / or, among the plurality of semiconductor structures 100, a plurality of semiconductor structures 100 are stacked in sequence in a direction perpendicular to the substrate 10. By means of such a setting, an array structure and / or a 3D stacking structure can be formed, which can improve the storage capacity of the memory, reduce the storage cost, improve the integration and storage density, and help to achieve miniaturization; at the same time, the number of bit lines and word lines can be reduced, which is beneficial to layout design, and improves the structural density and practicality.
[0142] It should be noted that, since the memory of the embodiment of the present application includes the semiconductor structure of the embodiment of the present application, the memory of the embodiment of the present application also has the above-mentioned beneficial effects of the semiconductor structure of the embodiment of the present application, which will not be repeated here.
[0143] In some optional implementations of the present application, the memory may be a random access memory, specifically a static random access memory or a dynamic random access memory, and of course, may also be a flash memory.
[0144] Based on the same inventive concept, an embodiment of the present application further provides an electronic device, which includes: the above-mentioned semiconductor structure or memory.
[0145] It should be noted that since the electronic device of the embodiment of the present application includes the semiconductor structure or memory of the embodiment of the present application, the electronic device of the embodiment of the present application also has the above-mentioned beneficial effects of the semiconductor structure or memory of the embodiment of the present application, which will not be repeated here.
[0146] In some optional embodiments of the present application, the electronic device includes a storage device, a smart phone, a computer, a tablet computer, an artificial intelligence device, a wearable device or a mobile power supply, etc. Among them, the storage device may include a memory in a computer, etc., which is not limited here.
[0147] By applying the embodiments of the present application, at least the following beneficial effects can be achieved:
[0148] In the embodiment of the present application, the material of the channel layer includes an oxide semiconductor material, the material of the first conductive layer is aluminum, the material of the second conductive layer is aluminum oxide, the material of the third conductive layer is aluminum, and the material of the fourth conductive layer is aluminum oxide, so that the channel layer forms an ohmic contact with the first conductive layer through the second conductive layer, and the channel layer forms an ohmic contact with the third conductive layer through the fourth conductive layer. Based on the structure of the ring-channel semiconductor device, the technical solution of the present application can effectively reduce the contact resistance between the source and drain and the channel material without increasing the size of the device, thereby significantly improving the on-state current of the semiconductor device.
[0149] The technical solution of the present application can form a channel layer made of oxide semiconductor material, a first conductive layer made of aluminum, a second conductive layer made of aluminum oxide, a third conductive layer made of aluminum oxide, and a fourth conductive layer made of aluminum oxide without adding additional graphic processes or increasing the size of the device, so that the channel layer forms an ohmic contact with the first conductive layer through the second conductive layer, and the channel layer forms an ohmic contact with the third conductive layer through the fourth conductive layer, which can greatly reduce the contact resistance between the source and drain and the channel material, thereby significantly improving the on-state current of the semiconductor device.
[0150] Those skilled in the art will appreciate that the various operations, methods, steps, measures, and schemes in the processes discussed in this application may be alternated, altered, combined, or deleted. Further, other steps, measures, and schemes in the various operations, methods, and processes discussed in this application may also be alternated, altered, rearranged, decomposed, combined, or deleted. Further, the steps, measures, and schemes in the prior art that are similar to those disclosed in this application may also be alternated, altered, rearranged, decomposed, combined, or deleted.
[0151] In the description of the present application, the directions or positional relationships indicated by words such as "center", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside" and "outside" are based on the exemplary directions or positional relationships shown in the accompanying drawings. They are for the convenience of describing or simplifying the description of the embodiments of the present application, and do not indicate or imply that the referred device or component must have a specific orientation, be constructed and operated in a specific orientation. Therefore, they should not be understood as limitations on the present application.
[0152] The terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of this application, unless otherwise specified, "plurality" means two or more.
[0153] In the description of this application, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a direct connection, or an indirect connection through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.
[0154] In the description of this specification, specific features, structures, materials or characteristics may be combined in an appropriate manner in any one or more embodiments or examples.
[0155] It should be understood that, although the various steps in the flowchart of the accompanying drawings are displayed in sequence according to the indication of the arrows, the order of implementation of these steps is not limited to the order indicated by the arrows. Unless there is a clear description herein, in some implementation scenarios of the embodiments of the present application, the steps in each process can be performed in other orders according to demand. Moreover, some or all of the steps in each flow chart may include multiple sub-steps or multiple stages based on actual implementation scenarios. Some or all of these sub-steps or stages may be executed at the same time, or may be executed at different times in different scenarios at the execution time, and the execution order of these sub-steps or stages may be flexibly configured according to demand, and the embodiments of the present application do not limit this.
[0156] The above is only a partial implementation method of the present application. It should be pointed out that for ordinary technicians in this technical field, without departing from the technical concept of the scheme of the present application, other similar implementation methods based on the technical ideas of the present application are also within the protection scope of the embodiments of the present application.
Claims
1. A semiconductor structure, characterized in that: include: substrate; A channel layer is disposed on one side of the substrate, and at least a portion of the channel layer extends in a direction perpendicular to the substrate; A first electrode is located on a side of the channel layer facing the substrate, and the channel layer is in contact with the first electrode; a second electrode, arranged on one side of the substrate and surrounding the outer periphery of the channel layer, the channel layer is in contact with the second electrode, an extension direction of the second electrode is arranged at an angle to an extension direction of the first electrode, and the second electrode is insulated from the first electrode; in: The first electrode comprises a first conductive layer and a second conductive layer, and the first conductive layer and the second conductive layer are arranged in sequence along a direction from the substrate to the channel layer, and the channel layer forms an ohmic contact with the first conductive layer through the second conductive layer; and / or, The second electrode includes a third conductive layer and a fourth conductive layer. The third conductive layer is located on a side of the fourth conductive layer away from the channel layer. The channel layer forms an ohmic contact with the third conductive layer through the fourth conductive layer.
2. The semiconductor structure according to claim 1, characterized in that: The material of the channel layer includes an oxide semiconductor material; The material of the first conductive layer is aluminum, and the material of the second conductive layer is aluminum oxide; and / or, The material of the third conductive layer is aluminum, and the material of the fourth conductive layer is aluminum oxide.
3. The semiconductor structure according to claim 1 or 2, characterized in that: The substrate has a first groove, the opening of the first groove faces the side where the channel layer is located, and the first groove extends along a first direction parallel to the substrate; The first conductive layer and the second conductive layer are both disposed in the first groove, and the second conductive layer is located on a side of the first conductive layer facing an opening of the first groove.
4. The semiconductor structure according to claim 1 or 2, characterized in that: It also includes an insulating layer, which is arranged on one side of the substrate and covers a portion of the first conductive layer, and the second electrode is located on a side of the insulating layer away from the substrate; The semiconductor structure has a first through hole penetrating the second electrode and the insulating layer, the first through hole exposes the second conductive layer, and the channel layer at least covers the inner wall of the first through hole, so that the channel layer contacts the second electrode and the second conductive layer respectively.
5. The semiconductor structure according to claim 4, characterized in that: The insulating layer has a second groove, the opening of the second groove faces the side of the insulating layer away from the substrate, the second groove extends along a second direction parallel to the substrate, the second electrode is arranged in the second groove, and the orthographic projection of the first through hole on the substrate overlaps with the orthographic projection of the second groove on the substrate; and / or, The fourth conductive layer of the second electrode is disposed around the outer periphery of the first through hole, and the third conductive layer of the second electrode is located on a side of the fourth conductive layer away from the first through hole.
6. The semiconductor structure according to claim 1 or 2, characterized in that: It also includes an insulating layer, which is disposed on one side of the substrate and covers a portion of the first electrode, and the second electrode is located on a side of the insulating layer away from the substrate; The semiconductor structure has a first through hole, and the fourth conductive layer is arranged around the outer periphery of the first through hole. The first through hole penetrates the insulating layer and exposes the first electrode. The channel layer at least covers the inner wall of the first through hole, so that the channel layer contacts the fourth conductive layer and the first electrode respectively, and the third conductive layer is located on the side of the fourth conductive layer away from the first through hole.
7. The semiconductor structure according to claim 4, characterized in that: Also includes: a first dielectric layer, disposed on a side of the second electrode away from the substrate and covering the second electrode and the insulating layer, wherein the first through hole penetrates the first dielectric layer and extends in a direction perpendicular to the substrate; A gate dielectric layer is disposed on a side of the channel layer away from the substrate, and at least a portion of the gate dielectric layer is located in the first through hole; A gate is disposed on a side of the gate dielectric layer away from the substrate and fills the first through hole.
8. A memory, characterized in that: include: The semiconductor structure according to any one of claims 1 to 7.
9. A method for preparing a semiconductor structure, characterized in that: include: Providing a substrate and manufacturing a first initial electrode, wherein the first initial electrode is located on one side of the substrate; A second initial electrode is fabricated on one side of the substrate, wherein an extension direction of the second initial electrode is arranged at an angle with an extension direction of the first initial electrode, and the second initial electrode is insulated from the first initial electrode; Making a first through hole penetrating the second initial electrode, wherein the first through hole extends in a direction perpendicular to the substrate, and the first through hole exposes the first initial electrode; Manufacturing a channel layer, wherein the channel layer at least covers the inner wall of the first through hole, so that the first initial electrode is located on a side of the channel layer facing the substrate, and the second initial electrode is arranged around the periphery of the channel layer, and the channel layer is in contact with the first initial electrode and the second initial electrode respectively; as well as Performing heat treatment so that a portion of the first initial electrode in contact with the channel layer is oxidized, a portion of the first initial electrode that is not oxidized forms a first conductive layer, an oxidized portion forms a second conductive layer, the first conductive layer and the second conductive layer form a first electrode, and the channel layer forms an ohmic contact with the first conductive layer through the second conductive layer; and / or, a portion of the second initial electrode in contact with the channel layer is oxidized, a portion of the second initial electrode that is not oxidized forms a third conductive layer, an oxidized portion forms a fourth conductive layer, the third conductive layer and the fourth conductive layer form a second electrode, and the channel layer forms an ohmic contact with the third conductive layer through the fourth conductive layer.
10. The method for preparing a semiconductor structure according to claim 9, characterized in that: Providing a substrate and manufacturing a first initial electrode, including: providing an initial substrate; A first groove is formed on the initial substrate, wherein the first groove extends along a first direction, and the initial substrate having the first groove formed thereon forms a substrate; Depositing aluminum material in the first groove to form a first initial electrode layer, wherein the first initial electrode layer fills the first groove; The first initial electrode layer is planarized, and the planarized first initial electrode layer forms a first initial electrode.
11. The method for preparing a semiconductor structure according to claim 10, characterized in that: Producing a second initial electrode, comprising: Forming an initial insulating layer on one side of the substrate, wherein the initial insulating layer covers the first initial electrode; A second groove is formed on the initial insulating layer, wherein the second groove extends along a second direction, and the initial insulating layer having the second groove is formed into an insulating layer; Depositing aluminum material in the second groove to form a second initial electrode layer, wherein the second initial electrode layer fills the second groove, and an orthographic projection of the second initial electrode layer on the substrate has an overlapping area with an orthographic projection of the first initial electrode layer on the substrate; The second initial electrode layer is planarized, and the planarized second initial electrode layer forms a second initial electrode.
12. The method for preparing a semiconductor structure according to claim 11, characterized in that: Before making the first through hole, it also includes: Forming a first dielectric layer on a side of the insulating layer away from the substrate, wherein the first dielectric layer covers at least a portion of the second initial electrode; Making a first through hole, comprising: Graphic processing is performed to form a first through hole that sequentially penetrates the first dielectric layer, the second initial electrode and the insulating layer, wherein the orthographic projection of the first through hole on the substrate is located in the overlapping area, and the first through hole exposes the first initial electrode.
13. The method for preparing a semiconductor structure according to claim 12, characterized in that: Fabricating a channel layer, including: depositing an oxide semiconductor material in the first through hole to form a channel layer; Heat treatment is performed, including: By annealing, the portion of the first initial electrode in contact with the channel layer is spontaneously oxidized to form an aluminum oxide film, the portion of the first initial electrode that is not oxidized forms a first conductive layer, and the aluminum oxide film formed by oxidation forms a second conductive layer; and / or, The portion of the second initial electrode in contact with the channel layer is spontaneously oxidized to form an aluminum oxide film, the portion of the second initial electrode that is not oxidized forms a third conductive layer, and the aluminum oxide film formed by oxidation forms a fourth conductive layer.
14. The method for preparing a semiconductor structure according to any one of claims 9 to 13, characterized in that: After heat treatment, it also includes: A gate dielectric layer is formed on a side of the channel layer away from the substrate, wherein at least a portion of the gate dielectric layer is located in the first through hole; A gate is manufactured on a side of the gate dielectric layer away from the substrate, and at least a portion of the gate is located in the first through hole.