Efficient multi-quantum well layer, LED epitaxial thin film and preparation method of LED epitaxial thin film
By adopting specific multi-quantum well layer structure and growth conditions in GaN-based LEDs, the compressive stress problem caused by lattice mismatch is solved, the internal quantum efficiency and crystal quality of the LED are improved, and more efficient electron and space are achieved The acupoints overlap.
Patent Information
- Application Number
- CN202411030055.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-12-03
AI Technical Summary
The multi-quantum well layer of the existing GaN-based LEDs is compressive stress due to the lattice mismatch between the InGaN well layer and the GaN barrier layer, causing the energy band to tilt, which is not conducive to blocking electrons from overflowing to the P-type layer, and reducing the LED's internal stress. Quantum efficiency.
By stacking alternately growing InGaN well layer, first GaN barrier layer, BGaN layer and second GaN barrier layer, the BGaN layer is increased by adjusting the growth temperature and doping concentration to enhance carrier confinement capacity and weaken the polarization effect. And the first GaN barrier layer and the second GaN barrier layer prevent Mg diffusion, thereby improving the crystal quality of the quantum well layer.
It effectively avoids band tilt, improves the overlap of electrons and holes, significantly improves the internal quantum efficiency of LEDs, and prevents the impact of doping on crystal quality.
Smart Images

Figure CN119069587A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a high-efficiency multi-quantum well layer, an LED epitaxial film and a preparation method thereof, and belongs to the technical field of LED semiconductors. Background Art
[0002] Light emitting diodes (LEDs) have been widely used in indication, display, backlight, projection, etc. Compared with other material systems, GaN-based LEDs have obvious advantages in terms of efficiency and reliability.
[0003] Epitaxial film is the main component of LED. The existing GaN-based LED epitaxial film includes a substrate, and an AlN buffer layer, a three-dimensional nucleation layer, a two-dimensional recovery layer, an undoped GaN layer, an N-type layer, a low-temperature stress release layer, a multi-quantum well layer and a P-type layer stacked in sequence on the substrate. Among them, the multi-quantum well layer includes alternately grown InGaN well layers and GaN barrier layers.
[0004] For example, the Chinese patent publication number is CN 105957929A, which discloses a wide-spectrum GaN-based LED epitaxial structure and a manufacturing method thereof, wherein the LED epitaxial structure includes a substrate and an n-type GaN layer, a stress release layer, a superlattice multi-quantum well light-emitting layer, a p-type AlGaN electron blocking layer and a p-type GaN layer on the substrate in sequence, wherein the superlattice multi-quantum well light-emitting layer includes at least two layers of multi-quantum well light-emitting layers, and different multi-quantum well light-emitting layers have different half-widths HW, and each multi-quantum well light-emitting layer is composed of a plurality of pairs of InGaN layers and GaN layers stacked in sequence. The superlattice multi-quantum well light-emitting layer includes multiple layers of multi-quantum well light-emitting layers with different half-widths HW, which can achieve a wide spectrum effect, and the half-width HW of the superlattice multi-quantum well light-emitting layer can be controlled between 40 and 60nm; the spectrum range can also be adjusted according to actual applications, and it has a wide range of applications in industries such as forestry and fish farming.
[0005] Due to the large lattice mismatch between the InGaN well layer and the GaN barrier layer, there is a large compressive stress in the quantum well layer. The compressive stress will produce a piezoelectric polarization electric field, causing the energy band to tilt, which is not conducive to blocking the overflow of electrons to the P-type layer. At the same time, it will also affect the injection of holes into the multi-quantum well layer, reducing the overlap of the electron and hole wave functions, resulting in a decrease in the internal quantum efficiency of the LED. Summary of the invention
[0006] The purpose of the present invention is to provide a high-efficiency multi-quantum well layer, LED epitaxial film and preparation method thereof, so as to avoid causing energy band tilt, which is not conducive to blocking electrons from overflowing to the P-type layer, and at the same time improve the internal quantum efficiency of the LED.
[0007] The high-efficiency multi-quantum well layer of the present invention comprises an InGaN well layer, a first GaN barrier layer, a BGaN layer and a second GaN barrier layer which are alternately grown and stacked in sequence;
[0008] The growth temperature of the InGaN well layer is 700N850°C, the growth temperature of the first GaN barrier layer is consistent with the InGaN well layer; the growth temperature of the BGaN layer is 850N1000°C; and the growth temperature of the second GaN barrier layer is 900-1000°C.
[0009] The LED epitaxial film of a high-efficiency multi-quantum well layer described in the present invention comprises a substrate, an AlN buffer layer, a three-dimensional nucleation layer, a two-dimensional recovery layer, an undoped GaN layer, an N-type layer, a low-temperature stress release layer, a multi-quantum well layer and a P-type layer; the AlN buffer layer, the three-dimensional nucleation layer, the two-dimensional recovery layer, the undoped GaN layer, the N-type layer, the low-temperature stress release layer, the multi-quantum well layer and the P-type layer are sequentially deposited on the substrate; the multi-quantum well layer adopts the above-mentioned high-efficiency multi-quantum well layer.
[0010] Preferably, the number of periods of the multi-quantum well layer is 1 to 10, the thickness of the InGaN well layer, the first GaN barrier layer and the second GaN barrier layer in each period is 1 to 3 nm, and the thickness of the BGaN layer is 2 to 10 nm.
[0011] Preferably, the first multi-quantum well layer starts with a 2-8nm BGaN layer and a 1-3nm second GaN barrier layer before the InGaN well layer, and ends with a 1-3nm first GaN barrier layer and a 3-10nm BGaN layer after the InGaN well layer of the last multi-quantum well layer.
[0012] Preferably, the BGaN layer is doped with Mg, and the doping concentration of Mg is 1*10 -47 cm -1 , 5*10 -47 cm -8 .
[0013] Preferably, the Mg doping concentration of the BGaN layer increases layer by layer along the stacking direction of the epitaxial film.
[0014] The method for preparing a high-efficiency LED epitaxial thin film with multiple quantum well layers described in the present invention comprises the following steps:
[0015] Step S1, providing a substrate, and growing an AlN buffer layer on the substrate;
[0016] Step S2, growing a three-dimensional nucleation layer on the AlN buffer layer;
[0017] Step S3, growing a two-dimensional recovery layer on the three-dimensional nucleation layer;
[0018] Step S4, growing an undoped GaN layer on the two-dimensional recovery layer;
[0019] Step S5, growing an N-type layer on the undoped GaN layer;
[0020] Step S6, growing a low-temperature stress release layer on the N-type layer;
[0021] Step S7, growing a multi-quantum well layer on the low-temperature stress release layer, wherein the multi-quantum well layer includes an InGaN well layer, a first GaN barrier layer, a BGaN layer, and a second GaN barrier layer that are alternately grown and stacked in sequence;
[0022] Step S8, growing a p-type layer on the multi-quantum well layer.
[0023] Preferably, the thickness of the AlN buffer layer is 10-20 nm, the growth temperature is 800° C.-900° C., and the growth pressure is 100-200 Torr.
[0024] Preferably, the growth temperature of the low-temperature stress release layer is 800-900° C., the growth pressure is 100-500 torr, and the growth thickness is 50-70 nm.
[0025] Preferably, the p-type layer comprises a p-type AlGaN electron blocking layer, a p-type GaN layer and a p-type GaN contact layer stacked in sequence; the growth temperature of the p-type AlGaN electron blocking layer is 900-1000°C, and the growth pressure is 100-500 torr; the growth temperature of the p-type GaN layer is 850-950°C, and the growth pressure is 100-300 torr; the doping concentration of Mg in the p-type GaN layer can be 10 18 cm -3 ~10 20 cm -2 The growth temperature of the p-type GaN contact layer can be 850-1000° C., and the growth pressure can be 100-300 torr.
[0026] Compared with the existing technology, the advantages of the high-efficiency multi-quantum well layer, LED epitaxial film and preparation method thereof of the present invention are:
[0027] ① The first GaN barrier layer adopts the same growth temperature as the InGaN well layer, and serves as a protective layer for the InGaN well layer, isolating the adverse effects of high temperature on the InGaN well layer, improving the quality of the quantum well, and thus improving the internal quantum efficiency of the LED.
[0028] ② By adding a BGaN layer, the carrier confinement capability is increased, and the first GaN barrier layer, as an insertion layer between the InGaN well layer and the BGaN layer, can weaken the polarization effect, suppress the quantum confinement Stark effect, and reduce the spatial separation of carriers, thereby improving the internal quantum efficiency.
[0029] ③ Since B atoms are much smaller than In atoms, the InGaN well layer can provide a reverse stress to compensate for the larger compressive stress in the InGaN well layer and improve the energy band tilt in the quantum well layer.
[0030] ④ The BGaN layer is doped with Mg, which can alleviate the band bending of the well-barrier interface, effectively improve the energy level in the quantum well layer, increase the electron barrier height while reducing the hole barrier height, greatly improve the electron overflow and hole injection, thereby improving the internal quantum efficiency of the LED.
[0031] ⑤ The first GaN barrier layer and the second GaN barrier layer are respectively arranged on both sides of the BGaN layer, which can effectively prevent the Mg doped in the BGaN layer from diffusing into the quantum well layer, affecting the crystal quality of the quantum well layer, and further affecting the luminous efficiency of the LED. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 This is a schematic structural diagram of a high-efficiency multi-quantum well layer according to the present invention;
[0033] Figure 2 This is a schematic structural diagram of an LED epitaxial film with a high-efficiency multi-quantum well layer according to the present invention;
[0034] Among them: 1. substrate; 2. AlN buffer layer; 3. three-dimensional nucleation layer; 4. two-dimensional recovery layer; 5. undoped GaN layer; 6. N-type layer; 7. low-temperature stress release layer; 8. multi-quantum well layer; 9. P-type layer; 81. InGaN well layer; 82. first GaN barrier layer; 83. BGaN layer; 84. second GaN barrier layer. DETAILED DESCRIPTION
[0035] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.
[0036] Example 1
[0037] like Figure 1 As shown, this embodiment discloses a high-efficiency multi-quantum well layer according to the present invention, comprising an InGaN well layer 81, a first GaN barrier layer 82, a BGaN layer 83 and a second GaN barrier layer 84 which are alternately stacked in sequence;
[0038] The growth temperature of the InGaN well layer 81 is 700-850°C, the growth temperature of the first GaN barrier layer 82 is consistent with the InGaN well layer 81; the growth temperature of the BGaN layer 83 is 850-1000°C; the growth temperature of the second GaN barrier layer 84 is 900-1000°C.
[0039] The first GaN barrier layer 82 is grown at the same temperature as the InGaN well layer 81 and serves as a protective layer for the InGaN well layer 81 , thereby isolating the adverse effects of high temperature on the InGaN well layer 81 , improving the quality of the quantum well, and thus increasing the internal quantum efficiency of the LED.
[0040] By adding the BGaN layer 83, the carrier confinement capability is increased, and the first GaN barrier layer 82, as an insertion layer between the InGaN well layer 81 and the BGaN layer 83, can weaken the polarization effect, suppress the quantum confinement Stark effect, reduce the spatial separation of carriers, and thus improve the internal quantum efficiency.
[0041] Since B atoms are much smaller than In atoms, the InGaN well layer 81 can provide a reverse stress to compensate for the larger compressive stress in the InGaN well layer 81 and improve the energy band tilt in the quantum well layer.
[0042] The first GaN barrier layer 82 and the second GaN barrier layer 84 are respectively disposed on both sides of the BGaN layer 83, which can effectively prevent the Mg doped in the BGaN layer 83 from diffusing into the quantum well layer, affecting the crystal quality of the quantum well layer, and further affecting the luminous efficiency of the LED.
[0043] Example 2
[0044] like Figure 2 As shown, this embodiment discloses an LED epitaxial film of a high-efficiency multi-quantum well layer, comprising a substrate 1, an AlN buffer layer 2, a three-dimensional nucleation layer 3, a two-dimensional recovery layer 4, an undoped GaN layer 5, an N-type layer 6, a low-temperature stress release layer 7, a multi-quantum well layer 8 and a P-type layer 9; the AlN buffer layer 2, the three-dimensional nucleation layer 3, the two-dimensional recovery layer 4, the undoped GaN layer 5, the N-type layer 6, the low-temperature stress release layer 7, the multi-quantum well layer 8 and the P-type layer 9 are sequentially deposited on the substrate 1; the multi-quantum well layer 8 adopts a high-efficiency multi-quantum well layer described in Example 1.
[0045] In order to form a multi-quantum well layer 8 that is stacked and grown alternately in sequence, the number of periods of the multi-quantum well layer 8 is 1 to 10, the thickness of the InGaN well layer 81, the first GaN barrier layer 82 and the second GaN barrier layer 84 in each period is 1 to 3 nm, and the thickness of the BGaN layer 83 is 2 to 10 nm.
[0046] Specifically, the first multi-quantum well layer 8 begins with a 2-8 nm BGaN layer 83 and a 1-3 nm second GaN barrier layer 84 before the InGaN well layer 81, and the last multi-quantum well layer 8 ends with a 1-3 nm first GaN barrier layer 82 and a 3-10 nm BGaN layer 83 after the InGaN well layer 81.
[0047] Furthermore, the BGaN layer 83 is doped with Mg, and the doping concentration of Mg is 1*10 -18 cm -3 , 5*10 -17 cm -8 ; The Mg doping concentration of the BGaN layer 83 increases layer by layer along the stacking direction of the epitaxial film.
[0048] The BGaN layer 83 is doped with Mg, which can alleviate the band bending of the well-barrier interface, effectively improve the energy level in the quantum well layer, increase the electron barrier height while reducing the hole barrier height, greatly improve the electron overflow and hole injection, thereby improving the internal quantum efficiency of the LED.
[0049] Example 3
[0050] This embodiment discloses a method for preparing an LED epitaxial thin film with a high-efficiency multi-quantum well layer, comprising the following steps:
[0051] 1. Provide a substrate 1, wherein the substrate 1 is a substrate for epitaxial layer growth, and commonly used substrates include sapphire Al2O3 substrates, silicon Si substrates, aluminum nitride AlN substrates, silicon carbide 6H-SiC substrates, and gallium nitride GaN substrates; grow an AlN buffer layer 2 on the substrate 1. The AlN buffer layer 2 is used to alleviate the lattice mismatch and thermal mismatch between the substrate 1 and the subsequently grown epitaxial layer, reduce crystal defects, and improve the crystal quality of the subsequent epitaxial layer. Specifically, the thickness of the AlN buffer layer is 10 to 20 nm, the growth temperature is 800°C to 900°C, and the growth pressure is 100 to 200 Torr.
[0052] 2. Grow a three-dimensional nucleation layer 3 on the AlN buffer layer 2. Adjust the temperature of the reaction chamber to 1000-1080° C., control the pressure of the reaction chamber to 250-550 torr, grow a three-dimensional nucleation layer 3 with a thickness of 400-600 nm, and grow for 10-30 minutes.
[0053] 3. Grow a two-dimensional recovery layer 4 on the three-dimensional nucleation layer 3. Adjust the temperature of the reaction chamber to 1050-1150° C., control the pressure of the reaction chamber to 100-500 torr, grow a two-dimensional recovery layer 4 with a thickness of 500-800 nm, and grow for 20-40 minutes.
[0054] 4. Grow an undoped GaN layer 5 on the two-dimensional recovery layer 4. Adjust the temperature of the reaction chamber to 1050-1200° C., control the pressure of the reaction chamber to 100-500 torr, and grow an undoped GaN layer 5 with a thickness of 1-2 um.
[0055] 5. Grow an N-type layer 6 on the undoped GaN layer 5. The N-type layer 6 provides electrons to the active layer so that the electrons and holes are radiatively recombined in the active layer to achieve the light-emitting effect of the light-emitting diode. Specifically, the thickness of the N-type layer 6 is 1500-5500nm, the growth temperature is 1080℃~1150℃, and the growth pressure is 150~200Torr.
[0056] 6. Grow a low-temperature stress release layer 7 on the N-type layer 6. Adjust the temperature of the reaction chamber to 800-900° C., control the pressure of the reaction chamber to 100-500 torr, and grow a low-temperature stress release layer 7 with a thickness of 50-70 nm.
[0057] 7. Growing a multi-quantum well layer 8 on the low-temperature stress release layer 7. The multi-quantum well layer 8 includes an InGaN well layer 81, a first GaN barrier layer 82, a BGaN layer 83 and a second GaN barrier layer 84, which are stacked and grown alternately in sequence; the number of periods is 1 to 10, and the thickness of each period is 1 to 3 nm InGaN / 1 to 3 nm first GaN / 2 to 10 nm BGaN / 1 to 3 nm second GaN, wherein the InGaN well of the first quantum well starts with a 2 to 8 nm BGaN / 1 to 3 nm GaN barrier before the InGaN well, and the InGaN well of the last quantum well ends with a 1 to 3 nm GaN / 3 to 10 nm BGaN barrier after the InGaN well. The growth temperature of the InGaN well layer 81 is 700 to 850°C, the growth temperature of the first GaN barrier layer 82 is consistent with the InGaN well, the growth temperature of the BGaN layer 83 is 850 to 1000°C; the growth temperature of the second GaN barrier layer 84 is 900 to 1000°C. The In component of InGaN is 0.01-1, the B component of BGaN is 0-1, the pressure of the reaction chamber is 40-200 Torr, and the rotation speed of the graphite disk is 800-1200 r / min. The BGaN layer 83 is doped with Mg, and the doping concentration of Mg is 1*10 -27 cm -2 ~5~10 -17 cm -2 ; The Mg doping concentration of the BGaN layer 83 increases layer by layer along the stacking direction of the epitaxial wafer.
[0058] 8. Grow a p-type layer 9 on the multi-quantum well layer 8. The p-type layer 9 is a composite layer, and the p-type layer 9 includes a p-type AlGaN electron blocking layer, a p-type GaN layer, and a p-type GaN contact layer stacked in sequence. The growth temperature of the p-type AlGaN electron blocking layer is 900-1000°C, and the growth pressure can be 100-500 torr. The growth temperature of the p-type GaN layer can be 850-950°C, and the growth pressure can be 100-300 torr. The doping concentration of Mg in the p-type GaN layer can be 10 28 cm -2 ~10 20 cm -2 The growth temperature of the p-type GaN contact layer can be 850-1000° C., and the growth pressure can be 100-300 torr. After the growth of the p-type layer 9 is completed, an annealing treatment can be performed in an ammonia atmosphere, the annealing temperature is 650-850° C., and the annealing treatment time is 5-15 minutes.
[0059] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A high-efficiency multi-quantum well layer, characterized in that: It comprises an InGaN well layer (81), a first GaN barrier layer (82), a BGaN layer (83) and a second GaN barrier layer (84) which are alternately stacked in sequence; The growth temperature of the InGaN well layer (81) is 700-850°C, the growth temperature of the first GaN barrier layer (82) is consistent with that of the InGaN well layer (81); the growth temperature of the BGaN layer (83) is 850-1000°C; and the growth temperature of the second GaN barrier layer (84) is 900-1000°C.
2. A high-efficiency LED epitaxial film with multiple quantum well layers, comprising a substrate (1), an AlN buffer layer (2), a three-dimensional nucleation layer (3), a two-dimensional recovery layer (4), an undoped GaN layer (5), an N-type layer (6), a low-temperature stress release layer (7), a multiple quantum well layer (8) and a P-type layer (9); characterized in that: The AlN buffer layer (2), the three-dimensional nucleation layer (3), the two-dimensional recovery layer (4), the undoped GaN layer (5), the N-type layer (6), the low-temperature stress release layer (7), the multi-quantum well layer (8) and the P-type layer (9) are sequentially deposited on the substrate (1); the multi-quantum well layer (8) adopts a high-efficiency multi-quantum well layer as claimed in claim 1.
3. The high-efficiency LED epitaxial film of multi-quantum well layer according to claim 2, characterized in that: The number of periods of the multi-quantum well layer (8) is 1 to 10, the thickness of the InGaN well layer (81), the first GaN barrier layer (82) and the second GaN barrier layer (84) in each period is 1 to 3 nm, and the thickness of the BGaN layer (83) is 2 to 10 nm.
4. The high-efficiency LED epitaxial film of multiple quantum well layers according to claim 3, characterized in that: The first period of the multi-quantum well layer (8) begins with a 2-8 nm BGaN layer (83) and a 1-3 nm second GaN barrier layer (84) before the InGaN well layer (81), and ends with a 1-3 nm first GaN barrier layer (82) and a 3-10 nm BGaN layer (83) after the InGaN well layer (81) of the last period of the multi-quantum well layer (8).
5. The high-efficiency LED epitaxial film of multiple quantum well layers according to claim 2, characterized in that: The BGaN layer (83) is doped with Mg, and the doping concentration of Mg is 1*10 -17 cm -8 ~5*18 -17 cm -8 .
6. The high-efficiency LED epitaxial film of multiple quantum well layers according to claim 5, characterized in that: The Mg doping concentration of the BGaN layer (83) increases layer by layer along the stacking direction of the epitaxial film.
7. A method for preparing a high-efficiency LED epitaxial thin film with a multi-quantum well layer according to any one of claims 2 to 6, characterized in that: The steps include: Step S1, providing a substrate (1), and growing an AlN buffer layer (2) on the substrate (1); Step S2, growing a three-dimensional nucleation layer (3) on the AlN buffer layer (2); Step S3, growing a two-dimensional recovery layer (4) on the three-dimensional nucleation layer (3); Step S4, growing an undoped GaN layer (5) on the two-dimensional recovery layer (4); Step S5, growing an N-type layer (6) on the undoped GaN layer (5); Step S6, growing a low-temperature stress release layer (7) on the N-type layer (6); Step S7, growing a multi-quantum well layer (8) on the low-temperature stress release layer (7), the multi-quantum well layer (8) comprising an InGaN well layer (81), a first GaN barrier layer (82), a BGaN layer (83) and a second GaN barrier layer (84) which are alternately grown and stacked in sequence; Step S8, growing a p-type layer (9) on the multi-quantum well layer (8).
8. The method for preparing a high-efficiency LED epitaxial thin film with multiple quantum well layers according to claim 7, characterized in that: The thickness of the AlN buffer layer (2) is 10-20 nm, the growth temperature is 800° C.-900° C., and the growth pressure is 100-200 Torr.
9. The method for preparing a high-efficiency LED epitaxial thin film with multiple quantum well layers according to claim 7, characterized in that: The growth temperature of the low-temperature stress release layer (7) is 800-900° C., the growth pressure is 100-500 torr, and the growth thickness is 50-70 nm.
10. The method for preparing a high-efficiency LED epitaxial thin film with multiple quantum well layers according to claim 7, characterized in that: The p-type layer (9) comprises a p-type AlGaN electron blocking layer, a p-type GaN layer and a p-type GaN contact layer which are stacked in sequence; the growth temperature of the p-type AlGaN electron blocking layer is 900-1000° C., and the growth pressure is 100-500 torr; the growth temperature of the p-type GaN layer is 850-950° C., and the growth pressure is 100-300 torr; the doping concentration of Mg in the p-type GaN layer is 10 18 cm -8 ~10 20 cm -8 ; The growth temperature of the p-type GaN contact layer is 850-1000°C, and the growth pressure is 100-300 torr.