Light emitting diode and preparation method thereof

By introducing an insertion layer between the first semiconductor layer and the light emitting layer of the LED, including a raised and a fill layer, and forming a stress control layer by using an annealing process, the problem of low luminescence efficiency caused by lattice mismatch stress is solved, and the problem of low luminescence efficiency caused by lattice mismatch stress is improved The luminous efficiency and quality of LEDs.

CN119069593AActive Publication Date: 2024-12-03HC SEMITEK (SUZHOU) CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410956395.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-12-03
Estimated Expiration
2044-07-17

AI Technical Summary

Technical Problem

The luminous efficiency of LEDs is lower than expected, mainly due to the accumulation of stress caused by the lattice mismatch between the substrate and the semiconductor material, which affects the quality of the luminous layer and the radiation recombination efficiency.

Method used

An insertion layer is introduced between the first semiconductor layer and the light emitting layer. The insertion layer includes a plurality of protrusions and fill layers. A stress control layer is provided in the protrusion. The stress control layer is decomposed by annealing process, and the fill layer is filled with the protrusion. In between, the extension of dislocation to the light emitting layer is reduced, and the quality of the light emitting layer is improved.

Benefits of technology

By releasing lattice mismatch stress, reducing polarization effect, improving the radiation recombination efficiency of electrons and holes, improving the luminous efficiency and overall quality of LEDs, simplifying process steps and reducing the impact of etching damage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069593A_ABST
    Figure CN119069593A_ABST
Patent Text Reader

Abstract

The embodiment of the invention provides a light emitting diode and a preparation method thereof, and belongs to the technical field of semiconductors. The light-emitting diode comprises a first semiconductor layer, an insertion layer, a light-emitting layer and a second semiconductor layer which are stacked in sequence, the insertion layer comprises a plurality of protrusions and a filling and leveling layer, the protrusions are located between the first semiconductor layer and the light-emitting layer, each protrusion comprises a stress regulation and control layer, and the stress regulation and control layer is formed through decomposition of an annealing process; and the filling and leveling layer is filled among the plurality of bulges. According to the embodiment of the invention, the luminous efficiency and quality of the LED can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to the field of semiconductor technology, and in particular to a light emitting diode and a method for preparing the same. Background Art

[0002] Light Emitting Diode (LED) has been widely used in various light source fields such as backlight, lighting, and landscaping due to its small size, long service life, rich colors, and low energy consumption.

[0003] In the related art, an LED includes a substrate and a first semiconductor layer, a light emitting layer, and a second semiconductor layer sequentially stacked on the substrate.

[0004] However, there is a large lattice mismatch between the substrate and the semiconductor material. The stress generated by the lattice mismatch will accumulate in the first semiconductor layer and then accumulate upward to the light-emitting layer. The lattice mismatch stress accumulated in the light-emitting layer will produce a higher dislocation density in the light-emitting layer, affecting the quality of the light-emitting layer and producing a polarization effect in the light-emitting layer, thereby reducing the radiation recombination efficiency of electrons and holes in the light-emitting layer and affecting the luminous efficiency of the LED. Summary of the invention

[0005] The embodiment of the present disclosure provides a light emitting diode and a method for manufacturing the same, which can improve the light emitting efficiency and quality of the LED. The technical solution is as follows:

[0006] On the one hand, a light-emitting diode is provided, comprising a first semiconductor layer, an insertion layer, a light-emitting layer and a second semiconductor layer stacked in sequence, the insertion layer comprising a plurality of protrusions and a filling layer, the plurality of protrusions being located between the first semiconductor layer and the light-emitting layer, the protrusions comprising a stress regulation layer, the stress regulation layer being formed by decomposition through an annealing process; the filling layer being filled between the plurality of protrusions.

[0007] Optionally, the stress regulating layer is an InN layer or an InSb layer.

[0008] Optionally, the stress regulation layer has a thickness of 50 nm to 100 nm.

[0009] Optionally, the protrusion further includes a metal mask layer, the stress regulation layer and the metal mask layer are stacked in sequence in a direction away from the first semiconductor layer, and the metal mask layer is formed by shrinking through an annealing process.

[0010] Optionally, the metal mask layer is an Al layer, an Ag layer, a Sn layer or a Zn layer.

[0011] Optionally, the thickness of the metal mask layer is 1 nm to 5 nm.

[0012] Optionally, the insertion layer further includes an isolation layer, and the isolation layer is located between the first semiconductor layer and the plurality of protrusions.

[0013] Optionally, the isolation layer is an AlN layer or an AlGaN layer.

[0014] Optionally, the filling layer is an InGaN layer.

[0015] On the other hand, a method for preparing a light-emitting diode is provided, comprising: forming an insertion layer on a first semiconductor layer, the insertion layer comprising a plurality of protrusions and a filling layer, the plurality of protrusions being located between the first semiconductor layer and the light-emitting layer, the protrusions comprising a stress regulation layer, the stress regulation layer being formed by decomposing through an annealing process, and the filling layer being filled between the plurality of protrusions; forming a light-emitting layer on the insertion layer; and forming a second semiconductor layer on the light-emitting layer.

[0016] The technical solution provided by the embodiments of the present disclosure has the following beneficial effects:

[0017] In the disclosed embodiment, an insertion layer is provided between the first semiconductor layer and the light-emitting layer, the insertion layer includes a plurality of protrusions and a filling layer, the plurality of protrusions are located between the first semiconductor layer and the light-emitting layer, the protrusions include a stress regulating layer, the stress regulating layer can release the stress accumulated in the first semiconductor layer due to the lattice mismatch between the substrate and the semiconductor material, guide the dislocations generated by the lattice mismatch stress to be transferred to the side walls of the plurality of protrusions, so as to reduce the probability of the dislocations extending upward to the light-emitting layer, improve the quality of the light-emitting layer, reduce the polarization effect of the light-emitting layer, thereby improving the radiation recombination efficiency of electrons and holes in the light-emitting layer, and improving the luminous efficiency of the LED. The filling layer is filled between the plurality of protrusions, and the filling layer can fill the gaps between the plurality of protrusions, so as to ensure that the growth quality of the insertion layer and the light-emitting layer is good, thereby improving the quality of the LED.

[0018] Furthermore, the stress regulating layer is formed by decomposing it through an annealing process, which can reduce the probability of the quality of the LED being affected by etching damage introduced when the stress regulating layer is formed through an etching process, thereby further improving the quality of the LED. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] In order to more clearly illustrate the technical solutions in the embodiments of the present disclosure, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present disclosure. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0020] Figure 1 is a schematic diagram of the structure of an LED provided by an embodiment of the present disclosure;

[0021] Figure 2 is a flow chart of a method for preparing an LED provided by an embodiment of the present disclosure;

[0022] Figure 3 is a flow chart of another method for preparing an LED provided by an embodiment of the present disclosure;

[0023] Figure 4 This is a schematic diagram of a structure of an LED manufacturing process provided by an embodiment of the present disclosure;

[0024] Figure 5 This is a schematic diagram of a structure of an LED manufacturing process provided by an embodiment of the present disclosure;

[0025] Figure 6 This is a schematic diagram of a structure of an LED manufacturing process provided by an embodiment of the present disclosure;

[0026] Figure 7 It is a structural schematic diagram of an LED preparation process provided by an embodiment of the present disclosure.

[0027] Reference numerals:

[0028] 10: substrate; 20: first semiconductor layer; 30: insertion layer; 31: isolation layer; 32: protrusion; 321: stress regulation layer; 321a: initial InN layer; 322: metal mask layer; 322a: initial metal layer; 33: filling layer; 40: light-emitting layer; 50: second semiconductor layer; 60: first buffer layer; 61: second buffer layer; 70: electron blocking layer; 80: contact layer. DETAILED DESCRIPTION

[0029] In order to make the objectives, technical solutions and advantages of the present disclosure more clear, the embodiments of the present disclosure will be further described in detail below with reference to the accompanying drawings.

[0030] Unless otherwise defined, the technical or scientific terms used herein shall have the usual meanings understood by persons of ordinary skill in the field to which the present disclosure belongs. The words "first", "second", "third" and similar terms used in the patent application specification and claims of the present disclosure do not indicate any order, quantity or importance, but are only used to distinguish different components. Similarly, similar words such as "one" or "one" do not indicate a quantitative limitation, but rather indicate the presence of at least one. Similar words such as "include" mean that the elements or objects appearing before "include" include the elements or objects listed after "include" and their equivalents, and do not exclude other elements or objects. "Up", "down", etc. are only used to indicate relative positional relationships. When the absolute position of the described object changes, the relative positional relationship may also change accordingly.

[0031] Figure 1is a schematic diagram of the structure of an LED provided by an embodiment of the present disclosure. The LED may be a mini light emitting diode (Mini-LED) or a micro light emitting diode (Micro-LED) of various sizes or types. Figure 1 As shown, the LED includes a first semiconductor layer 20, an insertion layer 30, a light emitting layer 40 and a second semiconductor layer 50 which are sequentially stacked.

[0032] The insertion layer 30 includes a plurality of protrusions 32 and a filling layer 33. The plurality of protrusions 32 are located between the first semiconductor layer 20 and the light-emitting layer 40. The protrusions 32 include a stress regulating layer 321, which is formed by decomposition through an annealing process. The filling layer 33 is filled between the plurality of protrusions 32.

[0033] In the embodiment of the present disclosure, an insertion layer 30 is provided between the first semiconductor layer 20 and the light-emitting layer 40, and the insertion layer 30 includes a plurality of protrusions 32 and a filling layer 33, and the plurality of protrusions 32 are located between the first semiconductor layer 20 and the light-emitting layer 40. The protrusions 32 include a stress regulating layer 321, and the stress regulating layer 321 can release the stress accumulated in the first semiconductor layer 20 due to the lattice mismatch between the substrate and the semiconductor material, and guide the dislocations generated by the lattice mismatch stress to be transferred to the sidewalls of the plurality of protrusions 32, so as to reduce the probability of the dislocations extending upward to the light-emitting layer 40, improve the quality of the light-emitting layer 40, reduce the polarization effect of the light-emitting layer 40, thereby improving the radiation recombination efficiency of electrons and holes in the light-emitting layer 40, and improving the luminous efficiency of the LED. The filling layer 33 is filled between the plurality of protrusions 32, and the filling layer 33 can fill the gaps between the plurality of protrusions 32, so as to ensure that the growth quality of the insertion layer 30 and the light-emitting layer 40 is good, thereby improving the quality of the LED.

[0034] Furthermore, the stress regulating layer 321 is formed by decomposing it through an annealing process, which can reduce the probability of the quality of the LED being affected by etching damage introduced when the stress regulating layer 321 is formed through an etching process, thereby further improving the quality of the LED.

[0035] Optionally, the stress regulation layer 321 is an InN layer. The InN material and the semiconductor material in the first semiconductor layer 20 and the light-emitting layer 40 of the LED are heterogeneous materials, which can effectively release the stress accumulated in the first semiconductor layer 20 due to the lattice mismatch between the substrate and the semiconductor material, and improve the quality of the light-emitting layer 40. And because the dissociation temperature of the InN material is low, when the InN material is annealed at a higher temperature, the InN material will be decomposed, which is conducive to decomposing and forming a convex stress regulation layer 321 through the annealing process.

[0036] In other embodiments, the stress regulating layer 321 may also be an InSb layer. InSb material can also play a role in relieving stress, and the decomposition temperature of InSb material is relatively low, and it can also be decomposed and formed by an annealing process.

[0037] Optionally, the thickness of the stress regulating layer 321 is 50nm to 100nm. If the thickness of the stress regulating layer 321 is too small, the effect of the stress regulating layer 321 in releasing the lattice mismatch stress and blocking the dislocation from extending upward is poor; if the thickness of the stress regulating layer 321 is too large, the effect of releasing the lattice mismatch stress and blocking the dislocation from extending upward is limited, resulting in increased production costs and possibly affecting the quality of the stress regulating layer 321. When the thickness of the stress regulating layer 321 is within this range, the lattice mismatch stress can be effectively released and the dislocation can be blocked from extending upward, thereby effectively improving the quality of the light-emitting layer 40 and ensuring that the quality of the stress regulating layer 321 is good.

[0038] Exemplarily, the thickness of the stress regulation layer 321 may be 70 nm to 80 nm. For example, the thickness of the stress regulation layer 321 may be 70 nm, 75 nm, or 80 nm.

[0039] Optionally, the In component content of the stress regulation layer 321 is 0.8 to 1.

[0040] For example, the In component content of the stress regulation layer 321 may be 0.8, 0.9, or 1.

[0041] Optionally, the protrusion 32 further includes a metal mask layer 322 , the stress regulation layer 321 and the metal mask layer 322 are sequentially stacked in a direction away from the first semiconductor layer 20 , and the metal mask layer 322 is formed by shrinking through an annealing process.

[0042] In this way, a metal mask layer 322 is arranged on the stress regulating layer 321. When annealing and decomposition are performed at a higher temperature, the metal mask layer 322 can protect the InN material below it, so that the InN material below the metal mask layer 322 will not be decomposed, and the InN material not protected by the metal mask layer 322 will be decomposed, that is, it plays the role of a mask. The metal mask layer 322 is formed by shrinking through the annealing process, which is conducive to forming a plurality of protrusions 32 including the stress regulating layer 321 through the annealing process. There is no need to form a plurality of protrusions 32 through the etching process, which can reduce the probability of the etching damage introduced by the etching process affecting the quality of the LED. In addition, since the etching process needs to interrupt the epitaxial growth process and then perform secondary epitaxy, not only the process steps are increased, but the secondary epitaxy is also easy to introduce impurity particles to pollute the film layer. Therefore, forming a plurality of protrusions 32 including the stress regulating layer 321 through the annealing process is also conducive to simplifying the process steps, which can reduce the probability of impurities in the etching process polluting the film layer and ensure the quality of the protrusions 32 is good.

[0043] Optionally, the metal mask layer 322 is an Al layer. Since the Al material layer will be in an unstable state when annealed under high temperature conditions, there is tension on the surface of the Al material layer, which will cause the Al material layer to break and shrink into a plurality of nanometer-scale Al droplets distributed at intervals, thereby facilitating the patterning masking effect on the stress regulation layer 321 below. In addition, Al has a high reflectivity, and the multiple protrusions 32 arranged in this way are conducive to multiple reflections of the light emitted by the light-emitting layer 40 between the multiple protrusions 32, making it easier for the light to be emitted outward, which can improve the light extraction efficiency of the LED.

[0044] In other embodiments, the metal mask layer 322 may also be an Ag layer, a Sn layer, a Zn layer, etc., which is not limited in the present disclosure.

[0045] Optionally, the thickness of the metal mask layer 322 is 1 nm to 5 nm. In this way, the metal mask layer 322 can effectively protect the InN material thereunder when annealing is performed at a relatively high temperature, and the metal mask layer 322 will not have a significant impact on the quality of the insertion layer 30 .

[0046] By way of example, the thickness of the metal mask layer 322 may be 1 nm, 3 nm, or 5 nm.

[0047] like Figure 1 As shown, the insertion layer 30 further includes an isolation layer 31, which is located between the first semiconductor layer 20 and the plurality of protrusions 32. The isolation layer 31 can isolate the plurality of protrusions 32 from the first semiconductor layer 20, reduce the effect of annealing on the quality of the first semiconductor layer 20 when forming the plurality of protrusions 32, and ensure that the quality of the first semiconductor layer 20 is good.

[0048] Optionally, the isolation layer 31 is an AlN layer or an AlGaN layer. In this way, the isolation layer 31 can isolate the plurality of protrusions 32 from the first semiconductor layer 20, so as to reduce the probability of high-temperature decomposition of the first semiconductor layer 20 when annealing at a higher temperature to form the plurality of protrusions 32, thereby ensuring good quality of the first semiconductor layer 20. Among them, the AlN layer can also release the stress accumulated in the first semiconductor layer 20 due to the lattice mismatch between the substrate and the semiconductor material, thereby further improving the luminous efficiency of the LED.

[0049] Exemplarily, the thickness of the isolation layer 31 is 1 nm to 10 nm.

[0050] Optionally, the filling layer 33 is an InGaN layer. Filling the InGaN layer between the plurality of protrusions 32 can ensure that the surface of the insertion layer 30 away from the first semiconductor layer 20 is relatively flat, which is beneficial to improving the quality of the LED. In addition, the lattice mismatch between the InGaN material and the semiconductor material in the light-emitting layer 40 is small, and the InGaN layer is beneficial to reducing the stress when growing the light-emitting layer 40, ensuring that the growth quality of the light-emitting layer 40 is good.

[0051] Illustratively, the In component content of the leveling layer 33 is 0.1 to 0.4.

[0052] Exemplarily, the thickness of the leveling layer 33 is greater than or equal to the height of the protrusions 32. That is, the leveling layer 33 may not only be filled between the plurality of protrusions 32, but also be located on the surface of the plurality of protrusions 32 away from the first semiconductor layer 20. In this way, it is beneficial to make the surface for growing the light-emitting layer 40 more flat, thereby improving the quality of the light-emitting layer 40.

[0053] Optionally, the thickness of the leveling layer 33 is 100 nm to 200 nm. Exemplarily, the thickness of the leveling layer 33 may be 140 nm to 160 nm.

[0054] like Figure 1 As shown, the LED further includes a substrate 10 , which is located on a surface of the first semiconductor layer 20 away from the insertion layer 30 .

[0055] Optionally, the substrate 10 may be a sapphire substrate, a silicon substrate or a silicon carbide substrate.

[0056] Optionally, the first semiconductor layer 20 may be an N-type GaN layer, and the second semiconductor layer 50 may be a P-type GaN layer.

[0057] Exemplarily, the first semiconductor layer 20 is a Si-doped GaN layer.

[0058] For example, the Si doping concentration of the first semiconductor layer 20 is 1*10 19 cm -3 Up to 1*10 21 cm -3 .

[0059] Exemplarily, the thickness of the first semiconductor layer 20 is 1 μm to 3 μm.

[0060] Exemplarily, the second semiconductor layer 50 is a Mg-doped GaN layer.

[0061] For example, the Mg doping concentration of the second semiconductor layer 50 is 1*10 19 cm -3 Up to 5*10 21 cm -3 .

[0062] Exemplarily, the thickness of the second semiconductor layer 50 is 30 nm to 100 nm.

[0063] Optionally, the light-emitting layer 40 is a multi-quantum well layer, including multiple pairs of InGaN layers and GaN layers stacked alternately. Different materials can be selected for the light-emitting layer 40 according to the different light-emitting wavelength ranges of the LED. For example, the light-emitting layer 40 of the blue-green LED can use multiple pairs of InGaN layers and GaN layers stacked alternately, and the light-emitting layer 40 of the red LED can use multiple pairs of InGaAs layers and GaAs layers stacked alternately.

[0064] Exemplarily, the light emitting layer 40 includes 5 to 12 pairs of alternately stacked InGaN layers and GaN layers, for example, 8 pairs of alternately stacked InGaN layers and GaN layers, and other pairs, which are not limited in the present disclosure.

[0065] Exemplarily, the thickness of the InGaN layer in the light emitting layer 40 is 2 nm to 4 nm.

[0066] Illustratively, the In component content of the InGaN layer in the light emitting layer 40 is 0.1 to 0.4.

[0067] Exemplarily, the thickness of the GaN layer in the light emitting layer 40 is 8 nm to 20 nm.

[0068] It should be noted that the materials of the first semiconductor layer 20, the light-emitting layer 40 and the second semiconductor layer 50 are only used as an example. In other embodiments, the materials of the first semiconductor layer 20, the light-emitting layer 40 and the second semiconductor layer 50 can be selected according to actual needs, and the present disclosure does not limit this.

[0069] like Figure 1 As shown, the LED further includes a first buffer layer 60 , which is located between the substrate 10 and the first semiconductor layer 20 .

[0070] Optionally, the first buffer layer 60 may be an AlN buffer layer. The AlN buffer layer may reduce the lattice mismatch between the substrate 10 and the semiconductor material, which is beneficial to reducing the lattice defects of the LED. Since the AlN buffer layer is grown at a relatively low temperature, the first buffer layer 60 may also be referred to as a low-temperature buffer layer.

[0071] Exemplarily, the thickness of the first buffer layer 60 is 15 nm to 30 nm.

[0072] Optionally, the LED further includes a second buffer layer 61 , and the second buffer layer 61 is located between the first buffer layer 60 and the first semiconductor layer 20 .

[0073] Optionally, the second buffer layer 61 may be an undoped GaN buffer layer. The undoped GaN buffer layer may reduce the thermal mismatch stress between the substrate 10 and the semiconductor material, thereby ensuring better quality of the LED. Since the undoped GaN buffer layer is grown at a relatively high temperature, the second buffer layer 61 may also be referred to as a high-temperature buffer layer.

[0074] Exemplarily, the thickness of the second buffer layer 61 is 1 μm to 3 μm.

[0075] like Figure 1 As shown, the LED chip further includes an electron blocking layer 70, which is located between the light-emitting layer 40 and the second semiconductor layer 50. The electron blocking layer 70 can block electrons, reduce the probability of electrons escaping from the light-emitting layer 40 to the second semiconductor layer 50, and thus improve the radiation recombination efficiency of electrons and holes.

[0076] Optionally, the electron blocking layer 70 may be an AlGaN layer. Exemplarily, the Al component content of the electron blocking layer 70 is 0.1 to 0.5.

[0077] Optionally, the thickness of the electron blocking layer 70 is 50 nm to 100 nm. Exemplarily, the thickness of the electron blocking layer 70 may be 70 nm to 80 nm.

[0078] Optionally, the LED chip further includes a contact layer 80 , and the contact layer 80 is located on a surface of the second semiconductor layer 50 away from the light emitting layer 40 .

[0079] Optionally, the contact layer 80 may be a P-type GaN contact layer. The P-type GaN contact layer may be used to provide holes and is beneficial to reducing contact resistance.

[0080] Exemplarily, the contact layer 80 is a Mg-doped GaN contact layer.

[0081] For example, the Mg doping concentration of the contact layer 80 is 1*10 19 cm -3 Up to 5*10 21 cm -3 .

[0082] Exemplarily, the thickness of the contact layer 80 is 10 nm to 30 nm.

[0083] It should be noted that the above-mentioned film layer structure is only used as an example. In other embodiments, the LED may also include more or fewer film layer structures, and the present disclosure does not limit this.

[0084] Figure 2 FIG. 1 is a flow chart of a method for preparing an LED provided by an embodiment of the present disclosure. Figure 2 As shown, the preparation method comprises:

[0085] In step S101 , an insertion layer is formed on a first semiconductor layer.

[0086] Among them, the insertion layer includes multiple protrusions and a filling layer, the multiple protrusions are located between the first semiconductor layer and the light-emitting layer, the protrusions include a stress regulation layer, the stress regulation layer is decomposed and formed by an annealing process, and the filling layer is filled between the multiple protrusions.

[0087] In step S102 , a light emitting layer is formed on the insertion layer.

[0088] In step S103 , a second semiconductor layer is formed on the light emitting layer.

[0089] In the disclosed embodiment, an insertion layer is provided between the first semiconductor layer and the light-emitting layer, the insertion layer includes a plurality of protrusions and a filling layer, the plurality of protrusions are located between the first semiconductor layer and the light-emitting layer, the protrusions include a stress regulating layer, the stress regulating layer can release the stress accumulated in the first semiconductor layer due to the lattice mismatch between the substrate and the semiconductor material, guide the dislocations generated by the lattice mismatch stress to be transferred to the side walls of the plurality of protrusions, so as to reduce the probability of the dislocations extending upward to the light-emitting layer, improve the quality of the light-emitting layer, reduce the polarization effect of the light-emitting layer, thereby improving the radiation recombination efficiency of electrons and holes in the light-emitting layer, and improving the luminous efficiency of the LED. The filling layer is filled between the plurality of protrusions, and the filling layer can fill the gaps between the plurality of protrusions, so as to ensure that the growth quality of the insertion layer and the light-emitting layer is good, thereby improving the quality of the LED.

[0090] Furthermore, the stress regulating layer is formed by decomposing it through an annealing process, which can reduce the probability of the quality of the LED being affected by etching damage introduced when the stress regulating layer is formed through an etching process, thereby further improving the quality of the LED.

[0091] Figure 3 FIG. 1 is a flow chart of another method for preparing an LED provided by an embodiment of the present disclosure. Figure 3 As shown, the preparation method comprises:

[0092] In step S201 , a first buffer layer is formed on a substrate.

[0093] Optionally, the substrate may be a sapphire substrate.

[0094] For example, the substrate may be placed in a physical vapor deposition (PVD) device, the temperature may be controlled to be 500° C. to 650° C., and the pressure may be controlled to be 1 torr to 10 torr, to form an AlN buffer layer on the substrate, so as to obtain a first buffer layer.

[0095] Exemplarily, the sputtering power of the PVD equipment is 2500W to 4000W.

[0096] Optionally, before performing step S201, the preparation method may further include: decomposing oxides on the surface of the substrate using hydrogen under high temperature conditions to remove the oxides on the surface of the substrate to obtain a clean substrate.

[0097] Optionally, after completing step S201, the preparation method may further include: placing the product having the first buffer layer formed on the substrate into a metal-organic chemical vapor deposition (MOCVD) reaction chamber, controlling the temperature of the reaction chamber to 1000°C to 1200°C and the pressure to 150 torr to 500 torr, and performing annealing treatment in a hydrogen atmosphere for 5 min to 10 min.

[0098] In step S202 , a second buffer layer is formed on the first buffer layer.

[0099] Optionally, in step S202, the temperature of the reaction chamber can be controlled to be 1050° C. to 1200° C., the pressure can be 100 torr to 300 torr, NH3 and TMGa can be introduced to form an undoped GaN buffer layer on the first buffer layer to obtain a second buffer layer.

[0100] In step S203 , a first semiconductor layer is formed on the second buffer layer.

[0101] Optionally, in step S203, the temperature of the reaction chamber can be controlled to be 1100° C. to 1200° C., the pressure can be 100 torr to 300 torr, NH3, TMGa and SiH4 can be introduced to form a Si-doped GaN layer on the second buffer layer to obtain a first semiconductor layer.

[0102] In step S204 , an initial InN layer is formed on the first semiconductor layer.

[0103] Figure 4 Schematic diagram of a structure of an LED manufacturing process provided by an embodiment of the present disclosure. Figure 4 As shown, in step S204 , the temperature of the reaction chamber can be controlled to be 500° C. to 600° C., the pressure can be 50 torr to 100 torr, and NH 3 and TMIn can be introduced to form an initial InN layer 321 a on the first semiconductor layer 20 .

[0104] Optionally, before performing step S204, the temperature of the reaction chamber can be controlled to be 1000° C. to 1100° C., the pressure can be 30 torr to 50 torr, NH3 and TMAl can be introduced, and an AlN layer can be formed on the first semiconductor layer 20 to obtain an isolation layer 31. When the isolation layer 31 is formed, step S204 is to form an initial InN layer 321a on the isolation layer 31.

[0105] In step S205 , a plurality of metal mask layers in a protruding shape are formed on the initial InN layer.

[0106] Optionally, step S205 may include the following steps:

[0107] In the first step, an initial metal layer is formed on the initial InN layer.

[0108] like Figure 4 As shown, the temperature of the reaction chamber can be controlled to be 700° C. to 800° C., the pressure can be 30 torr to 50 torr, and TMAl can be introduced to form an Al material layer on the initial InN layer 321 a to obtain the initial metal layer 322 a .

[0109] In the second step, the initial metal layer is annealed to form a plurality of metal mask layers in a convex shape.

[0110] Figure 5 Schematic diagram of a structure of an LED manufacturing process provided by an embodiment of the present disclosure. Figure 5 As shown, the temperature of the reaction chamber can be controlled to be 1000°C to 1100°C, the pressure to be 50 torr to 100 torr, and hydrogen gas to be introduced as a carrier gas to Figure 4 The initial metal layer 322a in the embodiment is annealed to form Figure 5 A plurality of metal mask layers 322 are formed in a convex shape.

[0111] Optionally, the duration of annealing the initial metal layer may be 10 s to 100 s.

[0112] When annealed at a high temperature, the Al material layer will be in an unstable state. There is tension on the surface of the Al material layer, which will cause the Al material layer to rupture and shrink into multiple nano-scale Al droplets arranged at intervals, that is, forming Figure 5 The metal mask layer 322 is convex in shape. The metal mask layer 322 is beneficial for protecting the InN material thereunder in the subsequent annealing step and plays the role of a mask.

[0113] Through the above two steps, a plurality of protruding metal mask layers 322 can be formed on the initial InN layer 321 a.

[0114] In step S206 , the initial InN layer is annealed under the cover of the plurality of protrusion-shaped metal mask layers to form a plurality of protrusions.

[0115] Figure 6 Schematic diagram of a structure of an LED manufacturing process provided by an embodiment of the present disclosure. Figure 6 As shown, the temperature of the reaction chamber can be controlled to be 900° C. to 1000° C., the pressure can be 50 torr to 100 torr, hydrogen can be introduced as a carrier gas, and the protruding multiple metal mask layers 322 can be covered to form a plurality of metal mask layers 322. Figure 5 The initial InN layer 321a in the embodiment is annealed to form Figure 6 A plurality of protrusions 32 are shown.

[0116] Optionally, the duration of annealing the initial InN layer may be 1 min to 5 min.

[0117] Since the metal mask layer 322 can protect the InN material thereunder and act as a mask, the InN material protected by the metal mask layer 322 will not decompose during annealing, while the InN material not protected by the metal mask layer 322 will be decomposed, thereby forming a plurality of protrusions 32 .

[0118] In step S207, a filling layer is filled between the plurality of protrusions to obtain an insertion layer.

[0119] Figure 7 Schematic diagram of a structure of an LED manufacturing process provided by an embodiment of the present disclosure. Figure 7 As shown, the temperature of the reaction chamber can be controlled to be 700°C to 900°C, the pressure to be 50 torr to 100 torr, NH3, TMGa and TMIn are introduced, and a filling layer 33 is filled between multiple protrusions 32, and the filling layer 33 is an InGaN layer to obtain an insertion layer 30.

[0120] Through the above steps S204 to S207 , the insertion layer 30 can be formed on the first semiconductor layer 20 .

[0121] In step S208 , a light emitting layer is formed on the insertion layer.

[0122] Optionally, NH 3 , TEGa and TMIn may be introduced in step S208 to form a plurality of pairs of alternately stacked InGaN layers and GaN layers on the insertion layer to obtain a light-emitting layer.

[0123] Optionally, the growth temperature of the InGaN layer is 800° C. to 900° C., and the growth pressure is 100 torr to 300 torr.

[0124] Optionally, the growth temperature of the GaN layer is 900° C. to 1000° C., and the growth pressure is 100 torr to 300 torr.

[0125] In step S209 , an electron blocking layer is formed on the light emitting layer.

[0126] Optionally, in step S209, the temperature of the reaction chamber can be controlled to be 950° C. to 1050° C., the pressure can be 50 torr to 100 torr, NH3, TEGa and TMAl can be introduced to form an AlGaN layer on the light-emitting layer to obtain an electron blocking layer.

[0127] In step S210 , a second semiconductor layer is formed on the electron blocking layer.

[0128] Optionally, in step S210, the temperature of the reaction chamber can be controlled to be 950° C. to 1050° C., the pressure can be controlled to be 100 torr to 600 torr, NH3, TEGa and Cp2Mg can be introduced to form a Mg-doped GaN layer on the electron blocking layer to obtain a second semiconductor layer.

[0129] In step S211 , a contact layer is formed on the second semiconductor layer.

[0130] Optionally, in step S211, the temperature of the reaction chamber can be controlled to be 1000° C. to 1100° C., and the pressure can be controlled to be 100 torr to 300 torr, and NH3, TEGa and Cp2Mg can be introduced to form a Mg-doped GaN contact layer on the second semiconductor layer to obtain a contact layer.

[0131] Optionally, after completing step S211, the preparation method may include: controlling the temperature of the reaction chamber to be 650° C. to 850° C., and performing annealing treatment on the LED in a nitrogen atmosphere for a duration of 5 min to 15 min.

[0132] Optionally, the material, doping concentration, thickness, component content and number of cycles of each layer can be found in Figure 1 The detailed description of the related embodiments is omitted here.

[0133] The above description does not limit the present disclosure in any form. Although the present disclosure has been disclosed as above through the embodiments, it is not used to limit the present disclosure. Any technician familiar with the profession can make some changes or modifications to equivalent embodiments of equivalent changes using the technical contents disclosed above without departing from the scope of the technical solution of the present disclosure. However, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present disclosure without departing from the content of the technical solution of the present disclosure still falls within the scope of the technical solution of the present disclosure.

Claims

1. A light emitting diode, characterized in that: The invention comprises a first semiconductor layer (20), an insertion layer (30), a light-emitting layer (40) and a second semiconductor layer (50) which are sequentially stacked. The insertion layer (30) comprises a plurality of protrusions (32) and a filling layer (33), the plurality of protrusions (32) are located between the first semiconductor layer (20) and the light-emitting layer (40), the protrusions (32) comprise a stress regulating layer (321), and the stress regulating layer (321) is formed by decomposition using an annealing process; The filling layer (33) is filled between the plurality of protrusions (32).

2. The light emitting diode according to claim 1, characterized in that: The stress regulating layer (321) is an InN layer or an InSb layer.

3. The light emitting diode according to claim 2, characterized in that: The thickness of the stress regulating layer (321) is 50nm to 100nm.

4. The light emitting diode according to any one of claims 1 to 3, characterized in that: The protrusion (32) further comprises a metal mask layer (322), the stress regulating layer (321) and the metal mask layer (322) are stacked in sequence in a direction away from the first semiconductor layer (20), and the metal mask layer (322) is formed by shrinking through an annealing process.

5. The light emitting diode according to claim 4, characterized in that: The metal mask layer (322) is an Al layer, an Ag layer, a Sn layer or a Zn layer.

6. The light emitting diode according to claim 5, characterized in that: The thickness of the metal mask layer (322) is 1 nm to 5 nm.

7. The light emitting diode according to any one of claims 1 to 3 and claims 5 to 6, characterized in that: The insertion layer (30) further includes an isolation layer (31), wherein the isolation layer (31) is located between the first semiconductor layer (20) and the plurality of protrusions (32).

8. The light emitting diode according to claim 7, characterized in that: The isolation layer (31) is an AlN layer or an AlGaN layer.

9. The light emitting diode according to any one of claims 1 to 3, claims 5 to 6 and claim 8, characterized in that: The filling layer (33) is an InGaN layer.

10. A method for preparing a light emitting diode, characterized in that: include: An insertion layer (30) is formed on the first semiconductor layer (20), the insertion layer (30) comprising a plurality of protrusions (32) and a filling layer (33), the plurality of protrusions (32) being located between the first semiconductor layer (20) and the light-emitting layer (40), the protrusions (32) comprising a stress regulating layer (321), the stress regulating layer (321) being formed by decomposition through an annealing process, and the filling layer (33) being filled between the plurality of protrusions (32); forming a light-emitting layer (40) on the insertion layer (30); A second semiconductor layer (50) is formed on the light emitting layer (40).

Citation Information

Patent Citations

  • Gallium nitride-based light emitting diode epitaxial wafer and preparation method thereof

    CN113517381A

  • Ohmic contact structure preparation method and device based on self-assembly mask technology

    CN114420750A

  • Light emitting diode and preparation method thereof

    CN115398653A

  • Semiconductor optical element

    JP2007335854A

  • Methods to reshape spacers for multi-patterning processes using thermal decomposition materials

    US20200013619A1