Fast-charging silicon negative electrode material as well as preparation method and application thereof

By using double-layer coated fast-charging silicon negative electrode material in lithium-ion batteries, fluorine and phosphorus elements improve the diffusion and surface stability of lithium ions, the poor diffusion and poor circulation performance of lithium ions in lithium batteries are solved. The problem is that more efficient fast charging and better high temperature stability are achieved.

CN119069667APending Publication Date: 2024-12-03EVE ENERGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411098773.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Due to the structural defects of graphite negative electrode materials, existing lithium-ion fast charging lithium batteries have poor diffusion performance, poor circulation performance and insufficient high temperature stability, which limits the industrial application of lithium batteries.

Method used

Using double-layer coated fast charging silicon negative electrode material, including silicon-containing particles, fluorine-element coating and phosphorus-element coating, enhance surface stability through hydrogen bonding, absorb HF to isolate the electrolyte, improve conductivity and thermal stability , forming a more stable structure.

Benefits of technology

It significantly improves the fast charging rate performance, cycle performance and high temperature stability of lithium batteries, shortens charging time, and improves energy density and safety performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004989860790000111
    Figure BDA0004989860790000111
Patent Text Reader

Abstract

The invention specifically discloses a fast-charging silicon negative electrode material and a preparation method and application thereof. The fast-charging silicon negative electrode material comprises silicon-containing particles, a first coating layer coating the silicon-containing particles and a second coating layer coating the first coating layer, the first coating layer comprises a fluorine element, and the second coating layer comprises a phosphorus element. The preparation method has the advantages that the energy density, the rate capability, the cycle performance and the high-temperature stability of the fast-charging lithium battery are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of lithium battery technology, and in particular to a fast-charging silicon negative electrode material and a preparation method and application thereof. Background Art

[0002] In the development of new energy vehicles, in order to alleviate the problem of long charging time, the development of fast charging technology has become one of the main directions of the industry. In this context, the use of high power to charge the power battery of the whole vehicle has become a trend in market applications. Among them, since high-rate charging can further reduce the time required for charging, the research of high-rate and high-performance power batteries has become a key factor in promoting the development of the industry.

[0003] Compared with many industries, the study found that the charging rate of small power batteries in the consumer field can often reach more than 10C, while in the automotive field, the charging rate of power batteries is mostly 1C. In addition, the current commercial fast charging is mainly concentrated in the graphite system, but there are still some bottlenecks in the direct application of graphite negative electrodes to fast-charging lithium-ion batteries: (1) Due to the anisotropy of the graphite layer and the narrow interlayer spacing, lithium ions can only move parallel to the graphite layers and cannot move vertically, which reduces the diffusion coefficient of lithium ions; (2) When lithium ions are embedded in the graphite layer, they enter from the layered edge of the graphite structure, making the diffusion path of lithium ions longer, and the longer diffusion path reduces the rate performance of lithium-ion batteries; (3) The graphite layers are connected by weak van der Waals forces, resulting in poor stability of the graphite structure. The process of lithium ion embedding into graphite is accompanied by the embedding of solvent molecules, causing the graphite layer to peel off; (4) Under fast charging conditions, the lithium insertion potential of the graphite layer will be close to the lithium deposition potential (the lithium plating effect mentioned above), thereby reducing the cycle performance of fast-charging lithium batteries.

[0004] Therefore, the current lithium-ion fast charging performance is poor, which is not conducive to the industrial application of lithium batteries. Summary of the invention

[0005] In order to increase the energy density of fast-charging lithium batteries and improve the rate performance, cycle performance and high-temperature stability of fast-charging lithium batteries, the present application provides a fast-charging silicon negative electrode material and a preparation method and application thereof.

[0006] In the first aspect, the present application provides a fast-charging silicon negative electrode material, which adopts the following technical solution:

[0007] A fast-charging silicon negative electrode material comprises silicon-containing particles, a first coating layer coated outside the silicon-containing particles, and a second coating layer coated outside the first coating layer; the first coating layer comprises fluorine element, and the second coating layer comprises phosphorus element.

[0008] First, silicon-containing particles are used as the main body of silicon negative electrode materials in this application, which have a high carrier concentration and mobility, and in the case of achieving high lithium storage, lithium ions have an excellent diffusion rate, thereby improving the conductivity of silicon negative electrode materials. Further, the high silicon negative electrode material of this application has a high energy density, which can improve the fast charging performance of lithium batteries while also improving the long-term performance of lithium batteries. Second, by doping the first coating layer with fluorine elements and doping the second coating layer with phosphorus elements, on the one hand, the first coating layer is in contact with silicon-containing particles, wherein the doped fluorine elements can react with the hydroxyl groups on the surface of the silicon-based material to form hydrogen bonds, and the presence of hydrogen bonds can improve the structural stability and flexibility of the SEI film on the negative electrode surface, thereby improving the conductivity of the silicon negative electrode material, especially, the silicon negative electrode material can more stably withstand the volume change of silicon-containing particles during lithium ion deintercalation, thereby achieving better fast charging cycle stability performance; on the other hand, the second coating layer can absorb HF in the electrolyte, which also helps to further isolate the silicon-containing particles from the electrolyte, further improving the stability of the silicon negative electrode material. Third, the double-layer coating structure formed by the cooperation of the second coating layer and the first coating layer can improve the coating integrity of the silicon negative electrode material, prevent the coated silicon-containing particles from contacting the electrolyte, thereby inhibiting side reactions and the formation of resistive surface films, and helping to improve the structural stability of fast-charging silicon negative electrode materials. Fourth, during the charging and discharging process, fast-charging lithium batteries will inevitably generate more heat than ordinary lithium batteries, and the first coating layer and the second coating layer can decompose at a certain temperature to produce fluorine free radicals and phosphorus free radicals, thereby improving the thermal stability and flame retardant properties of lithium batteries, and helping to improve the fast-charging safety of lithium batteries.

[0009] Preferably, the ratio of the mass of silicon element in the silicon-containing particles to the mass of fluorine element in the first coating layer is 5-20:1.

[0010] Silicon-containing particles will expand as lithium ions are inserted and extracted during the charge and discharge process. Generally, the higher the silicon content, the more significant the expansion effect of the silicon-containing particles. The present application controls the ratio of the mass of silicon in the silicon-containing particles to the mass of fluorine in the first coating layer. Controlling the fluorine content within a reasonable range helps to form an SEI film with a certain degree of flexibility, which is sufficient to alleviate the volume expansion of silicon-containing particles with the above silicon content during the charge and discharge process, thereby improving the stability of the coating structure and helping to improve the fast charging cycle performance of lithium batteries.

[0011] Preferably, the ratio of the mass of the fluorine element in the first coating layer to the mass of the phosphorus element in the second coating layer is 1-3:1.

[0012] By controlling the mass of the fluorine element in the first coating layer and the mass of the phosphorus element in the second coating layer, on the one hand, it helps to improve the conductivity of the coating layer, and on the other hand, the combination of the fluorine element in the first coating layer and the phosphorus element in the second coating layer can form a synergistic effect, significantly improving the thermal stability and flame retardant properties of the fast-charging silicon negative electrode material, further improving the structural stability of the silicon negative electrode material, and helping to improve the fast-charging performance of the lithium battery.

[0013] Preferably, the particle size D50 of the fast-charging silicon negative electrode material is 5-10 μm.

[0014] Controlling the particle size D50 of the silicon-containing particles within the above range helps to improve the coating effect of the first coating layer and the second coating layer. When the particle size D50 of the silicon-containing particles is too small, the coating effect of the first coating layer and the second coating layer is poor, which is not conducive to improving the fast charging performance of the silicon negative electrode material; when the particle size D50 of the silicon-containing particles is too large, the coating thickness of the first coating layer and the second coating layer will increase to a certain extent, which will lead to an increase in the ion transmission distance and a large interface reaction polarization, thereby reducing the rate performance of the lithium battery.

[0015] Preferably, the thickness of the first coating layer is 5-15 nm, and / or the thickness of the second coating layer is 2-10 nm.

[0016] By controlling the thickness of the first coating layer and the second coating layer, the first coating layer and the second coating layer cooperate to form a good ion path, which is beneficial to the migration and diffusion of lithium ions during the charge and discharge process, and can keep the migration coefficient of lithium ions within a good range, which helps to improve the rate performance of the lithium battery.

[0017] Preferably, the silicon-containing particles include at least one of silicon monoxide, silicon carbon, and silicon particles.

[0018] Preferably, in the first coating layer, the fluoride comprises CeF 3 , AlF 3 MgF 2 、LaF 3 At least one of .

[0019] Preferably, in the second coating layer, the phosphorus-containing compound includes at least one of lithium phosphate and calcium phosphate.

[0020] In a second aspect, the present application provides a method for preparing a fast-charging silicon negative electrode material, using the following technical solution:

[0021] A method for preparing a fast-charging silicon negative electrode material comprises the following steps:

[0022] S1, mixing a fluoride with a first organic solvent to obtain a fluorine-containing dispersion; mixing a phosphorus-containing compound with a second organic solvent to obtain a phosphorus-containing dispersion;

[0023] S2, mixing the silicon-containing particles with the fluorine-containing dispersion, stirring to obtain a first mixed liquid, and drying the first mixed liquid to obtain a first coated product;

[0024] S3, mixing the first coated product with the phosphorus-containing dispersion to obtain a second mixed liquid, and drying the second mixed liquid to obtain a second coated product, namely the fast-charging silicon negative electrode material.

[0025] Preferably, in S2, the temperature during the stirring process is 30-100°C, and the stirring time is 5-10h; the drying process is spray drying, the inlet temperature of spray drying is 100-200°C, and the outlet temperature is 60-90°C; in S3, the drying process is spray drying, the inlet temperature of spray drying is 100-200°C, and the outlet temperature is 60-90°C.

[0026] Preferably, the first organic solvent and the second organic solvent are independently selected from at least one of N,N-dimethylformamide, dimethyl sulfoxide, toluene and dichloromethane.

[0027] In a third aspect, the present application provides a negative electrode sheet, which adopts the following technical solution:

[0028] A negative electrode sheet comprises a negative electrode current collector and a negative electrode active material layer, wherein the negative electrode active material layer comprises the fast-charging silicon negative electrode material as described above.

[0029] In a fourth aspect, the present application provides a lithium-ion battery, which adopts the following technical solution:

[0030] A lithium ion battery comprises a positive electrode, a separator, an electrolyte and the negative electrode sheet as described above. DETAILED DESCRIPTION

[0031] For better understanding and implementation, the technical solution of the present application will be clearly and completely described below in conjunction with embodiments. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all of the embodiments.

[0032] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.

[0033] Unless otherwise indicated, all numerical values ​​expressing quantities of ingredients, reaction conditions, and so forth used in the specification and claims are to be understood as modified by the term “about.” Accordingly, unless indicated to the contrary, the numerical parameters set forth herein are approximations that can vary depending upon the desired properties desired to be obtained.

[0034] As used herein, "and / or" means one or all of the mentioned elements.

[0035] As used herein, “including” and “comprising” encompasses the case where only the stated elements are present as well as the case where there are other elements other than the stated elements.

[0036] All percentages in this application are by weight unless otherwise stated.

[0037] Unless otherwise indicated, "a", "an", "an" and "the" used in this specification are intended to include "at least one" or "one or more". For example, "a component" means one or more components, so more than one component may be considered and may be employed or used in the implementation of the embodiment.

[0038] Example 1

[0039] 1. Preparation of fast-charging silicon negative electrode materials

[0040] S1, the fluorine source (CeF 3 ) is mixed with a first organic solvent (N,N-dimethylformamide) to obtain a fluorine-containing dispersion; a phosphorus source (lithium phosphate) is mixed with a second organic solvent (N,N-dimethylformamide) to obtain a phosphorus-containing dispersion;

[0041] S2, mixing the silicon-containing particles (silicon dioxide) with the above-mentioned fluorine-containing dispersion, stirring at 80° C. for 6 hours to obtain a first mixed liquid, spray drying the above-mentioned first mixed liquid (inlet temperature is 150° C., outlet temperature is 80° C.), to obtain a first coated product;

[0042] S3, mixing the above-mentioned first coated product with the above-mentioned phosphorus-containing dispersion to obtain a second mixed liquid, spray-drying the above-mentioned second mixed liquid (inlet temperature is 150°C, outlet temperature is 70°C) to obtain a second coated product, namely, a fast-charging silicon negative electrode material.

[0043] The fast-charging silicon negative electrode material includes silicon-containing particles with a particle size D50 of 7 μm, a first coating layer with a thickness of 10 nm coated on the outside of the silicon-containing particles, and a second coating layer with a thickness of 5 nm coated on the outside of the first coating layer; the first coating layer includes fluorine element, and the second coating layer includes phosphorus element; the ratio of the mass of silicon element in the silicon-containing particles to the mass of fluorine element in the first coating layer is 10:1, and the ratio of the mass of fluorine element in the first coating layer to the mass of phosphorus element in the second coating layer is 2:1.

[0044] 2. Preparation of positive electrode

[0045] The ternary material positive electrode active material (NCM811), polyvinylidene fluoride (PVDF), and conductive carbon black (SP) are mixed and stirred in a mass ratio of 94:3:3 to obtain a positive electrode slurry, and then the positive electrode slurry is coated on an aluminum foil through a coating process, and a positive electrode sheet is obtained after drying and cold pressing processes.

[0046] 3. Preparation of negative electrode

[0047] The above-mentioned fast-charging silicon negative electrode material, conductive agent SP, conductive agent SWCNT and binder PAA are dissolved in a solvent in a mass percentage of 80:9:1:10 and mixed, the solid content is controlled at 30%, coated on a copper foil current collector, and vacuum dried to obtain a negative electrode sheet.

[0048] 4. Lithium battery preparation

[0049] The above-mentioned negative electrode sheet, the above-mentioned positive electrode sheet, and 1 mol / L LiPF 6 / EC+DMC+EMC (the volume ratio of EC:DMC:EMC=1:1:1) electrolyte, PE+alumina separator and shell are assembled into soft-pack batteries using conventional production processes.

[0050] Example 2

[0051] 1. Preparation of fast-charging silicon negative electrode materials

[0052] S1, the fluorine source (AlF 3 MgF 2 、LaF 3 ) is mixed with a first organic solvent (dimethyl sulfoxide) to obtain a fluorine-containing dispersion; a phosphorus source (calcium phosphate) is mixed with a second organic solvent (dimethyl sulfoxide) to obtain a phosphorus-containing dispersion;

[0053] S2, mixing the silicon-containing particles (silicon-carbon particles) with the above-mentioned fluorine-containing dispersion, stirring at 40° C. for 10 hours to obtain a first mixed liquid, and spray-drying the above-mentioned first mixed liquid (inlet temperature is 100° C., outlet temperature is 60° C.) to obtain a first coated product;

[0054] S3, mixing the above-mentioned first coated product with the above-mentioned phosphorus-containing dispersion to obtain a second mixed liquid, spray-drying the above-mentioned second mixed liquid (inlet temperature is 100°C, outlet temperature is 60°C) to obtain a second coated product, namely, a fast-charging silicon negative electrode material.

[0055] The fast-charging silicon negative electrode material includes silicon-containing particles with a particle size D50 of 5 μm, a first coating layer with a thickness of 5 nm coated on the outside of the silicon-containing particles, and a second coating layer with a thickness of 2 nm coated on the outside of the first coating layer; the first coating layer includes fluorine element, and the second coating layer includes phosphorus element; the ratio of the mass of silicon element in the silicon-containing particles to the mass of fluorine element in the first coating layer is 5:1, and the ratio of the mass of fluorine element in the first coating layer to the mass of phosphorus element in the second coating layer is 1:1.

[0056] 2. Preparation of positive electrode

[0057] The ternary material positive electrode active material (NCM811), polyvinylidene fluoride (PVDF), and conductive carbon black (SP) are mixed and stirred in a mass ratio of 94:3:3 to obtain a positive electrode slurry, and then the positive electrode slurry is coated on an aluminum foil through a coating process, and a positive electrode sheet is obtained after drying and cold pressing processes.

[0058] 3. Preparation of negative electrode

[0059] The above-mentioned fast-charging silicon negative electrode material, conductive agent SP, conductive agent SWCNT and binder PAA are dissolved in a solvent in a mass percentage of 80:9:1:10 and mixed, the solid content is controlled at 30%, coated on a copper foil current collector, and vacuum dried to obtain a negative electrode sheet.

[0060] 4. Lithium battery preparation

[0061] The above-mentioned negative electrode sheet, the above-mentioned positive electrode sheet, and 1 mol / L LiPF 6 / EC+DMC+EMC (the volume ratio of EC:DMC:EMC=1:1:1) electrolyte, PE+alumina separator and shell are assembled into soft-pack batteries using conventional production processes.

[0062] Example 3

[0063] 1. Preparation of fast-charging silicon negative electrode materials

[0064] S1, the fluorine source (MgF 2 ) is mixed with a first organic solvent (toluene) to obtain a fluorine-containing dispersion; a phosphorus source (lithium phosphate) is mixed with a second organic solvent (toluene) to obtain a phosphorus-containing dispersion;

[0065] S2, mixing silicon-containing particles (silicon-carbon particles and silicon particles in a mass ratio of 1:1) with the above-mentioned fluorine-containing dispersion, stirring at 100° C. for 5 hours to obtain a first mixed liquid, and spray-drying the above-mentioned first mixed liquid (inlet temperature is 200° C., outlet temperature is 90° C.) to obtain a first coated product;

[0066] S3, mixing the above-mentioned first coated product with the above-mentioned phosphorus-containing dispersion to obtain a second mixed liquid, spray-drying the above-mentioned second mixed liquid (inlet temperature is 200°C, outlet temperature is 80°C) to obtain a second coated product, namely, a fast-charging silicon negative electrode material.

[0067] The fast-charging silicon negative electrode material includes silicon-containing particles with a particle size D50 of 10 μm, a first coating layer with a thickness of 15 nm coated on the outside of the silicon-containing particles, and a second coating layer with a thickness of 10 nm coated on the outside of the first coating layer; the first coating layer includes fluorine element, and the second coating layer includes phosphorus element; the ratio of the mass of silicon element in the silicon-containing particles to the mass of fluorine element in the first coating layer is 20:1, and the ratio of the mass of fluorine element in the first coating layer to the mass of phosphorus element in the second coating layer is 3:1.

[0068] 2. Preparation of positive electrode

[0069] The ternary material positive electrode active material (NCM811), polyvinylidene fluoride (PVDF), and conductive carbon black (SP) are mixed and stirred in a mass ratio of 94:3:3 to obtain a positive electrode slurry, and then the positive electrode slurry is coated on an aluminum foil through a coating process, and a positive electrode sheet is obtained after drying and cold pressing processes.

[0070] 3. Preparation of negative electrode

[0071] The above-mentioned fast-charging silicon negative electrode material, conductive agent SP, conductive agent SWCNT and binder PAA are dissolved in a solvent in a mass percentage of 80:9:1:10 and mixed, the solid content is controlled at 30%, coated on a copper foil current collector, and vacuum dried to obtain a negative electrode sheet.

[0072] 4. Lithium battery preparation

[0073] The above-mentioned negative electrode sheet, the above-mentioned positive electrode sheet, and 1 mol / L LiPF 6 / EC+DMC+EMC (the volume ratio of EC:DMC:EMC=1:1:1) electrolyte, PE+alumina separator and shell are assembled into soft-pack batteries using conventional production processes.

[0074] Example 4

[0075] The difference between this embodiment and embodiment 1 is that the ratio of the mass of silicon element in the silicon-containing particles to the mass of fluorine element in the first coating layer is 3:1; other steps and parameter settings are consistent with those in embodiment 1.

[0076] Example 5

[0077] The difference between this embodiment and embodiment 1 is that the ratio of the mass of silicon element in the silicon-containing particles to the mass of fluorine element in the first coating layer is 22:1; the other steps and parameter settings are consistent with those in embodiment 1.

[0078] Example 6

[0079] The difference between this embodiment and embodiment 1 is that the ratio of the mass of the fluorine element in the first coating layer to the mass of the phosphorus element in the second coating layer is 0.2:1; the other steps and parameter settings are consistent with those in embodiment 1.

[0080] Example 7

[0081] The difference between this embodiment and embodiment 1 is that the ratio of the mass of the fluorine element in the first coating layer to the mass of the phosphorus element in the second coating layer is 4:1; the other steps and parameter settings are consistent with those in embodiment 1.

[0082] Example 8

[0083] The difference between this embodiment and embodiment 1 is that the particle size D50 of the fast-charging silicon negative electrode material is 3 μm; the other steps and parameter settings are consistent with those of embodiment 1.

[0084] Example 9

[0085] The difference between this embodiment and embodiment 1 is that the particle size D50 of the fast-charging silicon negative electrode material is 12 μm; the other steps and parameter settings are consistent with those of embodiment 1.

[0086] Example 10

[0087] The difference between this embodiment and embodiment 1 is that the thickness of the first coating layer is 3 nm, and the thickness of the second coating layer is 15 nm; other steps and parameter settings are consistent with those in embodiment 1.

[0088] Embodiment 11

[0089] The difference between this embodiment and embodiment 1 is that the thickness of the first coating layer is 17 nm, and the thickness of the second coating layer is 1 nm; other steps and parameter settings are consistent with those in embodiment 1.

[0090] Comparative Example 1

[0091] The difference between this comparative example and Example 1 is that the lithium battery in this comparative example is a commercial fast-charge lithium battery. Specifically, in the commercial fast-charge lithium battery in this comparative example, the positive electrode active material is NCM811 and the negative electrode active material is graphite.

[0092] Comparative Example 2

[0093] The difference between this comparative example and Example 1 is that the fast-charging silicon negative electrode material does not include the first coating layer and the second coating layer; the other steps and parameter settings are consistent with Example 1.

[0094] Comparative Example 3

[0095] The difference between this comparative example and Example 1 is that the fast-charging silicon negative electrode material does not include the first coating layer; the other steps and parameter settings are consistent with Example 1.

[0096] Comparative Example 4

[0097] The difference between this comparative example and Example 1 is that the fast-charging silicon negative electrode material does not include a second coating layer; other steps and parameter settings are consistent with Example 1.

[0098] Comparative Example 5

[0099] The difference between this comparative example and Example 1 is that the first coating layer in the fast-charging silicon negative electrode material contains phosphorus element, and the second coating layer contains fluorine element; the other steps and parameter settings are consistent with Example 1.

[0100] Test Method

[0101] 1. Rate performance test

[0102] The rate performance test was carried out on the lithium batteries of the above embodiments and comparative examples. The specific test method was as follows: at 25°C, 1C constant current discharge to 2.5V, standing for 10 min, 6C constant current constant voltage charging to 4.2V, 0.05C cut-off, recording the constant current charging capacity of the lithium battery, the total constant current constant voltage charging capacity and the highest temperature during fast charging, constant current charging ratio = constant current charging capacity / constant current constant voltage charging total capacity × 100%; the test results are recorded in Table 1.

[0103] 2. Cycle performance test

[0104] The lithium batteries of the above embodiments and comparative examples were subjected to a cycle performance test. The specific test method was as follows: at 25°C, 2C constant current and constant voltage charging to 4.2V, 0.05C cutoff, standing for 10 min, 2C constant current discharge to 2.5V, standing for 10 min, and cycling for 500 weeks. The capacity retention rate of the lithium battery after 500 cycles of 2C / 2C was recorded. The test results are recorded in Table 1.

[0105] 3. Thermal runaway (ARC) test

[0106] The lithium batteries of the above embodiments and comparative examples were subjected to thermal runaway tests. The specific test method was as follows: an ARC adiabatic thermal runaway test was started (the test sample was heated from room temperature to 45±2°C in the chamber, and after being left for 90 minutes, the temperature rise rate of the battery was detected. If the temperature rise exceeded 0.2°C (i.e., SHR>0.02°C / min) within 10 minutes, it was considered that a self-exothermic reaction occurred inside the battery, and an adiabatic environment was maintained until thermal runaway occurred in the battery; if the temperature rise did not exceed 0.2°C (i.e., SHR≤0.02°C / min) within 10 minutes, the next step temperature rise test was continued; each temperature step was 5°C, and the steps were repeated on each step. The ARC test temperature range was 45°C-300°C, the self-heating starting temperature was T1 (temperature rise rate SHR>0.02°C / min), and the thermal runaway starting temperature was T2 (temperature rise rate SHR>1°C / min); the test results were recorded in Table 1.

[0107] Note: Self-heating Rate (SHR)

[0108] 4. Lithium battery energy density test

[0109] The energy density test was performed on the lithium batteries in the above embodiments and comparative examples. The specific test method was as follows: weigh the weight of the test battery, recorded as m; place the battery in a fixture, apply a force of 3000N, charge the single battery to 4.2V at a constant current of 0.33C, leave it for 30min, discharge it to 2.5V at a constant current of 0.33C, leave it for 30min, and cycle it for 3 consecutive times; calculate the discharge capacity (in Ah) and energy E (average value of three cycles), discharge energy density = E / m (in Wh / kg); the test results are recorded in Table 1.

[0110] 5. Element content test

[0111] The silicon content, fluorine content and phosphorus content in the fast-charging silicon negative electrode materials prepared in the above embodiments and comparative examples were tested, and the testing method is as follows:

[0112] The ion milling instrument uses argon ions to perform both plane grinding and cross-section cutting on the sample; using the ion beam milling (CP) test principle, after cross-section cutting with argon ions, X-ray energy spectrum analysis (EDS) is performed to calculate the mass ratio of silicon to fluorine, and the mass ratio of fluorine to phosphorus.

[0113] 6. Coating thickness test

[0114] The thickness of the first coating layer and the second coating layer of the fast-charging silicon negative electrode material prepared in the above examples and comparative examples was tested by TEM, and the test method was as follows:

[0115] (1) The silicon negative electrode material samples prepared in the above-mentioned embodiments and comparative examples are dispersed by ultrasonic vibration to remove soft agglomerates, and then dispersed in water or other solvents to prepare a sample suspension;

[0116] (2) Take a copper mesh covered with a carbon film or other polymer film, scoop out the sample suspension or use a dropper to obtain the required amount, drop it on the copper mesh, dry it with filter paper or let it dry, and then place it on the sample table for testing;

[0117] (3) Take photos at representative places with narrow size steps and good dispersion, and arbitrarily select silicon-containing particles with complete morphology to measure their size; after the first coating layer is coated on the silicon-containing particles and the sample is prepared, the thickness of the first coating layer is measured by TEM test h1; after the second coating layer is coated on the first coating layer and the sample is prepared, the total thickness of the first coating layer and the second coating layer is measured by TEM test and recorded as h; the thickness of the second coating layer is h2, so the calculation formula for the thickness of the second coating layer is: h2 = h-h1.

[0118] 7. Fast charging time test

[0119] The lithium batteries in the above-mentioned Example 1 and Comparative Example 1 were tested for fast charging time. The specific test method was as follows: at 25°C, 1C constant current discharge to 2.5V, standing for 10 minutes, 1C constant current charge to 10% SOC, standing for 10 minutes, and 7C constant current charge to 80% SOC for the fast charging time.

[0120] The test shows that the fast charging time of the lithium battery in Example 1 is 6 minutes, and the fast charging time of the lithium battery in Comparative Example 1 is 30 minutes.

[0121] Table 1

[0122]

[0123] Combining Examples 1-3, Comparative Examples 1-5 and Table 1, it can be seen that the fast-charging silicon negative electrode material prepared in the present application, which contains silicon particles, a first coating layer containing fluorine elements, and a second coating layer containing phosphorus elements, has excellent first-efficiency performance, rate performance, cycle capacity retention rate and thermal stability. Moreover, compared with the fast-charging time of commercial fast-charging lithium batteries of ≥30min, the energy density is generally <300Wh.kg -1 The fast charging time of the fast-charging lithium battery in this application is only 6 minutes (charging interval is 10% SOC-80% SOC), and the energy density can reach up to 347.4Wh.kg -1 .

[0124] This is because the fast-charging silicon negative electrode material in the present application can not only increase the diffusion rate of lithium ions, but also the introduction of fluorine can improve the flexibility and stability of the SEI film, thereby alleviating the volume change of silicon-containing particles during fast charging and discharging, and improving the cycle stability of the silicon negative electrode material; further, the second coating layer can absorb HF in the electrolyte, and combined with the first coating layer, it can isolate the silicon-containing particles from the electrolyte to the greatest extent, further improving the stability of the fast-charging silicon negative electrode material; finally, the combination of fluorine and phosphorus helps to improve the stability of the fast-charging silicon negative electrode material in a high-temperature environment. The fast charging process will inevitably generate more heat. Therefore, the combination of fluorine and phosphorus has a significant contribution to the high-temperature stability and safety performance of lithium batteries.

[0125] In combination with Example 1, Examples 4-5 and Table 1, it can be seen that when the mass ratio of silicon content to fluorine content is too low, the rate performance of the lithium battery is slightly reduced, and at this time, the effect of the combination of fluorine and phosphorus on the high temperature stability of the lithium battery is slightly reduced. When the mass ratio of silicon content to fluorine content is too high, the silicon-containing particles contain too much silicon, and the SEI film is not enough to buffer the volume expansion of the silicon-containing particles during the fast charging process, which will affect the structural stability of the fast-charging silicon negative electrode material, and then manifest as a decrease in the first-effect performance and rate performance of the lithium battery, and the coordination coating stability of the second coating layer and the first coating layer will also be affected, and in severe cases, it may even cause the silicon-containing particles to contact with the electrolyte, which is not conducive to the improvement of the cycle performance and high temperature performance of the lithium battery.

[0126] In combination with Example 1, Examples 6-7 and Table 1, it can be seen that when the mass ratio of fluorine to phosphorus is too high, it is not conducive to improving the cycle performance, rate performance and high temperature performance of the lithium battery; and when the mass ratio of fluorine to phosphorus is too low, it is not conducive to improving the rate performance and high temperature performance of the lithium battery.

[0127] Combining Example 1, Examples 8-9 and Table 1, it can be seen that if the particle size D50 of the silicon-containing particles is too large or too small, it will cause the first coating layer and the second coating layer to cover the silicon-containing particles, thereby affecting the rate performance of the lithium battery.

[0128] In combination with Example 1, Examples 10-11 and Table 1, it can be seen that by controlling the thickness of the first coating layer and the second coating layer to remain within a suitable range, a migration channel and migration distance that are beneficial to the lithium ion charge and discharge process can be formed, thereby helping to improve the rate performance of the lithium battery.

[0129] The above embodiments are only used to illustrate the technical solution of the present application rather than to limit the protection scope of the present application. Although the present application is described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that the technical solution of the present application can be modified or equivalently replaced, but these modifications or replacements are all within the protection scope of the present application.

Claims

1. A fast-charging silicon negative electrode material, characterized in that: It comprises silicon-containing particles, a first coating layer coated outside the silicon-containing particles, and a second coating layer coated outside the first coating layer; The first coating layer includes fluorine element, and the second coating layer includes phosphorus element.

2. The fast-charging silicon negative electrode material according to claim 1, characterized in that: The ratio of the mass of silicon element in the silicon-containing particles to the mass of fluorine element in the first coating layer is 5-20:

1.

3. The fast-charging silicon negative electrode material according to claim 1, characterized in that: The ratio of the mass of the fluorine element in the first coating layer to the mass of the phosphorus element in the second coating layer is 1-3:

1.

4. The fast-charging silicon negative electrode material according to claim 1, characterized in that: The particle size D50 of the fast-charging silicon negative electrode material is 5-10 μm.

5. The fast-charging silicon negative electrode material according to any one of claims 1 to 4, characterized in that: The thickness of the first coating layer is 5-15 nm, and / or the thickness of the second coating layer is 2-10 nm.

6. The fast-charging silicon negative electrode material according to claim 1, characterized in that: The silicon-containing particles include at least one of silicon oxide, silicon carbon, and silicon particles.

7. The fast-charging silicon negative electrode material according to claim 1, characterized in that: In the first coating layer, the fluoride includes at least one of CeF3, AlF3, MgF2, and LaF3.

8. The fast-charging silicon negative electrode material according to claim 1, characterized in that: In the second coating layer, the phosphorus-containing compound includes at least one of lithium phosphate and calcium phosphate.

9. The method for preparing the fast-charging silicon negative electrode material according to any one of claims 1 to 8, characterized in that: The steps include: S1, mixing a fluoride with a first organic solvent to obtain a fluorine-containing dispersion; mixing a phosphorus-containing compound with a second organic solvent to obtain a phosphorus-containing dispersion; S2, mixing the silicon-containing particles with the fluorine-containing dispersion, stirring to obtain a first mixed liquid, and drying the first mixed liquid to obtain a first coated product; S3, mixing the first coated product with the phosphorus-containing dispersion to obtain a second mixed liquid, and drying the second mixed liquid to obtain a second coated product, namely the fast-charging silicon negative electrode material.

10. A negative electrode sheet, characterized in that: It comprises a negative electrode current collector and a negative electrode active material layer, wherein the negative electrode active material layer comprises the fast-charging silicon negative electrode material according to any one of claims 1 to 8.

11. A lithium ion battery, characterized in that: The invention comprises a positive electrode, a separator, an electrolyte and the negative electrode sheet as claimed in claim 10.