Composite current collector, preparation method thereof and secondary battery
By using a composite current collector containing hydroxyalumina and conductive carbon materials in secondary batteries, the problem of large contact resistance of traditional aluminum current collectors in high temperature and high humidity environments is solved, and the electrolyte resistance and service life of the electrode sheet are improved , and reduce the pole chip interface resistance.
Patent Information
- Application Number
- CN202310626473.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-30
- Publication Date
- 2024-12-03
AI Technical Summary
The traditional aluminum current collector has a large contact resistance with the active layer under high temperature and high humidity environment, and the carbon-containing conductive coating is prone to corrosion, causing the electrode material to fall off and affect the stability of the secondary battery.
Using a composite fluid including metal foil and conductive coating, the conductive coating consists of hydroxyl alumina, conductive carbon material and binder. The bond strength of the conductive coating and metal foil is improved through high-voltage homogenization process and corona discharge treatment. , and a protective layer is formed on both sides of the conductive coating.
It improves the electrolyte resistance of the electrode sheet in high temperature and high humidity environments, extends the service life of the secondary battery, reduces the interface resistance of the electrode sheet, and reduces the self-discharge phenomenon.
Smart Images

Figure CN119069711A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of secondary batteries, and in particular to a composite current collector and a preparation method thereof, and a secondary battery. Background Art
[0002] With the rapid development of electric vehicles, there is a constant demand for high energy and high power density in secondary batteries. The current collector is an important component of secondary batteries. Its function is to carry electrode materials, collect current from the electrodes, and realize the external output of current. Conventional lithium-ion battery electrode sheets are made by evenly coating the slurry composed of active materials, binders and conductive agents on the surface of the current collector, drying it, and rolling it.
[0003] Traditional aluminum current collector (2.70g / cm 3 ) Due to its relatively smooth surface, the current collector usually has a weak interaction with the active layer, resulting in a large contact resistance between the current collector and the active layer.
[0004] The prior art proposes a method of coating a carbon-containing conductive carbon layer on the surface of a current collector. The carbon-containing conductive coating has a high surface roughness and is in direct contact with the active layer through the carbon-containing conductive coating, thereby reducing the contact resistance between the current collector and the active layer.
[0005] However, in high temperature and high humidity environments, the carbon-containing conductive coating is easily corroded by electrolyte ions, which leads to the shedding of the carbon-containing conductive coating and the active layer, increased electrode interface resistance, and other problems, affecting the stability of the secondary battery under high temperature and high humidity. Summary of the invention
[0006] Based on this, it is necessary to provide a composite current collector that can solve the above problems.
[0007] In addition, it is also necessary to provide a method for preparing the above-mentioned composite current collector.
[0008] In addition, it is also necessary to provide a secondary battery including the composite current collector.
[0009] A composite current collector comprises a metal foil and a conductive coating arranged on the surface of the metal foil;
[0010] The conductive coating comprises aluminum oxyhydroxide, a conductive carbon material and a binder.
[0011] In one embodiment, the material of the conductive coating includes, by weight, 10.5 to 21.5 parts of the conductive carbon material, 0.5 to 1 part of the aluminum oxyhydroxide, and 7 to 12 parts of the binder.
[0012] In one embodiment, the particle size of the aluminum oxyhydroxide is 1 μm to 3 μm, and the specific surface area of the aluminum oxyhydroxide is 2 m2 / g~6m 2 / g.
[0013] In one embodiment, 10.5 to 21.5 parts of the conductive carbon material are 8 to 15 parts of conductive carbon black, 2 to 5 parts of conductive graphite and 0.5 to 1.5 parts of graphene in parts by weight, and the conductive coating material further includes 3 to 10 parts of a dispersant;
[0014] The particle size of the aluminum oxyhydroxide (AlOOH) is 1.2 μm to 2.5 μm;
[0015] The particle size of the conductive graphite is 3 μm to 10 μm, and the specific surface area is 4 m 2 / g~15m 2 / g;
[0016] The particle size of the conductive carbon black is 30nm-40nm, and the DBP is 250mL / 100g-500mL / 100g;
[0017] The particle size of the graphene is 2 μm to 12 μm, the number of layers of the graphene is no more than 15, and the interlayer spacing of the graphene is 0.1 nm to 0.3 nm.
[0018] In one embodiment, a protective layer of aluminum oxyhydroxide material is formed in the area near both side ends of the conductive coating.
[0019] In one embodiment, the metal foil is aluminum foil, copper foil, nickel foil, stainless steel foil, corroded aluminum foil, corroded copper foil, corroded nickel foil or corroded stainless steel foil;
[0020] The thickness of the conductive coating is 0.8 μm to 1 μm.
[0021] A method for preparing the above-mentioned composite current collector comprises the following steps:
[0022] Mixing raw materials and a solvent to form a conductive paste, wherein the raw materials include aluminum oxyhydroxide (AlOOH), a conductive carbon material, and a binder;
[0023] Providing a metal foil and pre-treating the metal foil;
[0024] The conductive paste is coated on the pretreated metal foil and dried to obtain a composite current collector.
[0025] In one embodiment, the method further comprises spraying an aqueous solution of aluminum oxyhydroxide (AlOOH) with a concentration of 0.5 wt % to 5 wt % on the areas near the two side ends of the conductive coating and drying the aqueous solution.
[0026] In one embodiment, the operation of mixing the raw material and the solvent to form the conductive paste is: mixing the raw material and the solvent to form the conductive paste through a high-pressure homogenization process;
[0027] The operation of pre-treating the metal foil is: performing corona discharge treatment on the surface of the metal foil;
[0028] The operation of coating the conductive paste on the pretreated metal foil is: coating the conductive paste on the pretreated metal foil by a micro-dimpled coating process.
[0029] A secondary battery comprises the composite current collector.
[0030] The composite current collector of the present invention comprises a metal foil and a conductive coating arranged on the surface of the metal foil. The material of the conductive coating comprises aluminum oxide hydroxyl (AlOOH), a conductive carbon material and a binder. The addition of aluminum oxide hydroxyl (AlOOH) improves the bonding strength between the metal foil and the conductive coating on the one hand, and on the other hand, when an active layer is coated on the conductive coating, it can also improve the bonding strength between the composite current collector and the active layer. In a high temperature and high humidity environment, the conductive coating is not easily corroded by electrolyte ions, thereby avoiding the problem that the carbon-containing conductive coating and the electrode material fall off, resulting in an increase in the interface resistance of the electrode sheet.
[0031] In combination with the specific embodiments, the bonding strength between the metal foil and the conductive coating of the composite current collector of the present invention is relatively high, which improves the electrolyte resistance of the prepared electrode sheet in a high temperature and high humidity environment, increases the service life of the secondary battery in a high temperature and high humidity harsh environment, reduces self-discharge during use, and also reduces the interface resistance of the electrode sheet.
[0032] Preferably, a protective layer of aluminum oxyhydroxide material is formed in the area near both side ends of the conductive coating, which reduces the wear of the cutting seam caused by cutting the pieces in the subsequent processing and plays a role in protecting the edge of the composite current collector. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0034] in:
[0035] Figure 1 The present invention is a flow chart of a method for preparing a composite current collector according to one embodiment.
[0036] Figure 2This is a test result diagram of the bonding strength between the conductive coating and the aluminum foil of the composite current collector prepared in Examples 1 to 3 and Comparative Examples 1 to 3. DETAILED DESCRIPTION
[0037] The following will be combined with the specific embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0038] It should be noted that all directional indications in the embodiments of the present invention (such as up, down, left, right, front, back, etc.) are only used to explain the relative position relationship, movement status, etc. between the various parts in a certain specific posture. If the specific posture changes, the directional indication will also change accordingly.
[0039] In addition, the descriptions of "first", "second", etc. in the present invention are only used for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In addition, the technical solutions between the various embodiments can be combined with each other, but they must be based on the ability of ordinary technicians in the field to implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such a combination of technical solutions does not exist and is not within the scope of protection required by the present invention.
[0040] The invention discloses a composite current collector according to an embodiment of the invention, comprising a metal foil and a conductive coating arranged on the surface of the metal foil.
[0041] The materials of the conductive coating include aluminum oxyhydroxide, conductive carbon material and a binder.
[0042] AlOOH is an orthorhombic crystal system with a layered structure. In each single structural layer, oxygen ions are arranged at the vertices of the octahedron in a cubic close-packed manner, aluminum ions are located in the center of the octahedron to form a double-layer structure, and hydroxides are located on the surface of the layered structure. The layers are connected by hydrogen bonds. Due to its unique crystal structure and morphology, AlOOH has the characteristics of zero point charge, high interfacial free energy, large porosity, large specific surface area, good dispersibility, good gel solubility, and high heat resistance.
[0043] The conductive coating with aluminum oxyhydroxide (AlOOH) added has large pores that can absorb liquid and expand in a high temperature and high humidity environment, so that the composite current collector is not corroded by the free HF in the electrolyte, and the bonding force between the composite current collector and the active layer is not affected, thereby improving the service life of the entire battery cell and reducing self-discharge.
[0044] The composite current collector of the present invention comprises a metal foil and a conductive coating arranged on the surface of the metal foil. The material of the conductive coating comprises aluminum oxide hydroxyl (AlOOH), a conductive carbon material and a binder. The addition of aluminum oxide hydroxyl (AlOOH) improves the bonding strength between the metal foil and the conductive coating on the one hand, and on the other hand, when an active layer is coated on the conductive coating, it can also improve the bonding strength between the composite current collector and the active layer. In a high temperature and high humidity environment, the conductive coating is not easily corroded by electrolyte ions, thereby avoiding the problem that the carbon-containing conductive coating and the electrode material fall off, resulting in an increase in the interface resistance of the electrode sheet.
[0045] In combination with the specific embodiments, the bonding strength between the metal foil and the conductive coating of the composite current collector of the present invention is relatively high, which improves the electrolyte resistance of the prepared electrode sheet in a high temperature and high humidity environment, increases the service life of the secondary battery in a high temperature and high humidity harsh environment, reduces self-discharge during use, and also reduces the interface resistance of the electrode sheet.
[0046] The applicant also needs to point out that aluminum oxyhydroxide (AlOOH) has a wide range of uses in the fields of polymer composite materials, fireproof materials, adsorption materials, biomaterials, etc.
[0047] In the present invention, the inventor creatively adds aluminum oxyhydroxide (AlOOH) to the conductive coating of the composite current collector, which not only greatly improves the bonding strength between the metal foil and the conductive coating, but also greatly improves the bonding strength between the active layer and the composite current collector.
[0048] Preferably, in this embodiment, the material of the conductive coating includes 10.5 to 21.5 parts of conductive carbon material, 0.5 to 1 part of aluminum oxyhydroxide, and 7 to 12 parts of a binder in parts by weight.
[0049] Preferably, in this embodiment, the particle size (D50) of aluminum oxyhydroxide (AlOOH) is 1 μm to 3 μm, and the specific surface area of aluminum oxyhydroxide is 2 m 2 / g~6m 2 / g.
[0050] In one embodiment, 10.5 to 21.5 parts of the conductive carbon material are 8 to 15 parts of conductive carbon black, 2 to 5 parts of conductive graphite and 0.5 to 1.5 parts of graphene in parts by weight, and the conductive coating material also includes 3 to 10 parts of a dispersant.
[0051] More preferably, in the present embodiment, the particle size of aluminum oxyhydroxide (AlOOH) is 1.2 μm to 2.5 μm.
[0052] More preferably, in this embodiment, the particle size of the conductive graphite is 3 μm to 10 μm, and the specific surface area is 4 m 2 / g~15m 2 / g.
[0053] The conductive graphite of the present invention is in the form of flakes under a field emission scanning electron microscope, and plays a role in lateral current transmission in the present invention. Due to its high anisotropy, if the size is too large, it will take up space, resulting in a reduction in the active material layer. If the size is too large, it will take too long in the dispersion equipment, resulting in increased costs. The smaller the size of the conductive graphite, the more expensive it is and the more difficult it is to disperse. Taking all factors into consideration, in this embodiment, the particle size of the conductive graphite is 3μm to 10μm, and the specific surface area is 4m 2 / g~15m 2 / g.
[0054] The conductive carbon black of the present invention has a high specific surface area, is densely packed, and is in point-to-point contact with the conductive graphite. Conductive carbon black, superconductive carbon black, special conductive carbon black, acetylene carbon black, etc. are selected. Conductive carbon black with a unique branched shape under a field emission scanning electron microscope is preferred, with a D50 of 30nm to 40nm and a DBP of 250mL / 100g to 500mL / 100g.
[0055] Taking advantage of graphene’s exceptionally high performance (SSA>40-100m 2 / g), the present invention selects graphene oxide powder, graphene liquid, chemical vapor deposition graphene powder, organic synthetic graphene powder, etc., considering batch stability and cost, preferably, in this embodiment, the particle size of graphene is 2μm~12μm, the number of graphene layers is not more than 15, and the interlayer spacing of graphene is 0.1nm~0.3nm.
[0056] In order to effectively reduce the interface resistance, the present invention uses a mixture of carbon materials with different conductivity and microscopic morphology, such as conductive graphite, conductive carbon black, and graphene. The amount of conductive graphite used in the present invention should not be the main amount, because cracks may occur inside the particles at high magnification.
[0057] The dispersant may be a hydrophilic high molecular homopolymer with a molecular weight (Mw) of 3w to 10w.
[0058] Generally speaking, the dispersant in the present invention can be selected from CMC-Na, modified amino alcohol, acrylic copolymer, butyrolactam-based polymer, modified polyurethane, polyethylene acetamide, etc., preferably linear polyethylene acetamide with a molecular weight (Mw) of 3w to 10w.
[0059] The binder can be linear polyethylene acetamide with a pH value of 2-4.
[0060] In order to achieve the connection between the carbon material particles and the current collector, the binder in the present invention is selected from water-soluble chain polymers, styrene-butadiene rubber, nitrile rubber, carboxyl nitrile rubber, hydrogenated nitrile rubber, polyvinyl alcohol, water-based acrylic resin, etc., preferably water-based acrylic resin, with a pH value of 2-4.
[0061] Preferably, in this embodiment, a protective layer of aluminum oxyhydroxide material is formed in the area near both side ends of the conductive coating, which reduces the wear of the cutting seam caused by cutting the pieces in the subsequent processing and plays a role in protecting the edge of the composite current collector.
[0062] Preferably, in this embodiment, a protective layer of aluminum oxyhydroxide material is formed 4 cm from both side edges of the conductive coating.
[0063] Preferably, in this embodiment, the metal foil is aluminum foil, copper foil, nickel foil, stainless steel foil, corroded aluminum foil, corroded copper foil, corroded nickel foil or corroded stainless steel foil.
[0064] Preferably, in this embodiment, the thickness of the conductive coating is 0.8 μm to 1 μm.
[0065] Combination Figure 1 The present invention also discloses a method for preparing the composite current collector according to an embodiment of the present invention, comprising the following steps:
[0066] S10, mixing raw materials and solvent to form conductive paste.
[0067] The raw materials include aluminum oxyhydroxide, conductive carbon material and a binder.
[0068] Typically, the solvent is deionized water.
[0069] The raw material is the material of the conductive coating mentioned above.
[0070] Generally speaking, the total number of parts by mass of the solvent and the raw materials is 100 parts.
[0071] Specifically, in this embodiment, the raw materials include conductive graphite, conductive carbon black, graphene, AlOOH, a dispersant and a binder.
[0072] Preferably, the operation of mixing the raw material and the solvent to form the conductive paste is: mixing the raw material and the solvent to form the conductive paste through a high-pressure homogenization process.
[0073] In this embodiment, the high-pressure homogenization process is completed by a high-pressure homogenizer (NanoMizer, model ME-H10).
[0074] Specifically, S10 is: premixing conductive carbon black, conductive graphite and AlOOH into a mixed powder, mixing the dispersant and the solvent evenly, adding the mixed powder and graphene, stirring evenly to obtain a first mixed slurry, adding a binder to the mixed solution, stirring evenly in vacuum to obtain a second mixed slurry, passing the second mixed slurry through a filter and an iron remover into a high-pressure homogenization chamber, circulating 4 to 8 times to obtain a uniformly distributed conductive slurry.
[0075] In the operation of premixing the conductive carbon black, conductive graphite and AlOOH into a mixed powder, the mixing equipment can be a V-type mixer, a double cone mixer, a three-dimensional mixer, a double motion mixer, a high-speed flying knife mixer, an air flow crushing mixer, a pear knife mixer, a kneading machine, etc., preferably a double motion mixer.
[0076] The vacuum mixing operation can be completed by using a double planetary mixer, a ball mill, a sand mill, a nano grinder, an ultrasonic homogenizer, a high-pressure homogenizer, etc.
[0077] Preferably, the viscosity of the conductive paste is 100 Cp to 500 Cp.
[0078] AlOOH and conductive carbon powder are pre-mixed to achieve uniform powder mixing, and are evenly dispersed in a binder, a dispersant and a high-pressure homogenization chamber, and an interconnected network is formed between the particles, so that the conductive slurry can be evenly coated on the surface of the metal foil.
[0079] S20, providing a metal foil, and pre-treating the metal foil.
[0080] Preferably, the operation of pre-treating the metal foil is: performing corona discharge treatment on the surface of the metal foil, so as to increase the surface roughness of the metal foil and improve the wettability of the metal foil to polar solvents by generating low-temperature plasma on the surface of the metal foil.
[0081] In this embodiment, the surface of the metal foil is subjected to a corona discharge treatment using a corona machine.
[0082] Preferably, during the operation of corona discharge treatment, the frequency is 10 kHz to 30 kHz and the power is 50 KW to 70 KW.
[0083] S30, coating the conductive slurry on the pretreated metal foil, and obtaining a composite current collector after drying.
[0084] The operation of coating the conductive paste on the pretreated metal foil is as follows: coating the conductive paste on the pretreated metal foil by a micro-dimpled coating process.
[0085] In this embodiment, the micro-dimpled coating process is completed by a coating machine.
[0086] In other embodiments, the conductive paste may be coated on the pretreated metal foil by using processes such as slit coating, blade coating, roller coating, spray coating, curtain coating, brush coating, etc.
[0087] Preferably, the method further comprises, after the operation of obtaining the composite current collector after drying, spraying an AlOOH aqueous solution with a concentration of 0.5 wt % to 5 wt % on the areas near the two side ends of the conductive coating and drying.
[0088] The operation of spraying 0.5wt-5wt% AlOOH aqueous solution on the areas near the two side ends of the conductive coating and drying it reduces the cutting wear caused by cutting the pieces in the subsequent processing process and plays a role in protecting the edge of the composite current collector.
[0089] More preferably, an AlOOH aqueous solution with a concentration of 1 wt% to 3 wt% is sprayed on 4 cm of both side edges of the conductive coating.
[0090] The present invention also discloses a secondary battery including the composite current collector according to an embodiment.
[0091] Preferably, the secondary battery is a lithium-ion battery.
[0092] The following is a specific embodiment. In the specific embodiment, the aluminum foil is a high-purity light foil (East Sunshine Aluminum, width 20 cm, thickness 12 μm), the conductive graphite is flake graphite YKF-8 (Qingdao Yanhai Carbon Material Co., Ltd.), the conductive carbon black is DENKA BLACK (Denka Electric Co., Ltd.), and the AlOOH is AOH60 Dispersant: PNVA TM (showa denko), graphene is HGP-3A (Qingdao Yanhai Carbon Material Co., Ltd.), and the binder is water-based acrylic resin (Shenzhen Tongtai Chemical Technology Co., Ltd. R-2680).
[0093] Example 1
[0094] Preparation of conductive slurry: 240 g of conductive carbon black, 60 g of conductive graphite, and 15 g of AlOOH were mixed in a double-motion mixer for 4 h to obtain mixed powder A.
[0095] Mix 90mL of dispersant and deionized water evenly; then, add mixed powder A and 15g of graphene, stir at high speed to obtain mixed solution B; add 210mL of binder to mixed liquid B, stir at 3000r / min for 4h, vacuum degree 1MPa, stir at 500r / min for 1h to obtain mixed liquid C; pump mixed liquid C into a high-pressure homogenization chamber through a filter and an iron remover, cycle 4 times to obtain a uniformly distributed conductive slurry.
[0096] Current collector pretreatment: Under the condition of 70kw power of the corona machine, the aluminum foil is passed through the high-voltage electrode at a rate of 80m / min, and both sides of the aluminum foil are degreased and the roughness is increased.
[0097] The conductive slurry is pumped into the coating machine trough A, and the conductive slurry is transferred to the pretreated aluminum foil surface through the micro-concave roller A; then AlOOH is applied to 4 cm on both sides of the edge of the aluminum foil through the spray area, and immediately enters the oven area for drying; then the conductive slurry in the trough B is transferred to the other side of the aluminum foil through the micro-concave roller B, and then AlOOH is applied to 4 cm on both sides of the edge of the aluminum foil through the spray area, and dried to obtain a composite current collector with a single-sided conductive coating with a thickness of 0.8 μm.
[0098] Example 2
[0099] Different from Example 1, 210 g of conductive carbon black, 54 g of conductive graphite and 15 g of AlOOH were mixed in a V-type mixer for 6 hours to obtain mixed powder A.
[0100] Mix 120mL of dispersant and deionized water evenly; then, add mixed powder A and 30g of graphene, stir at high speed to obtain mixed solution B; add 200mL of binder to mixed liquid A, stir at 3000r / min for 6h, vacuum degree 1MPa, stir at 500r / min for 1h to obtain mixed liquid B; pump mixed liquid C into a high-pressure homogenization chamber through a filter and an iron remover, cycle 6 times to obtain a uniformly distributed conductive slurry.
[0101] Example 3
[0102] Different from Example 1, 360 g of conductive carbon black, 30 g of conductive graphite and 30 g of AlOOH were mixed in a double-motion mixer for 8 h to obtain mixed powder A.
[0103] Mix 120mL of dispersant and deionized water evenly; then, add mixed powder A and 45g of graphene, stir at high speed to obtain mixed solution B; add 225mL of binder to mixed liquid A, stir at 3000r / min for 8h, vacuum degree 1MPa, stir at 500r / min for 1h to obtain mixed liquid B; pump mixed liquid C into a high-pressure homogenization chamber through a filter and an iron remover, cycle 8 times to obtain a uniformly distributed conductive slurry.
[0104] Comparative Example 1
[0105] Different from Example 1, the current collector of Comparative Example 1 uses aluminum foil that has not been pretreated.
[0106] Comparative Example 2
[0107] Different from Example 1, the conductive paste of Comparative Example 2 was not circulated in the high-pressure homogenization chamber.
[0108] Comparative Example 3
[0109] Different from Example 1, no AlOOH is added to the conductive paste of Comparative Example 3.
[0110] Test Case
[0111] The composite current collectors prepared in Examples 1 to 3 and Comparative Examples 1 to 3 were wiped back and forth 200 times with a cotton swab sticked with lithium ion electrolyte to observe whether the wiped surface was solvent resistant.
[0112] Lithium iron phosphate (LFP) slurry (LFP: carbon black: polyvinylidene fluoride (PVDF) = 80:10:10) was coated on the surface of the composite current collector prepared in Examples 1 to 3 and Comparative Examples 1 to 3, and the corresponding pole piece electrodes were obtained by drying and rolling. The corresponding pole piece electrodes were immersed in lithium ion battery electrolyte for 30 days, and the separation of the LFP layer and the current collector was observed; the corresponding pole piece electrodes were measured for pole piece interface resistance under a resistance tester.
[0113] Preparation of lithium-ion batteries: (1) Preparation of positive electrode sheets: LFP, PVDF and conductive carbon black were mixed evenly in a mass ratio of 80:10:10 to obtain a coating slurry; the slurry was applied on the surfaces of different current collectors (Examples 1 to 3 and Comparative Examples 1 to 3), and the positive electrode sheets of lithium-ion batteries were obtained after drying, rolling and cutting.
[0114] (2) Preparation of negative electrode sheet: Graphite, CMC and conductive carbon black are mixed evenly in a mass ratio of 85:5:10 to obtain a coating slurry; the slurry is coated on the surface of copper foil, and then dried, rolled and cut to obtain a negative electrode sheet for a lithium-ion battery.
[0115] (3) Assembly of lithium-ion battery: The positive electrode sheet, separator, and negative electrode sheet are stacked in order and placed in a shell, and a gasket is placed. Then, 1 mol / L LiTFSI / propylene carbonate electrolyte is injected, and a cover plate is put on and sealed to obtain a lithium-ion button battery.
[0116] The composite current collectors prepared in Examples 1 to 3 and Comparative Examples 1 to 3 were prepared into lithium iron phosphate batteries using the above method, and were cycled 500 times using 1C charging and 0.5C discharging. The results are shown in Table 1 below.
[0117] Table 1
[0118]
[0119]
[0120] It can be seen from Table 1 that the composite current collectors prepared in Examples 1 to 3 have low interface resistance and high adhesion between the composite current collector and the active material layer.
[0121] The bonding strength between the conductive coating and the aluminum foil of the composite current collector prepared in Examples 1 to 3 and Comparative Examples 1 to 3 was tested: a 19 cm wide transparent pressure-sensitive adhesive (3M 600) was adhered to the surface of the current collector, and a fixed load stick was used to press back and forth 10 times, and then one end was pressed, the adhesive was torn off, and the adhesive was adhered to a white paper. The results are shown in FIG. Figure 2 .
[0122] Depend on Figure 2 It can be seen that the current collector surfaces of Comparative Examples 1, 2 and 3 are all exposed to white after tearing, and there are dense small spots of material on the 3M tape of Comparative Example 2 that are torn off.
[0123] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A composite current collector, characterized in that: It includes a metal foil and a conductive coating arranged on the surface of the metal foil; The conductive coating comprises aluminum oxyhydroxide, a conductive carbon material and a binder.
2. The composite current collector according to claim 1, characterized in that: In terms of weight, the material of the conductive coating includes 10.5 to 21.5 parts of the conductive carbon material, 0.5 to 1 part of the aluminum oxyhydroxide, and 7 to 12 parts of the binder.
3. The composite current collector according to claim 2, characterized in that: The particle size of the aluminum oxyhydroxide is 1 μm to 3 μm, and the specific surface area of the aluminum oxyhydroxide is 2 m 2 / g~6m 2 / g.
4. The composite current collector according to claim 2, characterized in that: In terms of weight, 10.5 to 21.5 parts of the conductive carbon material are 8 to 15 parts of conductive carbon black, 2 to 5 parts of conductive graphite and 0.5 to 1.5 parts of graphene, and the conductive coating material also includes 3 to 10 parts of a dispersant; The particle size of the aluminum oxyhydroxide is 1.2 μm to 2.5 μm; The particle size of the conductive graphite is 3 μm to 10 μm, and the specific surface area is 4 m 2 / g~15m 2 / g; The particle size of the conductive carbon black is 30nm-40nm, and the DBP is 250mL / 100g-500mL / 100g; The particle size of the graphene is 2 μm to 12 μm, the number of layers of the graphene is no more than 15, and the interlayer spacing of the graphene is 0.1 nm to 0.3 nm.
5. The composite current collector according to claim 3, characterized in that: A protective layer of aluminum oxyhydroxide material is formed in the area near both side ends of the conductive coating.
6. The composite current collector according to any one of claims 1 to 5, characterized in that: The metal foil is aluminum foil, copper foil, nickel foil, stainless steel foil, corroded aluminum foil, corroded copper foil, corroded nickel foil or corroded stainless steel foil; The thickness of the conductive coating is 0.8 μm to 1 μm.
7. A method for preparing a composite current collector according to any one of claims 1 to 6, characterized in that: The steps include: Mixing raw materials and a solvent to form a conductive paste, wherein the raw materials include aluminum oxyhydroxide, a conductive carbon material, and a binder; Providing a metal foil and pre-treating the metal foil; The conductive paste is coated on the pretreated metal foil and dried to obtain a composite current collector.
8. The method for preparing a composite current collector according to claim 7, characterized in that: The method further comprises the steps of spraying an AlOOH aqueous solution with a concentration of 0.5 wt % to 5 wt % on the areas near the two side ends of the conductive coating and drying the aqueous solution.
9. The method for preparing a composite current collector according to claim 7, characterized in that: The operation of mixing the raw material and the solvent to form the conductive paste is: mixing the raw material and the solvent to form the conductive paste through a high-pressure homogenization process; The operation of pre-treating the metal foil is: performing corona discharge treatment on the surface of the metal foil; The operation of coating the conductive paste on the pretreated metal foil is: coating the conductive paste on the pretreated metal foil by a micro-dimpled coating process.
10. A secondary battery, characterized in that: Comprising the composite current collector as claimed in any one of claims 1 to 6.