Bimetal Fe-Ce-N-C oxygen reduction electrocatalyst and preparation method and application thereof

By doping cerium ions into the Fe-based oxygen reduction electrocatalyst, the bimetallic Fe-Ce-N-C oxygen reduction electrocatalyst is solved, and high activity, high stability and Low-cost catalysts reduce hydrogen peroxide yield and improve fuel cell performance.

CN119069728APending Publication Date: 2024-12-03SHANGHAI INST OF TECH
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411240688.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing Fe-based oxygen reduction electrocatalysts have problems such as complex preparation, poor stability and high hydrogen peroxide yield, which affects the performance of fuel cells.

Method used

Bimetallic Fe-Ce-N-C oxygen reduction electrocatalyst is used to eliminate free radicals by doping cerium ions, regulating the reaction process, improving the activity and stability of the catalyst, and a simple preparation method is used to reduce costs.

Benefits of technology

The ORR activity and stability of the catalyst is significantly improved, the yield of hydrogen peroxide is reduced, the preparation process is simplified, the cost is reduced, and the catalyst performance is excellent.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069728A_ABST
    Figure CN119069728A_ABST
Patent Text Reader

Abstract

The invention relates to a bimetallic Fe-Ce-N-C oxygen reduction electrocatalyst as well as a preparation method and application thereof. The preparation method comprises the following steps: mixing and grinding a carbon source, an iron source, a cerium source and a nitrogen source which are low in price to obtain a precursor, and calcining the precursor in an N2 atmosphere to obtain the bimetallic Fe-Ce-N-C oxygen reduction electrocatalyst. Compared with the prior art, the method has the advantages that a proper proportion of bimetal is added to serve as a metal source of the ORR catalyst, free radicals generated in the oxidation reduction process can be eliminated through reasonable doping of cerium ions, ORR tends to be subjected to a four-electron reaction, the hydrogen peroxide yield of the Fe-based catalyst is effectively reduced, and the yield of the Fe-based catalyst is increased. The prepared catalyst has excellent ORR activity and stability, and shows excellent performance in a fuel cell.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of oxygen reduction catalysts, and in particular to a bimetallic Fe-Ce-NC oxygen reduction electrocatalyst and a preparation method and application thereof. Background Art

[0002] As the energy crisis and environmental pollution become increasingly serious, there is a great demand for new renewable energy. Fuel cells, as a promising environmentally friendly energy source, are widely used in electric vehicles and household power supplies, especially due to their excellent conversion efficiency, high power density, and low carbon emissions.

[0003] The oxygen reduction reaction (ORR) in fuel cells is crucial. The existing Pt-based catalysts for ORR have the problems of expensive raw materials, cumbersome and complicated methods, and poor stability. Therefore, it is of great significance to explore simple and efficient synthesis methods to prepare ORR catalysts with good catalytic performance and faster rates. In recent years, Fe-based catalysts have been regarded as potential substitutes for Pt-based and other precious metal ORR catalysts. Chinese patent CN110718694A discloses a method for preparing Fe-NC oxygen reduction electrocatalysts, which are prepared by adding a carbon source to a transition metal precursor solution, evaporating, crystallizing under a nitrogen atmosphere, and calcining after acidification; wherein the transition metal precursor solution is configured by an iron source, a zinc source, and a solvent. The invention has a complex preparation method, a high overpotential, and stability and other properties need to be improved. Moreover, most Fe-based catalysts currently have the problem of too high H2O2 yield, which affects battery performance. The introduction of Ce sites as free radical scavengers can eliminate hydrogen peroxide to improve catalyst stability.

[0004] Therefore, it is urgent to develop a highly active and stable oxygen reduction electrocatalyst to solve the above problems. Summary of the invention

[0005] The purpose of the present invention is to overcome the defects of the above-mentioned prior art and provide a bimetallic Fe-Ce-NC oxygen reduction electrocatalyst and its preparation method and application, so that the oxygen reduction reaction of the fuel cell is more inclined to 4e by doping the bimetallic - The reaction process effectively improves the ORR activity and stability of the catalyst.

[0006] The applicant believes in the process of conception that oxygen reduction reaction is an important reaction in the process of renewable energy conversion and utilization. The oxygen reduction reaction can be divided into a one-step four-electron process and a two-step two-electron process. – Pathway reduction to water, or through 2e – The cerium ion is considered to be one of the most promising free radical scavengers.3+ The free radicals generated during the redox process can be eliminated, providing an effective method for reducing the hydrogen peroxide yield of iron-based catalysts.

[0007] The purpose of the present invention can be achieved by the following technical solutions:

[0008] A method for preparing a bimetallic Fe-Ce-NC oxygen reduction electrocatalyst comprises the following steps:

[0009] S1. Dissolve sodium hydroxide solution in deionized water, add dopamine hydrochloride, seal and stir at room temperature, and dry to obtain polydopamine;

[0010] S2, fully mixing the polydopamine prepared in S1 with deionized water and a pH adjuster, then adding an iron source and a cerium source, mixing and stirring at room temperature, and finally rotary evaporating and drying to obtain a solid mixture;

[0011] S3, mixing and grinding the solid mixture obtained in S2 with a nitrogen source to obtain a precursor;

[0012] S4. The precursor prepared in S3 is calcined under a N2 atmosphere to obtain a bimetallic Fe-Ce-NC oxygen reduction electrocatalyst.

[0013] Furthermore, in S1, the volume ratio of the sodium hydroxide solution to deionized water is 1:9, and the stirring time is 12-24 hours.

[0014] Furthermore, in S2, the mass ratio of the deionized water to the pH adjuster is 9:1.

[0015] Further, in S2, the pH adjusting agent is any one of ammonia water, sodium hydroxide solution, and tris(hydroxymethyl)aminomethane hydrochloric acid solution. The concentration of ammonia water is 25%, the concentration of sodium hydroxide solution is 10 -5 mol / L, the concentration of tris(hydroxymethyl)aminomethane hydrochloric acid solution is 0.1mol / L.

[0016] Furthermore, in S2, the pH value adjusted by the pH adjuster is in the range of 7.5-8.5.

[0017] Furthermore, in S2, the polydopamine is used as a carbon source, the iron source is any one of ferric nitrate, ferrous nitrate, ferrous acetate, and ammonium ferric citrate, and the cerium source is any one of cerium chloride, cerium nitrate, cerium oxalate, and cerium carbonate.

[0018] Furthermore, in S2, the time for fully mixing and stirring the polydopamine, deionized water and pH adjuster is 0.1-0.2 hours, and the time for mixing and stirring the polydopamine, deionized water, pH adjuster, iron source and cerium source is 10-24 hours.

[0019] Furthermore, in S3, the mass ratio of the solid mixture obtained in S2 to the nitrogen source is 1:10, the nitrogen source is any one of 2,2-bipyridine, triaminophenol, 4,4',4"-triphenylamine tricarboxylate, and dicyandiamide, and the grinding time is 0.3-0.5 hours.

[0020] Furthermore, the mass ratio of the polydopamine, iron source, cerium source and nitrogen source is 9:(0.5-0.9):(0.1-0.5):90.

[0021] Furthermore, in S4, the calcination temperature is 800-1000° C., and the calcination time is 1-5 hours.

[0022] On the other hand, the present invention provides a bimetallic Fe-Ce-NC oxygen reduction electrocatalyst prepared by the above method.

[0023] On the other hand, the present invention provides the use of the bimetallic Fe-Ce-NC oxygen reduction electrocatalyst in a fuel cell.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] (1) The preparation process of the present invention is simple, the experimental conditions are not stringent, and relatively low-priced carbon sources, iron sources, cerium sources, and nitrogen sources are used, which significantly reduces the production cost of the ORR catalyst.

[0026] (2) The present invention uses rotary drying to treat the solid mixture, which can effectively improve the yield and avoid the influence of phase separation on the performance of the ORR catalyst.

[0027] (3) The present invention adds a proper proportion of bimetallic as the metal source of the ORR catalyst. The reasonable doping of cerium ions helps to eliminate the free radicals generated during the redox process, so that the ORR tends to undergo a four-electron reaction, effectively reducing the hydrogen peroxide yield of the Fe-based catalyst, and making the catalyst have excellent ORR activity and stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 The electron transfer number curves of the bimetallic Fe-Ce-NC oxygen reduction electrocatalysts prepared in Example 1, Example 2, Example 3, Example 4, and Example 5 of the present invention;

[0029] Figure 2 The hydrogen peroxide yield curve of the bimetallic Fe-Ce-NC oxygen reduction electrocatalyst prepared in Example 1, Example 2, Example 3, Example 4, and Example 5 of the present invention;

[0030] Figure 3LSV polarization curves of the bimetallic Fe-Ce-NC oxygen reduction electrocatalysts prepared in Example 1, Example 2, Example 3, Example 4, and Example 5 of the present invention;

[0031] Figure 4 This is a cyclic voltammogram of the bimetallic Fe-Ce-NC oxygen reduction electrocatalyst prepared in Example 1, Example 2, Example 3, Example 4, and Example 5 of the present invention. DETAILED DESCRIPTION

[0032] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. Any features such as preparation means, materials, structures or composition ratios not clearly described in this technical solution are regarded as common technical features disclosed in the prior art.

[0033] It should be noted that the concentration of the sodium hydroxide solution in Examples 1-5 is 10 -5 mol / L.

[0034] Example 1

[0035] A method for preparing a bimetallic Fe-Ce-NC oxygen reduction electrocatalyst comprises the following steps:

[0036] S1. Dissolve 10 mL of sodium hydroxide solution in 90 mL of deionized water, add 0.008 g of dopamine hydrochloride, seal and stir at room temperature for 12 hours, and dry to obtain polydopamine;

[0037] S2, 0.09 g of polydopamine prepared in S1 was fully mixed with 90 mL of deionized water and 10 mL of sodium hydroxide solution and stirred for 0.2 hours, then mixed with 0.005 g of ferric nitrate and 0.005 g of cerium nitrate at room temperature and stirred for 12 hours, and finally dried by rotary evaporation to obtain a solid mixture;

[0038] S3, mechanically grinding and mixing 0.09 g of the solid mixture obtained in S2 with 0.9 g of dicyandiamide to obtain a precursor;

[0039] S4. The precursor prepared in S3 was calcined in a N2 atmosphere at 900°C for 2 hours to obtain a Fe-Ce-NC oxygen reduction catalyst.

[0040] Example 2

[0041] A method for preparing a bimetallic Fe-Ce-NC oxygen reduction electrocatalyst comprises the following steps:

[0042] S1. Dissolve 10 mL of sodium hydroxide solution in 90 mL of deionized water, add 0.008 g of dopamine hydrochloride, seal and stir at room temperature for 12 hours, and dry to obtain polydopamine;

[0043] S2, 0.09 g of polydopamine prepared in S1, 90 mL of deionized water, and 10 mL of sodium hydroxide solution were fully mixed and stirred for 0.2 hours, and then mixed and stirred with 0.006 g of ferric nitrate and 0.004 g of cerium nitrate at room temperature for 12 hours, and finally dried by rotary evaporation to obtain a solid mixture;

[0044] S3, mechanically grinding and mixing 0.09 g of the solid mixture obtained in S2 with 0.9 g of dicyandiamide to obtain a precursor;

[0045] S4. The precursor prepared in S3 was calcined in a N2 atmosphere at 900°C for 2 hours to obtain a Fe-Ce-NC oxygen reduction catalyst.

[0046] Example 3

[0047] A method for preparing a bimetallic Fe-Ce-NC oxygen reduction electrocatalyst comprises the following steps:

[0048] S1. Dissolve 10 mL of sodium hydroxide solution in 90 mL of deionized water, add 0.008 g of dopamine hydrochloride, seal and stir at room temperature for 12 hours, and dry to obtain polydopamine;

[0049] S2, 0.09 g of polydopamine prepared in S1, 90 mL of deionized water, and 10 mL of sodium hydroxide solution were fully mixed and stirred for 0.2 hours, and then mixed and stirred with 0.007 g of ferric nitrate and 0.003 g of cerium nitrate at room temperature for 12 hours, and finally rotary evaporated and dried to obtain a solid mixture;

[0050] S3, mechanically grinding and mixing 0.09 g of the solid mixture obtained in S2 with 0.9 g of dicyandiamide to obtain a precursor;

[0051] S4. The precursor prepared in S3 was calcined in a N2 atmosphere at 900°C for 2 hours to obtain a Fe-Ce-NC oxygen reduction catalyst.

[0052] Example 4

[0053] A method for preparing a bimetallic Fe-Ce-NC oxygen reduction electrocatalyst comprises the following steps:

[0054] S1. Dissolve 10 mL of sodium hydroxide solution in 90 mL of deionized water, add 0.008 g of dopamine hydrochloride, seal and stir at room temperature for 12 hours, and dry to obtain polydopamine;

[0055] S2, 0.09 g of polydopamine prepared in S1, 90 mL of deionized water, and 10 mL of sodium hydroxide solution were fully mixed and stirred for 0.2 hours, and then mixed and stirred with 0.008 g of ferric nitrate and 0.002 g of cerium nitrate at room temperature for 12 hours, and finally rotary evaporated and dried to obtain a solid mixture;

[0056] S3, mechanically grinding and mixing 0.09 g of the solid mixture obtained in S2 with 0.9 g of dicyandiamide to obtain a precursor;

[0057] S4. The precursor prepared in S3 was calcined in a N2 atmosphere at 900°C for 2 hours to obtain a Fe-Ce-NC oxygen reduction catalyst.

[0058] Example 5

[0059] A method for preparing a bimetallic Fe-Ce-NC oxygen reduction electrocatalyst comprises the following steps:

[0060] S1. Dissolve 10 mL of sodium hydroxide solution in 90 mL of deionized water, add 0.008 g of dopamine hydrochloride, seal and stir at room temperature for 12 hours, and dry to obtain polydopamine;

[0061] S2, 0.09 g of polydopamine prepared in S1, 90 mL of deionized water, and 10 mL of sodium hydroxide solution were fully mixed and stirred for 0.2 hours, and then mixed and stirred with 0.009 g of ferric nitrate and 0.001 g of cerium nitrate at room temperature for 12 hours, and finally rotary evaporated and dried to obtain a solid mixture;

[0062] S3, mechanically grinding and mixing 0.09 g of the solid mixture obtained in S2 with 0.9 g of dicyandiamide to obtain a precursor;

[0063] S4. The precursor prepared in S3 was calcined in a N2 atmosphere at 900°C for 2 hours to obtain a Fe-Ce-NC oxygen reduction catalyst.

[0064] Application Example 1

[0065] This application example is the application of a bimetallic Fe-Ce-NC oxygen reduction electrocatalyst in a fuel cell.

[0066] (1) Cyclic voltammetry (CV) test

[0067] 2.5 mg of the bimetallic Fe-Ce-NC oxygen reduction electrocatalyst prepared in Example 1-5 was mixed with 0.48 mL of isopropanol and 0.02 mL of 5% Nafion solution and ultrasonically treated for 1 hour to obtain a slurry. The obtained slurry was drop-coated on a glassy carbon electrode to obtain a working electrode. Silver / silver chloride was used as a reference electrode and a platinum wire electrode was used as a counter electrode. A CV test was performed on an electrochemical workstation model CHI760E using a rotating disk electrode.

[0068] Figure 4 The cyclic voltammetry (CV) curves of different catalysts in Examples 1-5 are shown. In the tests of all catalysts, no oxygen reduction peak was detected in the N2 saturated electrolyte ( Figure 4 dashed line), while an oxygen reduction peak was observed in an O2-saturated electrolyte ( Figure 4 This indicates that all catalysts have a certain degree of catalytic activity in an alkaline medium environment.

[0069] (2) Linear sweep voltammetry (LSV) test

[0070] 2.5 mg of the bimetallic Fe-Ce-NC oxygen reduction electrocatalyst prepared in Example 1-5 was mixed with 0.48 mL of isopropanol and 0.02 mL of 5% Nafion solution and ultrasonically treated for 1 hour to obtain a slurry. The obtained slurry was drop-coated on a glassy carbon electrode to obtain a working electrode. Silver / silver chloride was used as a reference electrode and a platinum wire electrode was used as a counter electrode. The LSV test was performed on an electrochemical workstation model CHI760E using a rotating disk electrode. During the test, the rotating disk electrode rotated at a speed of 1600 r / min.

[0071] See also Figure 3 , a similar electrocatalytic trend for ORR was detected using linear sweep voltammetry (LSV) curves at a rotating disk electrode. Figure 3 As shown, the limiting current density of Example 1 is 5.463 mA / cm -2 The limiting current density of Example 2 is 5.276 mA / cm -2 .

[0072] (3) Hydrogen peroxide yield test

[0073] 2.5 mg of the bimetallic Fe-Ce-NC oxygen reduction electrocatalyst prepared in Example 1-5 was mixed with 0.48 mL of isopropanol and 0.02 mL of 5% Nafion solution and ultrasonically treated for 1 hour to obtain a slurry. The obtained slurry was drop-coated on a glassy carbon electrode to obtain a working electrode. Silver / silver chloride was used as a reference electrode and a platinum wire electrode was used as a counter electrode. The LSV test was performed on an electrochemical workstation model CHI760E using a rotating disk electrode. During the test, the rotation speed of the rotating disk electrode was 1600 r / min.

[0074] Combined with Examples 1-5 and Figure 1-2 It can be seen that according to the calculation results, the bimetallic Fe-Ce-NC oxygen reduction electrocatalyst prepared in Example 1 only produces about 0.24% to 0.85% H2O2 in the range of 0.2 to 0.8 V, and the electron transfer number is 3.97 to 3.99; the bimetallic Fe-Ce-NC oxygen reduction electrocatalyst prepared in Example 2 has a hydrogen peroxide yield of 1.72% to 2.4%, and an electron transfer number of 3.95 to 3.97, indicating that the oxygen reduction reaction is closer to a four-electron transfer reduction process.

[0075] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.

Claims

1. A method for preparing a bimetallic Fe-Ce-NC oxygen reduction electrocatalyst, characterized in that: The following steps are involved: S1. Dissolve sodium hydroxide solution in deionized water, add dopamine hydrochloride, seal and stir at room temperature, and dry to obtain polydopamine; S2, fully mixing the polydopamine prepared in S1 with deionized water and a pH adjuster, then adding an iron source and a cerium source, mixing and stirring at room temperature, and finally rotary evaporating and drying to obtain a solid mixture; S3, mixing and grinding the solid mixture obtained in S2 with a nitrogen source to obtain a precursor; S4. The precursor prepared in S3 is calcined under a N2 atmosphere to obtain a bimetallic Fe-Ce-NC oxygen reduction electrocatalyst.

2. The method for preparing a bimetallic Fe-Ce-NC oxygen reduction electrocatalyst according to claim 1, characterized in that: In S2, the mass ratio of the deionized water to the pH adjuster is 9:

1.

3. The method for preparing a bimetallic Fe-Ce-NC oxygen reduction electrocatalyst according to claim 1, characterized in that: In S2, the pH regulator is any one of ammonia water, sodium hydroxide solution, and tris(hydroxymethyl)aminomethane hydrochloric acid solution, and the pH value regulated by the pH regulator is in the range of 7.5-8.

5.

4. The method for preparing a bimetallic Fe-Ce-NC oxygen reduction electrocatalyst according to claim 1, characterized in that: In S2, the polydopamine is used as a carbon source, the iron source is any one of ferric nitrate, ferrous nitrate, ferrous acetate, and ammonium ferric citrate, and the cerium source is any one of cerium chloride, cerium nitrate, cerium oxalate, and cerium carbonate.

5. The method for preparing a bimetallic Fe-Ce-NC oxygen reduction electrocatalyst according to claim 1, characterized in that: In S2, the polydopamine, deionized water, and pH adjuster are fully mixed and stirred for 0.1-0.2 hours, and the polydopamine, deionized water, pH adjuster, iron source, and cerium source are mixed and stirred for 10-24 hours.

6. The method for preparing a bimetallic Fe-Ce-NC oxygen reduction electrocatalyst according to claim 1, characterized in that: In S3, the mass ratio of the solid mixture obtained in S2 to the nitrogen source is 1:10, the nitrogen source is any one of 2,2-bipyridine, triaminophenol, 4,4',4"-triphenylamine tricarboxylate, and dicyandiamide, and the grinding time is 0.3-0.5 hours.

7. The method for preparing a bimetallic Fe-Ce-NC oxygen reduction electrocatalyst according to claim 1, characterized in that: The mass ratio of the polydopamine, iron source, cerium source and nitrogen source is 9:(0.5-0.9):(0.1-0.5):

90.

8. The method for preparing a bimetallic Fe-Ce-NC oxygen reduction electrocatalyst according to claim 1, characterized in that: In S4, the calcination temperature is 800-1000° C., and the calcination time is 1-5 hours.

9. A bimetallic Fe-Ce-NC oxygen reduction electrocatalyst prepared by the method according to any one of claims 1 to 8.

10. Use of the bimetallic Fe-Ce-NC oxygen reduction electrocatalyst as claimed in claim 9 in a fuel cell.

Citation Information

Cited By

  • Fuel cell catalyst and fuel cell stack

    CN115244742A

  • High-stability bimetal oxygen reduction catalyst with accurately doped f-region metal as well as preparation method and application of high-stability bimetal oxygen reduction catalyst