Method for repairing and regenerating positive electrode material of waste lithium cobalt oxide battery

Through deep eutectic solvent and high temperature annealing treatment technology, the problems of complex repair process and high energy consumption of the positive electrode material of lithium-ion batteries are solved, and efficient repair and performance improvement of waste lithium cobalt oxide positive electrode materials are achieved, reducing environmental pollution and resource waste .

CN119069862APending Publication Date: 2024-12-03HARBIN INSTITUTE OF TECHNOLOGY (SHENZHEN) (INSTITUTE OF SCIENCE AND TECHNOLOGY INNOVATION HARBIN INSTITUTE OF TECHNOLOGY SHENZHEN)
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411556248.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-11-04
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing lithium-ion battery positive electrode material repair methods are complex and have high energy consumption, resulting in environmental pollution and waste of precious metal resources.

Method used

The deterior cobalt lithium-oxide battery positive electrode material is treated with deep eutectic solvent, and the lithium ions are supplemented and crystalline forms are reshaped through short high-temperature annealing treatment, thereby improving the cyclic stability and rate performance of the material.

Benefits of technology

It has achieved efficient repair of waste lithium cobalt oxide cathode materials, significantly improved cycle stability and rate performance, low energy consumption, and reduced recycling costs and environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069862A_ABST
    Figure CN119069862A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of lithium ion battery materials, in particular to a method for repairing and regenerating a positive electrode material of a waste lithium cobalt oxide battery. The method comprises the following steps: providing a waste lithium cobalt oxide battery positive electrode material; a hydrogen bond acceptor and a hydrogen bond donor are mixed, heated and stirred to obtain the deep eutectic solvent, the hydrogen bond acceptor is lithium acetate, lithium methoxide, lithium lactate, lithium phytate or n-butyllithium, and the hydrogen bond donor is glycollic acid, threonine, glycine, serine or alanine; the method comprises the following steps: mixing, heating and stirring the waste lithium cobalt oxide battery positive electrode material and a deep eutectic solvent, and separating to obtain a solid-phase material; and carrying out annealing treatment on the solid-phase material to obtain the regenerated positive electrode material. According to the method disclosed by the invention, the waste lithium cobalt oxide positive electrode material can be well repaired and regenerated, the obtained regenerated positive electrode material has good cycling stability and rate capability, and after 200 cycles, the capacity retention rate can be up to 95% or above.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of lithium ion battery materials, and in particular to a method for repairing and regenerating anode materials of waste lithium cobalt oxide batteries. Background Art

[0002] As one of the energy storage systems, lithium-ion batteries (LIBs) play an important role in our daily life. They can provide clean energy and improve the serious environmental pollution caused by the increasing depletion of fossil fuels. And due to the rapid development of energy storage systems and the rapid development of high-performance batteries for portable devices such as electric vehicles, mobile devices, laptops, electronic devices, and grid energy storage, conditions have been created for the research of new battery materials with high energy density.

[0003] However, more than 100,000 tons of scrapped lithium-ion batteries (LIBs) are generated from discarded portable electronic devices worldwide every year. Lithium cobalt oxide (LiCoO2) has become the main battery positive electrode material for these portable devices due to its stable performance and high specific capacity, accounting for 30% of the entire battery weight. The Co in LiCoO2 is a harmful and expensive metal that is harmful to human skin and respiratory system. Improper disposal of LIBs has caused serious environmental pollution and is a huge waste of precious metal resources.

[0004] Previously, many studies have focused on recovering valuable metals from the cathode materials of waste lithium batteries. In recent years, there have also been many studies on the regeneration of repaired cathode materials, but they all rely on strong acids, strong alkalis and long-term high temperatures, or require the addition of some reducing substances. Therefore, there is an urgent need to develop a more direct and effective method for recycling waste cathode materials to reduce energy costs and shorten the process.

[0005] Therefore, the prior art still needs to be improved and developed. Summary of the invention

[0006] In view of the above-mentioned deficiencies in the prior art, the purpose of the present invention is to provide a method for repairing and regenerating waste lithium cobalt oxide battery positive electrode materials, aiming to solve the problems of complex process and high energy consumption in the existing methods for repairing lithium ion battery positive electrode materials.

[0007] The technical solution of the present invention is as follows: The first aspect of the present invention provides a method for repairing and regenerating anode materials of waste lithium cobalt oxide batteries, which comprises the following steps: S1. Provide waste lithium cobalt oxide battery positive electrode materials; S2, mixing a hydrogen bond acceptor and a hydrogen bond donor, heating and stirring, to obtain a deep eutectic solvent, wherein the hydrogen bond acceptor is lithium acetate, lithium methoxide, lithium lactate, lithium phytate or n-butyl lithium, and the hydrogen bond donor is glycolic acid, threonine, glycine, serine or alanine; S3, mixing the waste lithium cobalt oxide battery positive electrode material and the deep eutectic solvent, heating and stirring, and obtaining a solid phase material by separation; S4, annealing the solid phase material to obtain a regenerated positive electrode material.

[0008] Optionally, the hydrogen bond acceptor is lithium acetate, and the hydrogen bond donor is glycolic acid.

[0009] Optionally, the molar ratio of the hydrogen bond acceptor to the hydrogen bond donor is 1:1 to 1:3.

[0010] Optionally, in step S2, the hydrogen bond acceptor and the hydrogen bond donor are mixed, heated and stirred at a heating temperature of 60°C to 120°C, a heating time of 1h to 2h, and a stirring rate of 400r / min to 800r / min.

[0011] Optionally, in step S3, the mass ratio of the deep eutectic solvent to the waste lithium cobalt oxide battery positive electrode material is 20:1 to 40:1.

[0012] Optionally, in step S3, the heating temperature for mixing, heating and stirring the waste lithium cobalt oxide battery positive electrode material and the deep eutectic solvent is 60° C. to 120° C., the heating time is 10 h to 14 h, and the stirring rate is 400 r / min to 800 r / min.

[0013] Optionally, in step S4, the solid phase material is annealed at a temperature of 800° C. to 850° C. and for a time of 1 h to 3 h.

[0014] Optionally, in step S1, the step of providing the positive electrode material of waste lithium cobalt oxide batteries specifically includes: The waste lithium cobalt oxide battery is immersed in a sodium chloride solution for discharge, the waste lithium cobalt oxide battery is disassembled to obtain a positive electrode, and the positive electrode is calcined to obtain a positive electrode material of the waste lithium cobalt oxide battery.

[0015] A second aspect of the present invention provides a regenerated positive electrode material, wherein the regenerated positive electrode material is prepared by the method for repairing and regenerating waste lithium cobalt oxide battery positive electrode materials described in the present invention.

[0016] According to a third aspect of the present invention, a lithium-ion battery is provided, comprising a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, wherein the positive electrode sheet comprises the regenerated positive electrode material described in the present invention.

[0017] Beneficial effect: The present invention provides a method for repairing and regenerating waste lithium cobalt oxide battery positive electrode materials. The waste lithium cobalt oxide battery positive electrode materials are first treated with a specific deep eutectic solvent, and then a regenerated positive electrode material is obtained by a short high-temperature annealing treatment. The method provided by the present invention can well repair and regenerate waste lithium cobalt oxide positive electrode materials, wherein the deep eutectic solvent acts as a lithium supplement and a reducing agent, which can effectively supplement the missing lithium ions in the waste lithium cobalt oxide, and make the Co in the waste lithium cobalt oxide 4+ Reduction to Co 3+ The high-temperature annealing treatment rearranges the atoms in the positive electrode material, further improves the crystallinity, eliminates the remaining structural defects, reshapes the crystal form, and further enhances the cycle stability of the regenerated positive electrode material. The regenerated positive electrode material obtained by the method of the present invention has good cycle stability and rate performance. After 200 cycles, the capacity retention rate can be as high as more than 95%. At the same time, the method of the present invention has a simple process, low energy consumption, reduces the waste of precious metal resources, reduces the cost of recycling positive electrode materials, and the deep eutectic solvent is an environmentally friendly solvent, which reduces pollution to the environment. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 FT-IR spectra of the deep eutectic solvents recovered in Examples 1 to 4 and the deep eutectic solvents before use.

[0019] Figure 2 XRD diagrams of the regenerated lithium cobalt oxide positive electrode materials prepared in Example 2, Comparative Example 1 and Comparative Example 2 and the untreated waste lithium cobalt oxide materials.

[0020] Figure 3 TEM images of the regenerated lithium cobalt oxide positive electrode material and the waste lithium cobalt oxide material prepared in Example 2.

[0021] Figure 4 The cycle performance diagrams of the regenerated lithium cobalt oxide positive electrode material and the waste lithium cobalt oxide positive electrode material prepared in Examples 1 to 3 as positive electrodes of lithium ion batteries are shown.

[0022] Figure 5 The diagrams show the rate performance of the regenerated lithium cobalt oxide positive electrode material and the waste lithium cobalt oxide positive electrode material prepared in Examples 1 to 3 as positive electrodes of lithium ion batteries, respectively.

[0023] Figure 6 The charge and discharge curves of the regenerated lithium cobalt oxide positive electrode material and the waste lithium cobalt oxide positive electrode material prepared in Example 2, Comparative Example 1 and Comparative Example 2 as the positive electrode of lithium ion batteries are shown respectively.

[0024] Figure 7 The rate cycle diagrams of the regenerated lithium cobalt oxide positive electrode material and the waste lithium cobalt oxide positive electrode material prepared in Example 2, Comparative Example 1 and Comparative Example 2 as the positive electrode of lithium ion batteries respectively. DETAILED DESCRIPTION

[0025] The present invention provides a method for repairing and regenerating the positive electrode material of waste lithium cobalt oxide batteries. In order to make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention is further described in detail below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0026] The embodiment of the present invention provides a method for repairing and regenerating anode materials of waste lithium cobalt oxide batteries, which comprises the following steps: S1. Provide waste lithium cobalt oxide battery positive electrode materials; S2, mixing a hydrogen bond acceptor and a hydrogen bond donor, heating and stirring, to obtain a deep eutectic solvent, wherein the hydrogen bond acceptor is lithium acetate, lithium methoxide, lithium lactate, lithium phytate or n-butyl lithium, and the hydrogen bond donor is glycolic acid, threonine, glycine, serine or alanine; S3, mixing the waste lithium cobalt oxide battery positive electrode material and the deep eutectic solvent, heating and stirring, and obtaining a solid phase material by separation; S4, annealing the solid phase material to obtain a regenerated positive electrode material.

[0027] The method for repairing and regenerating the positive electrode material of waste lithium cobalt oxide battery provided in an embodiment of the present invention first prepares a deep eutectic solvent (DES) by simply heating and stirring a hydrogen bond acceptor and a hydrogen bond donor, then mixes the waste lithium cobalt oxide battery positive electrode material and DES, heats and stirs them to obtain a regenerated lithium cobalt oxide positive electrode material (solid phase material), and finally obtains the final regenerated positive electrode material after a short high temperature annealing. The method of the present invention can well repair and regenerate waste lithium cobalt oxide positive electrode material, wherein the waste lithium cobalt oxide battery positive electrode material is treated with the specific DES, and DES, as a lithium supplement and reducing agent, can effectively supplement the missing lithium ions in the waste lithium cobalt oxide, and make the Co in the waste lithium cobalt oxide 4+ Reduction to Co 3+ No additional reducing additives are needed, and a short high-temperature annealing allows the atoms in the cathode material to rearrange, further improving the crystallinity, eliminating the remaining structural defects, and reshaping the crystal form, so that the cycle stability of the regenerated cathode material is further enhanced. The specific mechanism is that Li in DES + It is transferred to the surface of the waste lithium cobalt oxide positive electrode material and gradually diffuses into the interior to fill the vacancies in the lattice; the subsequent high-temperature annealing accelerates the rearrangement of Li atoms and Co atoms, causing the spinel LiCoO2 to transform back into layered LiCoO2.

[0028] The regenerated positive electrode material obtained by the method of the embodiment of the present invention has good cycle stability and rate performance. After 200 cycles, the capacity retention rate can be as high as 95% or more, which is much higher than commercial lithium cobalt oxide. At the same time, the method of the present invention has a simple process flow, low energy consumption, reduces the waste of precious metal resources, reduces the cost of recycling positive electrode materials, and the deep eutectic solvent is an environmentally friendly solvent, which reduces pollution to the environment.

[0029] The deep eutectic solvent used in the embodiment of the present invention is a deep eutectic solvent in which two components are bonded in the form of hydrogen bonds, with lithium acetate, lithium methoxide, lithium lactate, lithium phytate or n-butyl lithium as hydrogen bond acceptors, and glycolic acid, threonine, glycine, serine or alanine as hydrogen bond donors. The hydrogen bond donors and hydrogen bond acceptors have many advantages. They are not only widely available and low in cost, but also can efficiently construct intermolecular hydrogen bonds between them, which greatly promotes the formation process of deep eutectic solvent (DES). In addition, the temperature required for the preparation of DES in the embodiment of the present invention is low, the preparation time is short, and the energy consumption is effectively reduced; at the same time, the hydrogen bond donor as a key component itself exhibits good reducibility, and is non-toxic and harmless during the entire application process, ensuring environmental friendliness and safe operation.

[0030] In some embodiments, the hydrogen bond acceptor is lithium acetate, and the hydrogen bond donor is glycolic acid. The deep eutectic solvent prepared by mixing lithium acetate and glycolic acid has good thermal stability and chemical stability, and the electrochemical performance of the lithium cobalt oxide cathode material repaired and regenerated using this deep eutectic solvent is outstanding, and the first cycle discharge capacity can reach 134.83 mAh / g.

[0031] In some embodiments, the molar ratio of the hydrogen bond acceptor to the hydrogen bond donor is 1:1 to 1:3. Within this molar ratio range, the hydrogen bonds formed between the hydrogen bond donor and the hydrogen bond acceptor are more stable, and the viscosity of the DES formed at this ratio is moderate, which is beneficial to the Li + The diffusion has significant advantages.

[0032] In some embodiments, in step S2, the heating temperature for mixing, heating and stirring the hydrogen bond acceptor and the hydrogen bond donor is 60°C to 120°C (for example, 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, 120°C, etc.), the heating time is 1h to 2h, and the stirring rate is 400r / min to 800r / min (for example, 400r / min, 500r / min, 600r / min, 700r / min, 800r / min, etc.). Under the conditions of mixing, heating and stirring, the hydrogen bond donor and the hydrogen bond acceptor are uniformly mixed, and the deep eutectic solvent formed is clear and transparent, and the heating promotes the thermal motion between molecules and accelerates the kinetic process of hydrogen bond formation, so that the intermolecular interaction obstacles that may have existed can be overcome; at the same time, stirring ensures the uniform distribution of the components in the system in three-dimensional space, prevents the phenomenon of excessively high or low local concentrations, and creates favorable conditions for the extensive formation of hydrogen bonds.

[0033] In some embodiments, in step S3, the mass ratio of the deep eutectic solvent to the waste lithium cobalt oxide battery positive electrode material is 20:1 to 40:1. Within the mass ratio range, the Li + It can be replenished and restored to the maximum extent, and sufficient contact between the solvent and the material can be ensured, further improving the Li + The replenishment efficiency provides strong support for the recycling of waste lithium cobalt oxide materials.

[0034] In some embodiments, in step S3, the heating temperature of mixing, heating and stirring the waste lithium cobalt oxide battery positive electrode material and the deep eutectic solvent is 60°C to 120°C (for example, 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, 120°C, etc.), the heating time is 10h to 14h (for example, 10h, 11h, 12h, 13h, 14h, etc.), and the stirring rate is 400r / min to 800r / min (for example, 400r / min, 500r / min, 600r / min, 700r / min, 800r / min, etc.). Under the conditions of mixing, heating and stirring, the Li + It can effectively dissolve and penetrate into the microstructure of waste lithium cobalt oxide positive electrode materials, thereby restoring the electrochemical properties of the positive electrode materials.

[0035] In some embodiments, in step S4, the annealing temperature of the solid phase material is 800°C to 850°C (for example, 800°C, 810°C, 820°C, 830°C, 840°C, 850°C, etc.), and the annealing time is 1h to 3h (for example, 1h, 2h, 3h, etc.). Under the conditions of the high temperature annealing treatment, the Li and Co atoms in the lithium cobalt oxide material regenerated by deep eutectic solvent treatment are rearranged to form a more ordered and stable crystal structure. High temperature annealing not only promotes the repair of internal defects in the material, but also enhances the Li + The mobility of the materials in the lattice is enhanced, thereby improving the electrochemical activity and cycle stability of the materials.

[0036] In some embodiments, in step S1, the step of providing a waste lithium cobalt oxide battery positive electrode material specifically includes: The waste lithium cobalt oxide battery is immersed in a sodium chloride solution for discharge, the waste lithium cobalt oxide battery is disassembled to obtain a positive electrode, and the positive electrode is calcined to obtain a positive electrode material of the waste lithium cobalt oxide battery.

[0037] In some embodiments, the spent lithium cobalt oxide battery is immersed in the sodium chloride solution for 24 hours to 48 hours, so that the spent lithium cobalt oxide battery is fully discharged.

[0038] In some embodiments, the positive electrode is calcined at a temperature of 500°C to 550°C (for example, 500°C, 510°C, 520°C, 530°C, 540°C, 550°C, etc.), and the calcination time is 4h to 6h (for example, 4h, 5h, 6h, etc.).

[0039] An embodiment of the present invention further provides a regenerated positive electrode material, wherein the regenerated positive electrode material is prepared by the method for repairing and regenerating the positive electrode material of waste lithium cobalt oxide batteries described in the present invention.

[0040] An embodiment of the present invention further provides a lithium-ion battery, comprising a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, wherein the positive electrode sheet comprises the regenerated positive electrode material described in the present invention.

[0041] The present invention will be further described below by means of specific examples.

[0042] Example 1

[0043] This embodiment provides a method for repairing and regenerating the positive electrode material of waste lithium cobalt oxide batteries, which is as follows: (1) After soaking the waste lithium cobalt oxide battery in a 0.1M sodium chloride solution for 48 hours, the battery was dried in a vacuum drying oven at 60°C, the waste lithium cobalt oxide battery was disassembled to separate the positive electrode and the negative electrode, and then the positive electrode was dried and placed in a tubular furnace for calcination at 550°C for 4 hours at a heating rate of 5°C / min. After the positive electrode was cooled to room temperature, the waste lithium cobalt oxide powder and the aluminum foil were separated, and the waste lithium cobalt oxide powder obtained was the positive electrode material of the waste lithium cobalt oxide battery; (2) Glycolic acid and lithium acetate were mixed in a molar ratio of 3:1, heated and stirred to obtain a deep eutectic solvent, which was a uniform transparent liquid, wherein the heating temperature was 120°C, the heating time was 1 h, and the stirring rate was 500 r / min; (3) The deep eutectic solvent obtained in step (2) and the waste lithium cobalt oxide battery positive electrode material obtained in step (1) are mixed, heated and stirred, wherein the mass ratio of the deep eutectic solvent to the waste lithium cobalt oxide battery positive electrode material is 20:1, the heating temperature is 60°C, the heating time is 12h, and the stirring rate is 500r / min. After the stirring is completed, the mixed solution is filtered to separate the powder and the recovered deep eutectic solvent, the powder is washed three times with deionized water, and then washed three times with ethanol, and finally the powder is placed in a blast drying oven at 80°C for 12h to obtain a solid phase material; (4) The solid phase material obtained in step (3) is placed in a tubular furnace and annealed at 850° C. for 2 h at a heating rate of 5 r / min. After annealing, the solid phase material is cooled to room temperature to obtain a regenerated lithium cobalt oxide positive electrode material.

[0044] Example 2

[0045] The method of Example 2 is the same as the method of Example 1, except that the heating temperature during the mixing, heating and stirring of the deep eutectic solvent and the waste lithium cobalt oxide battery positive electrode material in step (3) is adjusted from 60° C. to 80° C., thereby finally obtaining a regenerated lithium cobalt oxide positive electrode material.

[0046] Example 3

[0047] The method of Example 3 is the same as the method of Example 1, except that the heating temperature during the mixing, heating and stirring of the deep eutectic solvent and the waste lithium cobalt oxide battery positive electrode material in step (3) is adjusted from 60° C. to 100° C., thereby finally obtaining a regenerated lithium cobalt oxide positive electrode material.

[0048] Example 4

[0049] The method of Example 4 is the same as the method of Example 1, except that the heating temperature during the mixing, heating and stirring of the deep eutectic solvent and the waste lithium cobalt oxide battery positive electrode material in step (3) is adjusted from 60° C. to 120° C., thereby finally obtaining a regenerated lithium cobalt oxide positive electrode material.

[0050] Example 5

[0051] The method of Example 5 is the same as the method of Example 2, except that the glycolic acid and lithium acetate in step (2) are replaced by alanine and lithium methoxide, and finally a regenerated lithium cobalt oxide positive electrode material is obtained.

[0052] Comparative Example 1 The method of Comparative Example 1 is the same as that of Example 2, except that glycolic acid and lithium acetate in step (2) are replaced by propylene glycol and lithium chloride, thereby finally obtaining a regenerated lithium cobalt oxide positive electrode material.

[0053] Comparative Example 2 The method of Comparative Example 2 is the same as that of Example 2, except that urea and lithium chloride are used to replace glycolic acid and lithium acetate in step (2), thereby obtaining a regenerated lithium cobalt oxide positive electrode material.

[0054] The recovered deep eutectic solvents obtained in Examples 1 to 4 were characterized by FT-IR (Fourier transform infrared spectroscopy) to explore the stability of the deep eutectic solvents used in the present invention. Figure 1 FT-IR spectra of the deep eutectic solvents recovered in Examples 1 to 4 and the deep eutectic solvents before use. The results show that compared with the deep eutectic solvents before use, the structures of the deep eutectic solvents recovered in Examples 1 to 4 have not changed, and the peak positions have not shifted or lost, which proves that the deep eutectic solvents used in the present invention have good stability and can be well recycled.

[0055] Figure 2 The XRD (X-ray diffraction) diagrams of the regenerated lithium cobalt oxide positive electrode materials prepared in Example 2, Comparative Examples 1 and 2, and the untreated waste lithium cobalt oxide material show that the characteristic peak of lithium cobalt oxide can be observed at about 18.9°, and the change in lithium content in the material will cause the (003) peak to shift to the right. It can be seen that the (003) peak of the regenerated lithium cobalt oxide positive electrode material prepared in Example 2 has the largest shift, so its supplemented lithium content is the largest, which means that the DES of the present invention can better repair and regenerate waste lithium cobalt oxide positive electrode materials.

[0056] Figure 3 TEM (transmission electron microscope) images of the regenerated lithium cobalt oxide positive electrode material and the waste lithium cobalt oxide material prepared in Example 2. It can be seen that there is an obvious spinel phase in the waste lithium cobalt oxide positive electrode material. However, after Example 2 is treated with the deep eutectic solvent of the present invention and subjected to a short period of high-temperature annealing, the spinel phase disappears, and the layered structure of lithium cobalt oxide is clearly observed, proving that the method of the present invention can well repair and regenerate waste lithium cobalt oxide positive electrode materials.

[0057] Example 6

[0058] In this example, the regenerated lithium cobalt oxide positive electrode materials prepared in Examples 1 to 3 and Comparative Examples 1 to 2, and the waste lithium cobalt oxide positive electrode materials were used as lithium ion battery positive electrode materials to prepare corresponding lithium ion batteries, and the electrochemical properties were investigated, as follows: Weigh the positive electrode material (the regenerated lithium cobalt oxide positive electrode material prepared in Examples 1 to 3 and Comparative Examples 1 to 2, and the waste lithium cobalt oxide positive electrode material are respectively used as the positive electrode material of the lithium ion battery), conductive carbon black and polyvinylidene fluoride (PVDF) in a 25 mL glass bottle in a mass ratio of 8:1:1, and then drop an appropriate amount of N-methylpyrrolidone (NMP), then put the glass bottle into a mixer for mixing and grinding to obtain a positive electrode slurry, and coat the positive electrode slurry on the surface of a 100 μm aluminum foil, vacuum dry at 80° C., press the sheet, and transfer it to a glove box in an argon atmosphere to obtain the corresponding working electrode (RLCO); A CR2032 button cell was assembled using RLCO as the working electrode, a metal lithium sheet as the counter electrode, a polyethylene / polypropylene film (Celgard2400) as the separator, and 1 M lithium hexafluorophosphate (LiPF6) and a mixture of ethylene carbonate (EC) / dimethyl carbonate (DMC) / diethyl carbonate (DEC) in a volume ratio of 1:1:1 as the electrolyte.

[0059] The cycling performance and rate performance tests of the batteries prepared using the recycled lithium cobalt oxide positive electrode materials prepared using Examples 1 to 3 and Comparative Examples 1 to 2, and the waste lithium cobalt oxide positive electrode materials were conducted on a battery testing system, and the voltage window was 3.0V to 4.2V.

[0060] Figure 4 The cycle performance diagrams of the regenerated lithium cobalt oxide positive electrode material and the waste lithium cobalt oxide positive electrode material prepared in Examples 1 to 3 as the positive electrode of a lithium ion battery are shown in Figure 1. According to the figure, the battery using the regenerated lithium cobalt oxide positive electrode material prepared in Example 1 as the positive electrode of a lithium ion battery has a first cycle discharge specific capacity of 118.45 mAh / g at a rate of 0.5C, and the battery using the regenerated lithium cobalt oxide positive electrode material prepared in Example 3 as the positive electrode of a lithium ion battery has a first cycle discharge specific capacity of 117.2 at a rate of 0.5C. 7mAh / g. Relatively speaking, the recycled lithium cobalt oxide positive electrode material prepared in Example 2 shows better cycle performance. The first-cycle discharge capacity is as high as 134.83mAh / g at a rate of 0.1C, and the first-cycle discharge capacity is as high as 128.96mAh / g at a rate of 0.5C. In addition, after 200 cycles, the discharge capacity is still maintained at 121.47mAh / g, and the capacity retention rate is as high as 95%, which is much higher than the cycle performance of the waste lithium cobalt oxide positive electrode material as the positive electrode of the lithium ion battery.

[0061] Figure 5The figure is a rate performance diagram of the regenerated lithium cobalt oxide positive electrode material and the waste lithium cobalt oxide positive electrode material prepared in Examples 1 to 3 as the positive electrode of a lithium ion battery. According to the figure, the battery using the regenerated lithium cobalt oxide positive electrode material obtained in Example 1, Example 2, and Example 3 as the positive electrode of a lithium ion battery releases a discharge capacity of 79.26 mAh / g, 95.05 mAh / g, and 85.60 mAh / g at a rate of 5C, respectively, and shows a discharge capacity of 94.47%, 97.67%, and 95.50 mAh / g at a recharge current of 0.1C, respectively. 1% equilibrium capacity. Overall, the regenerated lithium cobalt oxide positive electrode material prepared in Example 2 has the best rate performance. The discharge specific capacities of the regenerated lithium cobalt oxide positive electrode material prepared in Example 2 are 134.83mAh / g, 120.10mAh / g, 115.64mAh / g, 105.09mAh / g and 95.05mAh / g at current densities of 0.1C, 0.5C, 1C, 3C and 5C, respectively, and it shows an equilibrium capacity of 97.67% under the playback current condition of 0.1C.

[0062] Figure 6 The charge and discharge curves of the regenerated lithium cobalt oxide positive electrode material and the waste lithium cobalt oxide positive electrode material prepared in Example 2, Comparative Example 1 and Comparative Example 2 are respectively used as the positive electrode of lithium ion batteries. According to the figure, at a rate of 0.1C, the first-cycle discharge capacity of Example 2, Comparative Example 1, Comparative Example 2 and the waste lithium cobalt oxide are 134.83mAh / g, 120.47mAh / g, 117.80mAh / g and 103.01mAh / g, respectively. It can be seen from the data that Example 2 has the best electrochemical performance.

[0063] Figure 7 The regenerated lithium cobalt oxide positive electrode material and the waste lithium cobalt oxide positive electrode material prepared in Example 2, Comparative Example 1 and Comparative Example 2 are respectively used as the rate cycle diagram of the positive electrode of the lithium ion battery. According to the figure, the rate cycle performance of Example 2 is significantly better than that of Comparative Example 1 and Comparative Example 2. At a rate of 5C, the three exhibited a capacity of 95.05mAh / g, 87.44mAh / g, and 87.01mAh / g, respectively, and exhibited a balance capacity of 97.61%, 94.4%, and 94.5% at a playback current of 0.1C, respectively. The above data show that compared with other DES, the specific DES used in the present invention can better repair and regenerate waste lithium cobalt oxide positive electrode materials, and the repaired and regenerated lithium cobalt oxide positive electrode materials have better electrochemical properties.

[0064] In summary, the method for repairing and regenerating the positive electrode material of waste lithium cobalt oxide batteries provided by the present invention can well repair and regenerate the positive electrode material, wherein DES, as a lithium supplement and reducing agent, can effectively supplement the lithium ions missing in the waste lithium cobalt oxide positive electrode material, and make the Co in the waste lithium cobalt oxide 4+Reduction to Co 3+ , no additional reducing additives are needed in the process; in addition, the atoms in the positive electrode material are rearranged by short high-temperature annealing, the crystallinity is further improved, the remaining structural defects are eliminated, the crystal form is reshaped, and the cycle stability and rate performance of the lithium cobalt oxide material are enhanced. The regenerated positive electrode material obtained by the method of the present invention is used as a positive electrode material for lithium ion batteries, and the application effect is good.

[0065] It should be understood that the application of the present invention is not limited to the above examples. For ordinary technicians in this field, improvements or changes can be made based on the above description. All these improvements and changes should fall within the scope of protection of the claims attached to the present invention.

Claims

1. A method for repairing and regenerating the positive electrode material of waste lithium cobalt oxide batteries, It is characterized in that Includes steps: S1. Provide waste lithium cobalt oxide battery positive electrode materials; S2, mixing a hydrogen bond acceptor and a hydrogen bond donor, heating and stirring, to obtain a deep eutectic solvent, wherein the hydrogen bond acceptor is lithium acetate, lithium methoxide, lithium lactate, lithium phytate or n-butyl lithium, and the hydrogen bond donor is glycolic acid, threonine, glycine, serine or alanine; S3, mixing the waste lithium cobalt oxide battery positive electrode material and the deep eutectic solvent, heating and stirring, and obtaining a solid phase material by separation; S4, annealing the solid phase material to obtain a regenerated positive electrode material.

2. The method for repairing and regenerating the positive electrode material of waste lithium cobalt oxide batteries according to claim 1, It is characterized in that The hydrogen bond acceptor is lithium acetate, and the hydrogen bond donor is glycolic acid.

3. The method for repairing and regenerating the positive electrode material of waste lithium cobalt oxide batteries according to claim 1, It is characterized in that The molar ratio of the hydrogen bond acceptor to the hydrogen bond donor is 1:1 to 1:

3.

4. The method for repairing and regenerating the positive electrode material of waste lithium cobalt oxide batteries according to claim 1, It is characterized in that In step S2, the hydrogen bond acceptor and the hydrogen bond donor are mixed, heated and stirred at a heating temperature of 60°C to 120°C, a heating time of 1h to 2h, and a stirring rate of 400r / min to 800r / min.

5. The method for repairing and regenerating the positive electrode material of waste lithium cobalt oxide batteries according to claim 1, It is characterized in that In step S3, the mass ratio of the deep eutectic solvent to the waste lithium cobalt oxide battery positive electrode material is 20:1 to 40:

1.

6. The method for repairing and regenerating the positive electrode material of waste lithium cobalt oxide batteries according to claim 1, It is characterized in that In step S3, the waste lithium cobalt oxide battery positive electrode material and the deep eutectic solvent are mixed, heated and stirred at a heating temperature of 60° C. to 120° C., a heating time of 10 h to 14 h, and a stirring rate of 400 r / min to 800 r / min.

7. The method for repairing and regenerating the positive electrode material of waste lithium cobalt oxide batteries according to claim 1, It is characterized in that In step S4, the solid phase material is annealed at a temperature of 800° C. to 850° C. and for a time of 1 h to 3 h.

8. The method for repairing and regenerating the positive electrode material of waste lithium cobalt oxide batteries according to claim 1, It is characterized in that In step S1, the step of providing the positive electrode material of waste lithium cobalt oxide batteries specifically includes: The waste lithium cobalt oxide battery is immersed in a sodium chloride solution for discharge, the waste lithium cobalt oxide battery is disassembled to obtain a positive electrode, and the positive electrode is calcined to obtain a positive electrode material of the waste lithium cobalt oxide battery.

9. A regenerated positive electrode material, It is characterized in that The cathode material is prepared by the method for repairing and regenerating the cathode material of waste lithium cobalt oxide batteries as described in any one of claims 1 to 8.

10. A lithium ion battery comprising a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, It is characterized in that The positive electrode sheet includes the recycled positive electrode material as claimed in claim 9.

Citation Information

Patent Citations

  • Method for preparing ternary anode material by recycling waste lithium batteries

    CN110240207A

  • Method for recycling valuable metals of waste lithium ion battery and regenerating ternary positive electrode material

    CN112194201A

  • Method for recycling valuable metal in waste lithium ion battery positive electrode material

    CN115369250A

  • Deep eutectic lithium supplement agent and method for repairing and regenerating positive electrode material of waste lithium ion battery by deep eutectic lithium supplement agent

    CN116130818A