Long-life perovskite light-emitting diode and preparation method thereof

By introducing a suspended bridge hole structure into the perovskite light-emitting diode, fluorine-containing additives are used to reduce the surface tension of perovskite particles, the problem of short life of perovskite light-emitting diodes is solved, and higher stability and application potential are achieved.

CN119072141AInactive Publication Date: 2024-12-03NANJING TECH UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202310624801.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-30
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The short life of existing perovskite light-emitting diodes limits their application and commercialization in the field of display and lighting.

Method used

By introducing a suspended bridge hole structure into the perovskite light-emitting diode, fluorine-containing additives are used to reduce the surface tension of perovskite particles, prevent the hole transport layer from sinking into the perovskite particle gap, and form a suspended bridge hole-like interface to prevent the migration of halogen ions. , improve stability.

Benefits of technology

It realizes the long life of perovskite light-emitting diodes, extends the time of external quantum efficiency decay to a maximum value of 95%, and improves the stability and application potential of the equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119072141A_ABST
    Figure CN119072141A_ABST
Patent Text Reader

Abstract

The invention discloses a long-life perovskite light-emitting diode and a preparation method thereof. The long-life light emitting diode structurally comprises a transparent conductive substrate, an electron transport layer, a perovskite particle layer, a hole transport layer and an electrode layer from bottom to top in sequence, wherein the interface morphology between the perovskite particle layer and the hole transport layer is of a suspended bridge opening structure. According to the invention, the interface morphology between perovskite and the hole transport layer is regulated and controlled to prevent halogen ions from migrating to the electrode layer, the obtained device interface structure reduces the contact between the hole transport layer and residual raw materials in gaps of perovskite particles, the migration of the halogen ions from the perovskite layer to the hole transport layer is inhibited, and the performance of the device is improved. Therefore, the stability of the light-emitting diode is improved, and the perovskite light-emitting diode with long service life is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of perovskite light emitting diodes, and in particular relates to a long-life perovskite light emitting diode and a preparation method thereof. Background Art

[0002] Metal halide perovskite light-emitting diodes have great application potential in the field of display and lighting due to their advantages such as high external quantum efficiency, high color purity, wavelength tunability and low-temperature processability, and are expected to be applied in the field of new generation display technology. In recent years, through continuous optimization, the performance of perovskite light-emitting diodes (PeLEDs) has been significantly improved. The external quantum efficiency (EQE) of perovskite light-emitting diodes (PeLEDs) has exceeded 20%, but the current lifetime of perovskite light-emitting diodes is T 95 (The time required for the external quantum efficiency EQE to decay to 95% of the maximum value) can only be maintained for a few hours, which restricts the practical application and commercial development of perovskite light-emitting diodes.

[0003] The lifetime of perovskite light-emitting diodes remains a severe challenge, so it is urgent to improve the luminescence lifetime of perovskite light-emitting diodes. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a method for preparing a long-life perovskite light-emitting diode with a suspended bridge structure in order to solve the problem of short life of the existing perovskite light-emitting diode.

[0005] Another object of the present invention is to provide a method for preparing the long-life perovskite light-emitting diode.

[0006] The object of the present invention is achieved in the following ways:

[0007] The structure of the long-life light-emitting diode includes, from bottom to top, a transparent conductive substrate, an electron transport layer, a perovskite particle layer, a hole transport layer and an electrode layer; wherein the interface morphology between the hole transport layer and the perovskite particle layer is a suspended bridge-hole structure.

[0008] Preferably, the perovskite particle layer is composed of discrete perovskite micro-nano particles, the particle spacing is controllable, and presents a concave-convex wrinkled morphology; the hole transport layer does not sink to the bottom of the perovskite micro-nano particle gap. Further preferably, the perovskite micro-nano particles are uniformly distributed and the spacing distance is adjustable, and the adjustable range is between 10-1000nm.

[0009] The controllable particle spacing of the above-mentioned long-life perovskite light-emitting diode is achieved by controlling the proportion of the components of the perovskite precursor solution.

[0010] The perovskite particle layer is prepared by the following method: spin coating the electron transport layer with a perovskite precursor solution composed of cesium halide, methylamine halide, lead halide, zwitterionic additive, and fluorine-containing additive in a molar ratio of 0-1:1-5:1:0.01-5:0.01-0.5, with a mass fraction of 5%-20%, and the solvent is N,N-dimethylformamide or dimethyl sulfoxide; and then annealing on a heating plate at 90-150°C for 5-20 minutes. Preferably, the molar ratio of cesium halide, methylamine halide, lead halide, zwitterionic additive, and fluorine-containing additive is 0.2:2.2-2.7:1:0.5:0.05-0.1.

[0011] The perovskite particle layer can be modified by adding a fluorine-containing additive as a modifier to a perovskite precursor solution to modify the perovskite particles to obtain a discrete perovskite particle layer with hydrophobic and oleophobic properties. Alternatively, the perovskite film is post-treated with a fluorine-containing additive to form a discrete perovskite particle layer with low surface tension, presenting a concave-convex morphology. Due to the low surface tension of the perovskite, the interaction with the upper transmission layer is weakened, preventing the transmission layer from sinking into the gaps between the perovskite particles.

[0012] The fluorine-containing additive is a compound composed of one or more of a low polarizability functional group containing fluorine atoms, an aromatic group or an aliphatic group, an ammonium group or an acid group, and is not limited to a perfluorinated compound in which all hydrogen atoms in the carbon chain are replaced by fluorine atoms.

[0013] The low polarizability functional groups include monofluoromethyl (-CH2F), difluoromethyl (-CHF2), trifluoromethyl (-CF3), trifluoromethoxy (-OCF3), perfluoroalkyl (-C n F 2n+1 ) one or more; the aliphatic functional group comprises a straight chain group, an alicyclic hydrocarbon group (-C n H 2n-1 ) one or more; preferably the straight chain group includes alkyl (-C n H 2n+1 ), alkenyl (-C n H 2n-1 ), alkynyl (-C n H 2n-2 ); the aromatic functional group includes one or more of a benzene ring, a naphthalene ring, an anthracene ring, an imidazole ring, a benzimidazole ring, a pyridine ring, a quinoline ring, an indole ring and other condensed rings; the amine or acid group includes a primary amine group (-NH2), a secondary amine group (-NH), a tertiary amine group (-R2N), a quaternary amine group (-R3N + ), carboxylic acid group (-COOH), carboxylic acid ion group (-COO -), sulfonic acid group (-SO3H), sulfonate ion group (-SO3 - The most preferred fluorine-containing additive is trifluoromethoxyphenylethylamine acetic acid (TFPA) or p-(trifluoromethyl)benzylamine (CF3PMA).

[0014] Preferably, the zwitterionic additive is an amino acid molecule, preferably 5-aminovaleric acid (AVA).

[0015] The cesium halide is preferably CsI, the methylamine halide is preferably FAI, and the lead halide is preferably PbI2.

[0016] The preparation method of the long-life perovskite light-emitting diode comprises the following steps: first, spin-coating a zinc oxide layer on a transparent conductive substrate to obtain an electron transport layer, then spin-coating a perovskite precursor solution composed of cesium halide, methylamine halide, lead halide, zwitterionic additive, and fluorine-containing additive in a molar ratio of 0-1:1-5:1:0.01-5:0.01-0.5 on the electron transport layer, preferably a molar ratio of 0.2:2.2-2.7:1:0.5:0.05-0.1, a mass fraction of 5%-20%, and a solvent of N,N-dimethylformamide or dimethyl sulfoxide, and annealing on a heating plate at 90-150°C for 5-20 minutes to obtain a perovskite particle layer. Finally, spin-coating or evaporating a hole transport layer on the perovskite particle layer, and finally evaporating an electrode layer on the hole transport layer.

[0017] In the above steps, after obtaining the perovskite particle layer, a chloroform solution containing a fluorine additive can be deposited on the perovskite particle layer, and then annealed at 90-110°C on a heating plate for 3-5 minutes and cooled to room temperature to further reduce the surface tension of the perovskite and prevent the hole transport layer from sinking into the gaps between the particles.

[0018] Preferably, when evaporating the electrode layer, the evaporation rate is controlled below 0.01 nm / s, and the thickness is 4.5 nm. The evaporation rate of the electrode is maintained at 0.01 nm / s, and the thickness is 100 nm.

[0019] The preferred perovskite precursor solution is a mixture of FAI, CsI, PbI2, 5-aminopentanoic acid, and a fluorine-containing additive (p-trifluoromethoxyphenylethylamine acetic acid or p-(trifluoromethyl)benzylamine), preferably in a molar ratio of 2.2-2.7:0.2:1:0.5:0.05-0.1.

[0020] Preferably, the transparent conductive substrate is indium tin oxide conductive glass.

[0021] Preferably, the spin coating speed is 1000-4000rpm, and the time is 10-45s. The above-mentioned charge transport layer does not sink to the bottom of the particle gap by spin coating or evaporating the charge transport material with a mass fraction of 5-20mg / mL on discrete perovskite particles with hydrophobic and oleophobic properties. Therefore, the long-life light-emitting diode prepared by the method of the present invention has a controllable spacing between discrete perovskite particles, which can avoid sinking into the gap between perovskite particles to form wrinkles, and the interface morphology between the perovskite layer and the charge transport layer is a suspended bridge hole structure.

[0022] In the above method, the perovskite is an ABX3 structure, wherein: A is a cationic group (cesium ion Cs + , methylamine cation MA + , and methyl acylate FA + Any one or two of the following), B is a fourth group metal (Pb 2+ , Sn 2+ Any one of, or transition metal: Cu + , Cu 2+ , Mn 2+ ,Eu 2+ , Ni 2+ ,Co 2+ Any one of), X is a halogen anion or a combination of polyhalogen anions, such as any one or more of the halogen anions Cl, Br, and I.

[0023] The long-life light-emitting diode can be obtained by modification using the above method; the photodiode can be composed of a substrate, an anode (cathode), a hole (electron) transport layer, a light-emitting layer, an electron (hole) transport layer, and a cathode (anode).

[0024] Compared with the prior art, the present invention has the following beneficial effects: the present invention reduces the surface tension of the perovskite particles by using fluorine-containing additives, reduces the molecular force between the perovskite layer and the hole transport layer above, thereby preventing the hole transport material from being immersed in the gap between the perovskite particles. The transport layer and the particle gap form a suspended "bridge hole" interface structure. The realization of this interface structure reduces the migration of halogen ions from the perovskite layer to the hole transport layer, thereby improving the stability of the light-emitting diode and realizing a long-life perovskite light-emitting diode. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a schematic structural diagram of a long-life light-emitting diode according to Embodiment 1 of the present invention;

[0026] Figure 2 This is a cross-sectional SEM image of the long-life light-emitting diode of Example 1 of the present invention;

[0027] Figure 3is a cross-sectional structural diagram of a long-life light-emitting diode according to Embodiment 1 of the present invention;

[0028] Figure 4 is the contact angle of the perovskite film of Example 1 of the present invention;

[0029] Figure 5 The voltage-current density-irradiance curve of the light emitting diode of Example 1 of the present invention;

[0030] Figure 6 is a graph showing the external quantum efficiency-current density of the light emitting diode of Example 1 of the present invention;

[0031] Figure 7 is a light emitting diode stability curve diagram of Example 1 of the present invention;

[0032] Figure 8 is a cross-sectional structural diagram of a long-life light-emitting diode according to Embodiment 2 of the present invention;

[0033] Fig. 9 is a light emitting diode stability curve diagram of Example 2 of the present invention;

[0034] Fig.10 is a cross-sectional structural diagram of a long-life light-emitting diode according to Embodiment 3 of the present invention;

[0035] Fig.11 is a stability curve diagram of the long-life light-emitting diode of Example 3 of the present invention;

[0036] Fig.12 is a cross-sectional structural diagram of a long-life light-emitting diode according to Embodiment 4 of the present invention;

[0037] Fig.13 is a stability curve diagram of the long-life light-emitting diode of Example 4 of the present invention;

[0038] Fig.14 is a cross-sectional structural diagram of a light emitting diode according to Embodiment 5 of the present invention;

[0039] Fig.15 This is a stability curve diagram of the light emitting diode of Example 5 of the present invention. DETAILED DESCRIPTION

[0040] The present invention is described in detail below with reference to specific embodiments.

[0041] The long-life light-emitting diode structure includes a transparent conductive substrate, on which an electron transport layer, a perovskite particle layer, a hole transport layer, and an electrode layer are arranged in sequence. The current-voltage-radiation intensity and other characteristics of the diode are tested, and the life of the diode (the time when the external quantum efficiency EQE decays to 95% of the maximum value) T is also tested. 95 .

[0042] Example 1

[0043] Preparation of perovskite precursor solution: FAI, CsI, PbI2, 5-aminovaleric acid (AVA), and trifluoromethoxyphenylethylamine acetic acid (TFPA) were mixed at a molar ratio of 2.2:0.2:1:0.5:0.1, dissolved in a solvent N,N-dimethylformamide (DMF) with a mass fraction of 7wt%, and stirred at room temperature for 12h to obtain a clear yellow perovskite precursor solution. Among them, 5-aminovaleric acid (AVA) and trifluoromethoxyphenylethylamine acetic acid (TFPA) were used as modifiers.

[0044] Trifluoromethoxyphenylethylamine acetic acid (TFPA) was dissolved in chloroform (CHCl3) at a concentration of 0.05 mg / mL to obtain a post-treatment solution, which was stirred at room temperature for 12 h to obtain a clear and transparent post-treatment solution.

[0045] The preparation process of light-emitting diodes is as follows:

[0046] The long-life light-emitting diode structure includes a transparent conductive substrate, an electron transport layer, a perovskite particle layer, a hole transport layer, an electrode layer, and an Au electrode.

[0047] ① The substrate is indium tin oxide (ITO) conductive glass with a film thickness of 20-200nm. The transparent conductive substrate ITO glass is ultrasonically cleaned twice with acetone solution and ethanol solution respectively, and then blown dry with dry nitrogen. The ITO is transferred to an oxygen plasma cleaning machine and cleaned with oxygen plasma under vacuum conditions.

[0048] ② Preparation of electron transport layer: The prepared clear and transparent zinc oxide solution with a concentration of 50-200OD is coated on the treated ITO conductive glass by spin coating, and a dense zinc oxide film is formed after annealing at 150°C for 30 minutes. The charge transport layer has a smooth morphology structure.

[0049] ③ Preparation of perovskite particle layer: In a nitrogen glove box, take the perovskite precursor solution and use a one-step spin coating method at a speed of 4000 rpm for 45 seconds. After spin coating on the charge transport layer, anneal on a hot plate at 110°C for 10 minutes and cool to room temperature to obtain a perovskite film layer. Subsequently, TFPA chloroform solution is deposited on the upper perovskite layer and annealed on a hot plate at 100°C for 3 minutes and cooled to room temperature.

[0050] ④ Preparation of the hole transport layer: Take the hole transport layer solution poly[(9,9-dioctylfluorene-2,7-diyl)-co-(4,4-(N-(4-sec-butylphenyl)diphenylamine)] (TFB) on the perovskite particle layer and spin coat it using a one-step spin coating method at a rotation speed of 2000 rpm for 45 seconds.

[0051] ⑤ Preparation of electrode layer: In a vacuum evaporation chamber, MoO3 and Au are evaporated in sequence, the evaporation rate is controlled below 0.01nm / s, and the thickness is 4.5nm and 100nm respectively.

[0052] The structure of the long-life light-emitting diode in this embodiment is as follows: Figure 1 shown. Figure 2 This is a cross-sectional view of a long-life light-emitting diode. Figure 2 It can be seen from the cross section that the distance between perovskite particles is 50nm. TFB can be spread evenly on the upper layer of perovskite grains, avoiding penetration into the gaps between perovskite particles, forming a suspended "bridge hole" interface structure. This structure avoids the contact between the charge transfer layer and the iodine ions deposited in the gaps, thereby inhibiting the migration of iodine ions. The structural schematic diagram is shown in the figure. Figure 3 shown.

[0053] Figure 4 This is a contact angle experiment of the perovskite film. The contact angle of the film treated with TFPA according to the method of Example 1 is significantly increased, indicating that the surface tension of the perovskite particle layer is significantly reduced, showing hydrophobic and oil-transporting properties, and then forming a "bridge hole" structure with the upper charge transport layer.

[0054] Figure 5 The voltage-current-irradiance curve of the long-life light-emitting diode in Example 1 shows that the irradiance of the light-emitting diode treated by TFPA reaches 600W / sr -1 m -2 . Figure 6 The relationship between the external quantum efficiency (EQE) and current density of the long-lifetime light-emitting diode is shown in the graph. It shows that the EQE of the long-lifetime light-emitting diode processed by TFPA reaches 22.3% at 20 mA cm -2 Under constant current, diode life T 95 Up to 76 hours. Figure 7 ).

[0055] Example 2

[0056] This example is different from Example 1 in that different proportions of p-(trifluoromethyl)benzylamine (CF3PMA) are used for modification. In the perovskite precursor solution, FAI, CsI, PbI2, 5-aminovaleric acid (AVA), p-(trifluoromethyl)benzylamine (CF3PMA) are mixed at a molar ratio of 2.7:0.2:1:0.5:0.06, and the mass fraction is 7wt% dissolved in the solvent N,N-dimethylformamide (DMF). P-(trifluoromethyl)benzylamine (CF3PMA) is dissolved in the solvent chloroform (CHCl3) at a concentration of 0.2mg / mL to obtain a clear and transparent post-treatment solution.

[0057] The remaining steps refer to Example 1.

[0058] Figure 8 This is a cross-sectional view of a long-life light-emitting diode. Figure 8 It can be seen from the cross-section that the distance between perovskite particles is 100nm, and the TFB on the upper layer of the particles can be spread smoothly to avoid penetrating into the gaps between the perovskite particles, forming a suspended "bridge hole"-like interface structure. Fig. 9 Display, at 20mA cm -2 Under constant current, the life of long-life LED is T 95 Reached 69 hours.

[0059] Example 3

[0060] The difference between this example and Example 1 is that tin oxide is used as the electron transport layer coated on the treated ITO conductive glass, and zinc acetate solution is added to the perovskite precursor solution, and the molar ratio of zinc acetate to PbI2 is 1:0.8.

[0061] The method for preparing the light emitting diode is as described in Example 1.

[0062] like Fig.10 As shown in the figure, the distance between perovskite particles is 150nm, and TFB can be spread evenly on the upper layer of the modified perovskite grains, avoiding penetration into the gaps between perovskite particles, forming a suspended "bridge-hole" interface structure. -2 Under constant current, the life of long-life LED is T 95 Reached 79 hours. Fig.11 )

[0063] Example 4

[0064] The difference between this example and Example 1 is that the amount of 5-aminovaleric acid (AVA) additive is reduced, and the molar ratio of 5-aminovaleric acid (AVA) to PbI2 in the perovskite precursor solution is 0.2:1.

[0065] The remaining steps refer to Example 1.

[0066] Fig.12 This is a cross-sectional view of a perovskite light-emitting diode. From the cross-sectional view, it can be seen that the distance between discrete perovskite micro-nano particles is 150nm, forming a suspended "bridge-hole" interface structure with the upper charge transport layer. The perovskite light-emitting diode is 20mA cm -2 Stability at constant current T 95 Up to 30 hours. Fig.13 )

[0067] Example 5

[0068] This example is different from Example 1 in that FAI, CsI, PbI2, and 5-aminovaleric acid (AVA) in the perovskite precursor solution are mixed in a molar ratio of 2.2:0.2:1:0.5, and are dissolved in a solvent N,N-dimethylformamide (DMF) with a mass fraction of 7 wt%. The light-emitting diode preparation method refers to Example 1.

[0069] like Fig.14 As shown in the figure, the spacing between discrete perovskite micro-nano particles is 100 nm, but TFB cannot spread evenly on the modified perovskite grains and penetrate into the gaps between perovskite particles. -2 Under constant current, the lifetime of perovskite light-emitting diode is T 95 0.14 hours ( Fig.15 ).

Claims

1. A long-life perovskite light-emitting diode, characterized in that: The structure of the long-life light-emitting diode includes, from bottom to top, a transparent conductive substrate, an electron transport layer, a perovskite particle layer, a hole transport layer and an electrode layer; wherein the interface morphology between the perovskite particle layer and the hole transport layer is a suspended bridge-hole structure.

2. The long-life perovskite light-emitting diode according to claim 1, characterized in that: The perovskite particle layer is composed of discrete perovskite micro-nano particles, the particle spacing is controllable, and presents a concave-convex wrinkled morphology, which prevents the hole transport layer from sinking to the bottom of the gap between the perovskite micro-nano particles.

3. The long-life perovskite light-emitting diode according to claim 1, characterized in that: The perovskite particle layer is prepared by the following method: a perovskite precursor solution composed of cesium halide, methylamine halide, lead halide, zwitterionic additive and fluorine-containing additive in a molar ratio of 0-1:1-5:1:0.01-5:0.01-0.5 is spin-coated on the electron transport layer by a spin coating method, wherein the mass fraction of the solution is 5%-20%, and the solvent is N,N-dimethylformamide or dimethyl sulfoxide, and then annealed on a heating plate at 90-150°C for 5-20 minutes.

4. The long-life perovskite light-emitting diode according to claim 3, characterized in that: The fluorine-containing additive is a compound composed of one or more of a low polarizability functional group containing fluorine atoms, an aromatic group or an aliphatic group, an ammonium group or an acid group, and is not limited to a perfluorinated compound in which all hydrogen atoms in the carbon chain are replaced by fluorine atoms.

5. The long-life perovskite light-emitting diode according to claim 4, characterized in that: The low polarizability functional group includes one or more of monofluoromethyl, difluoromethyl, trifluoromethyl, trifluoromethoxy, and perfluoroalkyl; the aliphatic functional group includes one or more of a straight chain group and an alicyclic hydrocarbon group; the aromatic functional group includes one or more of a benzene ring, a naphthalene ring, an anthracene ring, an imidazole ring, a benzimidazole ring, a pyridine ring, a quinoline ring, an indole ring, and other condensed rings; the amine or acid group includes one or more of a primary amine group, a secondary amine group, a tertiary amine group, a quaternary amine group, a carboxylic acid group, a carboxylic acid ion group, a sulfonic acid group, and a sulfonate ion group.

6. The long-life perovskite light-emitting diode according to claim 3, characterized in that: The zwitterionic additive is an amino acid molecule.

7. A method for preparing a long-life perovskite light-emitting diode according to claim 1, characterized in that The method comprises the following steps: firstly, spin coating zinc oxide on a transparent conductive substrate to obtain an electron transport layer, then spin coating a perovskite precursor solution composed of cesium halide, methylamine halide, lead halide, zwitterionic additive and fluorine-containing additive in a molar ratio of 0-1:1-5:1:0.01-5:0.01-0.5 on the electron transport layer, wherein the mass fraction of the solution is 5%-20%, and the solvent is N,N-dimethylformamide or dimethyl sulfoxide, then annealing on a heating plate at 90-150°C for 5-20min to obtain a perovskite particle layer, then spin coating or vapor deposition of a hole transport layer on the perovskite particle layer, and finally vapor deposition of an electrode layer on the hole transport layer.

8. The method for preparing a long-life perovskite light-emitting diode according to claim 7, characterized in that The transparent conductive substrate is indium tin oxide conductive glass.

9. The method for preparing a long-life perovskite light-emitting diode according to claim 7, characterized in that The spin coating speed is 1000-4000 rpm, and the time is 10-45 s.

10. The method for preparing a long-life perovskite light-emitting diode according to claim 7, characterized in that The evaporation rate during the deposition of the electrode layer is controlled below 0.01 nm / s.

Citation Information

Patent Citations

  • Preparation method of perovskite film

    CN107302055A

  • Perovskite solar cell modified by fluorinated pyridine molecular additive and preparation method thereof

    CN116113245A