PbS light absorption layer preparation method, PbS quantum dot detector and preparation method

The PbS quantum dot film is deposited layer by layer by layer through liquid ligand exchange method and low vacuum annealing technology, and combined with the electron transport layer to set it on the minimum side of the quantum dot to form a pn junction interface, which solves the low local band light response of the quantum dot photodetector and the problem of spectral unevenness achieves wide spectrum detection and high external quantum efficiency, while reducing dark current density.

CN119072203APending Publication Date: 2024-12-03HUAZHONG UNIV OF SCI & TECH +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311833000.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-12-28
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Existing quantum dot photodetectors have problems with low local band light response and uneven spectral response, and there are limitations on the method of mixing large-size quantum dots into small-size quantum dots and spin-coated films, such as blending coating films. Weakening the peak light response of the original long wave, solvent limits and size gaps are high.

Method used

The liquid-phase ligand exchange method is used to configure a variety of PbS quantum dot solutions with different quantum dot sizes, deposit PbS quantum dot film layer by layer and perform low vacuum annealing to form a multi-layer quantum dot film to achieve energy band gap gradient changes, and combine electrons. The transport layer is arranged to form a pn junction interface on the side with the smallest quantum dot size to reduce defects.

Benefits of technology

Wide spectrum detection is realized, the original long wave peak light response is maintained, the flatness of the spectral response and external quantum efficiency are improved, while the dark current density is reduced, and the detector's design freedom is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119072203A_ABST
    Figure CN119072203A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a PbS light absorption layer, a PbS quantum dot detector and a preparation method. The preparation method of the PbS light absorption layer comprises the following steps: S1, respectively preparing a plurality of PbS quantum dot solutions with different quantum dot sizes by using a liquid-phase ligand exchange method; s2, treating the PbS quantum dot solution to obtain PbS quantum dot slurry; and S3, PbS quantum dot films are deposited on the PbS quantum dot slurry layer by layer according to the quantum dot size gradient change sequence, and low-vacuum-degree annealing treatment is carried out after deposition of each layer of PbS quantum dot film. Compared with a blending coating mode in the prior art, the PbS light absorption layer prepared by the preparation method of the PbS light absorption layer can maintain the light response at the original long wave peak value, the types of solvents used by different light absorption layers PbS do not need to be limited, the requirement for the size difference of quantum dots with different sizes is low, and the preparation method of the PbS light absorption layer is suitable for large-scale popularization and application. And the design freedom degree of the detector is high.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of photoelectric detectors, and in particular to a method for preparing a PbS light-absorbing layer, a PbS quantum dot detector and a preparation method thereof. Background Art

[0002] A photodetector is a device that can capture light signals within a specific wavelength range and convert them immediately into electrical signals. Compared with the photosensitive layer materials of conventional photodetectors on the market, colloidal quantum dots have cheap raw materials, simple processes, and good photoelectric properties, such as high absorption coefficient and adjustable bandgap width, which provide a basis for the rapid application and development of colloidal quantum dot materials in the field of optoelectronics.

[0003] Quantum dot material is a semiconductor nanocrystal with a radius between 1-10nm. When the three-dimensional size of the bulk material continues to shrink to the nm level, the quantum confinement effect will appear, that is, the energy band structure changes from a quasi-continuous state to a discrete energy level, and the band gap will be related to the size of the quantum dot. The smaller the size of the quantum dot, the larger the band gap. Due to the discrete energy level, some photons with energy greater than the band gap width cannot be absorbed, resulting in a decrease in the detection rate of the corresponding band, affecting the application.

[0004] In order to achieve spectral flattening of quantum dot detectors, there is currently a method of mixing small-sized quantum dots into large-sized quantum dot slurry and then spin-coating them into films to improve the flatness of the spectral response, but there are several limiting factors: 1. The mixed slurry coating will weaken the light response at the original long-wave peak; 2. When different quantum dots are blended and coated, the same solvent needs to be shared, which limits the freedom of device design; 3. The size difference between large and small quantum dots cannot be too large during blending, otherwise the photogenerated carriers will be easily confined in narrow-bandgap quantum dots due to the different energy level positions, resulting in a transmission barrier. Summary of the invention

[0005] Based on the above-mentioned problems existing in the prior art, the present invention aims to provide a PbS light absorbing layer preparation method, a PbS quantum dot detector and a preparation method, so as to solve the technical problems in the prior art that the quantum dot photoelectric detector has low light response in the local band, uneven spectral response, and the method of improving the flatness of the spectral response by mixing small-sized quantum dots into a large-sized quantum dot slurry and then spin-coating it into a film.

[0006] The present invention provides a method for preparing a PbS light absorbing layer, which comprises the following steps:

[0007] S1: Use the liquid phase ligand exchange method to prepare a variety of PbS quantum dot solutions with different quantum dot sizes;

[0008] S2: treating the PbS quantum dot solution to obtain a PbS quantum dot slurry;

[0009] S3: depositing a PbS quantum dot film layer by layer from the PbS quantum dot slurry in a quantum dot size gradient order, and performing a low vacuum annealing treatment after each layer of the PbS quantum dot film is deposited.

[0010] According to one embodiment of the present invention, the liquid phase ligand exchange method is used to prepare the PbS quantum dot solution in step S1, including: mixing the PbS quantum dot solution wrapped by the long-chain organic ligand with the short-chain ligand solution to perform ligand exchange to obtain the PbS quantum dot solution wrapped by the short-chain ligand.

[0011] According to one embodiment of the present invention, the short-chain ligand solution is a DMF ligand solution containing PbI2 and PbBr2; and the long-chain organic ligand is an oleic acid ligand.

[0012] According to an embodiment of the present invention, the low vacuum annealing treatment in step S3 includes: performing a primary annealing treatment and then performing a secondary negative pressure annealing treatment.

[0013] According to an embodiment of the present invention, the first annealing temperature is 85-95° C., and the time is 10-20 minutes; the second annealing temperature is 80-90° C., and the time is 1-2 hours.

[0014] The present invention also provides a PbS quantum dot detector, which includes a glass substrate and a bottom electrode, a hole transport layer, a PbS light absorbing layer, an electron transport layer and a top electrode sequentially arranged on the glass substrate;

[0015] The PbS light absorbing layer is arranged on the hole transport layer according to the PbS light absorbing layer preparation method, so that the PbS light absorbing layer includes multiple layers of PbS quantum dot films with gradient quantum dot sizes, and the electron transport layer is arranged on the side of the PbS quantum dot film with the smallest quantum dot size in the PbS light absorbing layer.

[0016] According to an embodiment of the present invention, the PbS light absorption layer includes at least two layers of PbS quantum dot films, and the quantum dot sizes of the two layers of PbS quantum dot films vary in a gradient manner.

[0017] According to one embodiment of the present invention, the hole transport layer comprises NiO x The hole transport layer and the PbS-EDT hole transport layer, the electron transport layer includes a C60 electron transport layer and a SnO2 electron transport layer.

[0018] The present invention also provides a detector preparation method for preparing the PbS quantum dot detector, which comprises the following steps:

[0019] A bottom electrode, a hole transport layer, a PbS light absorbing layer, an electron transport layer and a top electrode are sequentially prepared on a glass substrate; the electron transport layer is prepared on the side of the PbS light absorbing layer where the quantum dots have the smallest size.

[0020] The PbS light absorbing layer, PbS quantum dot detector and preparation method provided by the present invention have the following beneficial effects:

[0021] (1) The method for preparing the PbS light absorbing layer can prepare a PbS light absorbing layer having multiple energy band gaps and a gradient energy band gap, and can realize wide spectrum detection; compared with the method of using a blended coating in the prior art, the PbS light absorbing layer prepared in this scheme can maintain the light response at the original long-wave peak, and there is no need to limit the type of solvent used for different light absorbing layers of PbS, and the size difference requirements for quantum dots of different sizes are relatively low, so that the detector has a higher degree of freedom in design;

[0022] (2) After each layer of PbS quantum dot film is deposited, a low vacuum annealing treatment is performed to reduce the volatilization temperature of the solvent in the layer of PbS quantum dot film, thereby eliminating the residual solvent, so as to avoid the residual solvent from dissolving into the PbS quantum dot film deposited later and destroying the previously deposited PbS quantum dot film, that is, to avoid the film dissolution phenomenon;

[0023] (3) By preparing the electron transport layer on the side of the PbS light absorbing layer where the quantum dots have the smallest size, on the one hand, a pn junction interface is formed between the PbS light absorbing layer and the electron transport layer, and the small-sized quantum dots have a simple exposed crystal surface and are easier to passivate, thereby reducing the defects of the pn junction interface, improving the flatness of the spectral response, and maintaining the external quantum efficiency at a high level; on the other hand, the small-sized quantum dots have a wider energy band gap, while the wide-bandgap quantum dots have a low intrinsic carrier concentration, and the reverse saturation current density of the device is low, which can reduce the dark current density of the detector. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the technical solutions in the embodiments or the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0025] Figure 1 It is a structural schematic diagram of a PbS quantum dot detector provided by the present invention;

[0026] Figure 2 It is a cross-sectional schematic diagram of a PbS quantum dot detector provided by the present invention;

[0027] Figure 3This is a comparison diagram of the wide spectrum EQE of a PbS quantum dot detector provided by the present invention;

[0028] Figure 4 This is a dark current density comparison diagram of a PbS quantum dot detector provided by the present invention. DETAILED DESCRIPTION

[0029] The following descriptions of the embodiments are made with reference to the attached drawings to illustrate specific embodiments in which the present invention may be implemented. The directional terms mentioned in the present invention, such as [up], [down], [front], [back], [left], [right], [inside], [outside], [side], etc., are only with reference to the directions of the attached drawings. Therefore, the directional terms used are used to illustrate and understand the present invention, but not to limit the present invention. In the drawings, units with similar structures are represented by the same reference numerals.

[0030] The present invention provides a method for preparing a PbS light-absorbing layer, which comprises the following steps: S1: using a liquid phase ligand exchange method to respectively configure a plurality of PbS quantum dot solutions with different quantum dot sizes; S2: treating the PbS quantum dot solutions to obtain a PbS quantum dot slurry; S3: depositing a PbS quantum dot film layer by layer on the PbS quantum dot slurry in a gradient change order of quantum dot sizes, and performing a low vacuum annealing treatment on each layer of the PbS quantum dot film after deposition.

[0031] A method for preparing a PbS light absorbing layer provided by the present invention can prepare a PbS light absorbing layer with multiple energy band gaps and a gradient energy band gap, and can realize wide spectrum detection; compared with the method of using a blended coating in the prior art, the PbS light absorbing layer prepared by this scheme can maintain the light response at the original long-wave peak, and there is no need to limit the type of solvent used for different light absorbing layers of PbS, and the size difference requirements for quantum dots of different sizes are relatively low, so that the design freedom of the detector is relatively high; in addition, each layer of PbS quantum dot film in the present invention is subjected to a low vacuum annealing treatment after deposition, which can reduce the volatilization temperature of the solvent in the layer of PbS quantum dot film and thus eliminate the residual solvent, so as to avoid the residual solvent from dissolving into the PbS quantum dot film deposited later and destroying the previously deposited PbS quantum dot film, that is, the film dissolution phenomenon can be avoided.

[0032] According to an embodiment of the present invention, the liquid phase ligand exchange method is used to configure the PbS quantum dot solution in step S1, including: mixing the PbS quantum dot solution wrapped by the long-chain organic ligand with the short-chain ligand solution for ligand exchange to obtain the PbS quantum dot solution wrapped by the short-chain ligand. Specifically, the short-chain ligand solution is a DMF ligand solution containing 0.1229 mg / ml PbI2 and 0.0424 mg / ml PbBr2; the long-chain organic ligand is an oleic acid ligand.

[0033] According to an embodiment of the present invention, the low vacuum annealing treatment in step S3 includes: performing a primary annealing treatment and then performing a secondary negative pressure annealing treatment. Specifically, the first annealing temperature is 85-95°C for 10-20 minutes; the second annealing temperature is 80-90°C for 1-2 hours, and the vacuum is maintained during the heating process.

[0034] The present invention also provides a PbS quantum dot detector, the structure of which is as follows Figure 1 and Figure 2 As shown, it includes a glass substrate and a bottom electrode, a hole transport layer PbS light absorbing layer, an electron transport layer and a top electrode sequentially arranged on the glass substrate;

[0035] The PbS light absorbing layer is arranged on the hole transport layer according to the PbS light absorbing layer preparation method, so that the PbS light absorbing layer includes multiple layers of PbS quantum dot films with gradient quantum dot sizes, and the electron transport layer is arranged on the side of the PbS quantum dot film with the smallest quantum dot size in the PbS light absorbing layer.

[0036] The present invention also provides a detector preparation method for preparing the PbS quantum dot detector, which comprises the following steps:

[0037] A bottom electrode, a hole transport layer, the PbS light absorbing layer, an electron transport layer and a top electrode are sequentially prepared on a glass substrate; the electron transport layer is prepared on the side of the PbS light absorbing layer where the quantum dots have the smallest size.

[0038] Compared with the prior art, in a PbS quantum dot detector prepared by a detector preparation method provided by the present invention, by preparing the electron transport layer on the side of the PbS light absorbing layer with the smallest quantum dot size, on the one hand, a pn junction interface is formed between the PbS light absorbing layer and the electron transport layer, and the small-sized quantum dots have a simple crystal surface exposure and are easier to passivate, thereby reducing pn junction interface defects, improving the flatness of the spectral response, and maintaining the external quantum efficiency at a high level; on the other hand, the energy band gap of small-sized quantum dots is wider, and the intrinsic carrier concentration of wide-bandgap quantum dots is low, the reverse saturation current density of the device is low, and the dark current density of the detector can be reduced.

[0039] Specifically, the detector preparation method in the embodiment of the present invention specifically includes the following steps:

[0040] Preparation of NiO x Hole transport layer: magnetron sputtering coating technology is used, with a sputtering power of 200W, a sputtering pressure of 2Pa, and a sputtering time of 5min. A 1% Li-doped nickel oxide target is used to sputter 10-50nm thick NiO on the ITO glass substrate. x ;

[0041] Preparation of PbS-EDT hole transport layer: x The hole transport layer is spin-coated with a PbS quantum dot solution with an absorption peak of 880 nm dissolved in n-octane at a concentration of 40 mg / ml, and then spin-coated with an EDT solution dissolved in acetonitrile at a concentration of 0.01% to 0.05%, and allowed to stand for 20-60 seconds for solid phase exchange, and then spin-coated and washed twice with acetonitrile for use;

[0042] Preparation of PbS light-absorbing layer: (1) Prepare a variety of PbS quantum dot solutions with different quantum dot sizes: Prepare DMF ligand solutions containing 0.1229 mg / ml PbI2 and 0.0424 mg / ml PbBr2 in a nitrogen atmosphere glove box, dissolve oleic acid ligand PbS quantum dots with absorption peaks of 1550 nm, 1440 nm, and 1300 nm in n-octane, and exchange ligands with the three quantum dot solutions and the ligand solution respectively to prepare three quantum dot solutions with a concentration of 10 mg / ml each.

[0043] (2) Treat the PbS quantum dot solution to obtain a PbS quantum dot slurry; mix the quantum dot solution and the ligand solution in a volume ratio of 1:1 and shake vigorously. After static stratification, remove the upper colorless liquid, divide the lower black liquid into portions and centrifuge at a speed of 9000r / min for 5min, pour out the separated liquid, and then dry the quantum dot precipitate, vacuumize, and dry for 1h for later use. Prepare a dispersant with a volume ratio of DMF:DMSO:BTA:3-pyridinemethylamine = 35:25:37:3, dissolve the quantum dots at a concentration of 400mg / ml, and obtain three quantum dot slurries.

[0044] (3) Spin-coating the PbS quantum dot slurry on the PbS-EDT hole transport layer in descending order of quantum dot size, and drying each layer after spin coating: first, spin-coat the PbS quantum dot slurry with an absorption peak of 1550 nm on the PbS-EDT substrate, anneal at 90° C. for 10 min, then anneal the film at 85° C. under negative pressure for 1 h, and keep vacuuming with a mechanical pump during the heating process. Spin-coat the film after negative pressure annealing with PbS quantum dots with an absorption peak of 1440 nm at a concentration of 400 mg / ml, repeat the above operation, and then spin-coat PbS quantum dots with an absorption peak of 1300 nm at a concentration of 400 mg / ml, and anneal at 90° C. for 10 min. It should be noted that preparing the PbS quantum dot film on the PbS-EDT hole transport layer by spin coating is only a preferred embodiment of the present invention. In other embodiments, other methods may be used instead of spin coating, such as solution epitaxy, spray coating, etc.

[0045] Preparation C 60Electron transport layer: Using thermal evaporation, evaporate 8-20nm thick C on the side with the smallest quantum dot size in the PbS light absorption layer. 60 ;

[0046] Preparation of SnO2 electron transport layer: Atomic layer deposition was used in the C 60 SnO2 with a thickness of 20 to 60 nm is grown on the surface of the electron transport layer;

[0047] Preparation of ITO top electrode: Using magnetron sputtering, sputter ITO with a thickness of 200 to 300 nm on the surface of the SnO2 electron transport layer.

[0048] like Figure 3 The figure shows a comparison of the wide-spectrum EQE of the PbS quantum dot detector provided by the present invention and the PbS quantum dot standard detector with an absorption peak of 1550nm. It is not difficult to see from the figure that in the wide-spectrum EQE of the PbS quantum dot standard detector with an absorption peak of 1550nm, there is a strong light response in the 1550nm band, but in the short-wave direction, around 1450nm, the light response drops sharply, and the light response in the 900-1500nm band is relatively low. In the wide-spectrum EQE of the detector prepared by the preparation method of the PbS quantum dot wide-spectrum high external quantum efficiency detector of the present invention, the light response in the 1550 band increases slightly, the light response in the 900-1500nm band increases significantly, and the red line of the spectral response in the infrared band is flatter than the black line.

[0049] like Figure 4 The figure shows a comparison of the dark current density of the PbS quantum dot detector provided by the present invention and the PbS quantum dot standard detector with an absorption peak of 1550nm. It is not difficult to see from the figure that with the increase of the reverse bias voltage, the dark current density of the PbS quantum dot standard detector with an absorption peak of 1550nm becomes significantly larger. As the reverse bias voltage increases, the bending degree of the PN junction energy band increases, and more interface defects will greatly increase the trap-assisted tunneling current. The detector prepared by the preparation method of the PbS quantum dot wide spectrum high external quantum efficiency detector provided by the present invention has a significantly slower increase in dark current with the increase of reverse bias voltage. This can be attributed to the small-sized quantum dots contacting the N-type layer to form a PN junction, which has a lower defect concentration.

[0050] In summary, in a PbS quantum dot detector provided by the present invention, since a pn junction interface is formed between the PbS light absorbing layer and the electron transport layer, by arranging the electron transport layer on the side of the PbS light absorbing layer where the quantum dots have the smallest size, the pn junction interface defects can be reduced, the flatness of the spectral response can be improved, and the external quantum efficiency can be maintained at a high level; and since the energy band gap of small-sized quantum dots is wider and the intrinsic carrier concentration of wide-bandgap quantum dots is low, the reverse saturation current density of the device is low, which can reduce the dark current density of the detector.

[0051] It should be noted that although the present invention is disclosed as above by specific embodiments, the above embodiments are not intended to limit the present invention. Ordinary technicians in this field can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention shall be based on the scope defined in the claims.

Claims

1. A method for preparing a PbS light absorbing layer, characterized in that: It includes the following steps: S1: Use the liquid phase ligand exchange method to prepare a variety of PbS quantum dot solutions with different quantum dot sizes; S2: treating the PbS quantum dot solution to obtain a PbS quantum dot slurry; S3: depositing a PbS quantum dot film layer by layer from the PbS quantum dot slurry in a quantum dot size gradient order, and performing a low vacuum annealing treatment after each layer of the PbS quantum dot film is deposited.

2. The method for preparing a PbS light absorbing layer according to claim 1, characterized in that: In step S1, the liquid phase ligand exchange method is used to prepare the PbS quantum dot solution, which includes: mixing the PbS quantum dot solution wrapped by the long-chain organic ligand with the short-chain ligand solution to perform ligand exchange to obtain the PbS quantum dot solution wrapped by the short-chain ligand.

3. The method for preparing a PbS light absorbing layer according to claim 2, characterized in that: The short-chain ligand solution is a DMF ligand solution containing PbI2 and PbBr2; and the long-chain organic ligand is an oleic acid ligand.

4. The method for preparing a PbS light absorbing layer according to claim 1, characterized in that: The low vacuum annealing treatment in step S3 includes: performing a primary annealing treatment and then performing a secondary negative pressure annealing treatment.

5. The method for preparing a PbS light absorbing layer according to claim 4, characterized in that: The first annealing temperature is 85-95°C and the time is 10-20 minutes; the second annealing temperature is 80-90°C and the time is 1-2 hours.

6. A PbS quantum dot detector, characterized in that: It comprises a glass substrate and a bottom electrode, a hole transport layer, a PbS light absorption layer, an electron transport layer and a top electrode arranged in sequence on the glass substrate; The PbS light absorbing layer is arranged on the hole transport layer according to the PbS light absorbing layer preparation method according to any one of claims 1 to 5, so that the PbS light absorbing layer includes multiple layers of PbS quantum dot films with gradient quantum dot sizes, and the electron transport layer is arranged on the side of the PbS quantum dot film with the smallest quantum dot size in the PbS light absorbing layer.

7. The PbS quantum dot detector according to claim 6, characterized in that: The PbS light absorption layer includes at least two layers of PbS quantum dot films, and the quantum dot sizes of the multiple layers of the PbS quantum dot films vary in a gradient manner.

8. The PbS quantum dot detector according to claim 6, characterized in that: The hole transport layer includes NiO x The hole transport layer and the PbS-EDT hole transport layer, the electron transport layer includes a C60 electron transport layer and a SnO2 electron transport layer.

9. A detector preparation method for preparing the PbS quantum dot detector according to any one of claims 6 to 8, characterized in that: It includes the following steps: A bottom electrode, a hole transport layer, the PbS light absorbing layer, an electron transport layer and a top electrode are sequentially prepared on a glass substrate; the electron transport layer is prepared on the side of the PbS light absorbing layer where the quantum dots have the smallest size.