Polyolefin, plasticizer for electronic materials, base for cosmetics, cosmetics, and lubricant

By controlling the number average molecular weight and side chain ratio of the polyolefin, a new type of polyolefin is formed, which solves the problems of plasticization, water dispersion and lubricity reduction after temperature cycling, and achieves stable performance in a wide temperature range.

CN119072503APending Publication Date: 2024-12-03NOF CORP
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202380033362.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-13
Filing Date
2023-04-06
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

After the temperature cycling of existing polyolefins during use in winter, the plasticization of the plasticizer for electronic materials decreases, the percutaneous water dispersion loss inhibition effect and crystallization stability of the cosmetic matrix are poor, and the lubricity of the lubricating oil decreases.

Method used

The linear olefin monomer with a number average molecular weight of 250 to 10,000 and a number of 8 to 20 carbon atoms is used to polymerize the Lewis acid catalyst to control the side chain ratio of 1 to 40% of carbon atoms or less to form New polyolefins for electronic materials, cosmetics and lubricants.

Benefits of technology

Within the temperature range of -20℃~90℃, the plasticization of electronic material plasticizers, the percutaneous water dispersion loss inhibition effect and crystallization stability of cosmetics, and the lubricating properties of lubricants avoid stickiness and lubricity. reduce.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005077296000000171
    Figure BDA0005077296000000171
  • Figure BDA0005077296000000191
    Figure BDA0005077296000000191
  • Figure BDA0005077296000000221
    Figure BDA0005077296000000221
Patent Text Reader

Abstract

Provided is a polyolefin which is obtained from a linear olefin monomer having 8-20 carbon atoms, has a number average molecular weight of 250-10,000, and has a side chain rate of n-3 or less carbon atoms of 1-40% as calculated by formula (1): side chain rate (%) of n-3 or less carbon atoms = [Nx / (Nx + Ny) * 2n-3] / 3 * 100, the symbols in formula (1) being defined as in the description.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a novel polyolefin which can be effectively used in various applications such as a plasticizer for electronic materials and a base for cosmetics. The present invention also provides a plasticizer for electronic materials, a base for cosmetics, a cosmetic containing the base for cosmetics, and a lubricant. Background Art

[0002] Polyolefin refers to a polymer with olefins represented by ethylene or propylene as monomers. Polyolefin is a polymer composed only of C / H atoms and has no unsaturated bonds. It is characterized by low density and low polarity, as well as high water resistance and chemical resistance. Therefore, polyolefin is used in various applications such as lubricants, plasticizers for electronic materials, and bases for cosmetics.

[0003] Lubricants are used to reduce friction between mechanical components acting on machinery. In recent years, the environment in which lubricants are used has become more severe. On the other hand, in consideration of environmental issues, there is a trend to seek longer life, and the demand for polyalphaolefin (PAO) synthetic lubricants with excellent low-temperature viscosity characteristics and heat resistance / oxidation stability is increasing. However, from the perspective of reducing fuel consumption / energy saving, further improvements in viscosity index and low-temperature viscosity characteristics are required.

[0004] For example, Patent Document 1 discloses an α-olefin polymer and a synthetic lubricating oil composed of the same, wherein the α-olefin polymer contains a constituent unit derived from an α-olefin having 8 to 20 carbon atoms in a range of 50 to 100 mol % and has a number average molecular weight (Mn) of 500 to 15,000. Patent Document 1 discloses that the synthetic lubricating oil exhibits excellent viscosity index and low-temperature viscosity characteristics.

[0005] For example, Patent Document 2 discloses an α-olefin polymer and a synthetic lubricant oil composed of the same, wherein the α-olefin polymer contains a constituent unit derived from an α-olefin having 8 to 20 carbon atoms in a range of 90 to 100 mol % and has a number average molecular weight (Mn) of 500 to 15,000. Patent Document 2 discloses that the synthetic lubricant exhibits excellent viscosity index and low temperature viscosity characteristics.

[0006] In the field of information electronics, electronic components adapted to 5G communications and display components adapted to flexibility have been developed in recent years. In order to suppress the low delay caused by transmission loss or adapt to use in high temperature environments, polyolefin resins or additives are used as materials with low dielectric constants or low dielectric loss tangents, excellent heat resistance or strain resistance in these electronic components.

[0007] For example, Patent Document 3 discloses that a polyolefin resin such as a polyisobutylene resin or a propylene-butene copolymer containing a maleic anhydride group is used in a sealing resin composition for suppressing degassing due to thermal degradation. In addition, Patent Document 3 discloses that a liquid poly-α-olefin having a weight average molecular weight of 500 to 5000 is used as a plasticizer from the viewpoint of adhesiveness.

[0008] For example, Patent Document 4 discloses a PSA sheet having a PSA composition layer containing an isobutylene polymer and an ethylene-α-olefin oligomer as a plasticizer, and the PSA sheet has excellent adhesiveness, responsiveness to strain, and recovery properties.

[0009] In the field of cosmetics, in order to prevent water from being lost from the skin, liquid paraffin, ester oil, wax, grease, and higher alcohols were mostly used in the past. Generally, the higher the molecular weight of the cosmetic base, the more effective it is in preventing water from being lost. However, if a high molecular weight cosmetic base is used, it tends to cause stickiness. In recent years, consumers require a sense of use with a high-end feel, and require a cosmetic base that can create a sense of use with a high-end feel. The sense of high-end means that although there is a strong sense of thickness when applied, there is no stickiness, and there is a sense of melting on the skin.

[0010] In recent years, emulsified cosmetics or oily solid cosmetics blended with a large amount of wax, oil, or higher alcohol that is solid at room temperature have become popular from the viewpoint of improving the touch or enhancing the moisturizing effect. However, such cosmetics have the problem of poor stability due to crystallization of the components under low or high temperature conditions.

[0011] For example, Patent Document 5 discloses a cosmetic composition comprising at least one branched oligo-α-olefin characterized in that the side chain at the branch point is an ethyl group, a propyl group, or a longer branched alkyl chain. The cosmetic composition is not sticky and has a good smooth feel when applied to the skin.

[0012] For example, Patent Document 6 discloses a water-in-oil type cosmetic, characterized in that it contains an α-olefin oligomer having a weight average molecular weight of 5,000 to 60,000 and a viscosity value of 1,000 cp to 40,000 cp at 40° C. and a polyoxyalkylene-modified organic polysiloxane with an HLB of 2 to 8 and / or a polyoxyalkylene-modified organic polysiloxane containing a long-chain alkyl group. The water-in-oil type cosmetic spreads well on the skin, has excellent adhesion to the skin, and has a high moisturizing effect.

[0013] Prior art literature

[0014] Patent Literature

[0015] Patent Document 1: Japanese Patent Application Publication No. 2005-200446;

[0016] Patent document 2: Japanese Patent Application Publication No. 2006-176760;

[0017] Patent Document 3: Japanese Patent Application Publication No. 2017-27941;

[0018] Patent document 4: Japanese Patent Application Publication No. 2021-54980;

[0019] Patent Document 5: Japanese Patent Application No. 2006-523635;

[0020] Patent document 6: Japanese Patent Application Publication No. 2001-72533. Summary of the invention

[0021] Problems to be solved by the invention

[0022] Conventional polyolefins blended with additives for plasticizers for electronic materials may have their plasticizing properties reduced by precipitation of the additives after being subjected to temperature cycles of -20°C to 90°C, which is assumed for use in winter.

[0023] Furthermore, although various attempts have been made to improve the feel of cosmetics during use, conventional polyolefins used as bases for cosmetics may not fully satisfy the effects of suppressing transepidermal water loss, eliminating stickiness, and suppressing crystallization.

[0024] Furthermore, cosmetics containing conventional polyolefins as a cosmetic base and containing a large amount of ingredients that are solid at room temperature (e.g., waxes, oils, higher alcohols, etc.) may have their ingredients crystallized and their stability deteriorated under severe conditions such as a temperature cycle of -20°C to 50°C, which is assumed to be a bathroom temperature in winter. In addition, if it is desired to give the above cosmetics a thick feeling, a sticky feeling may occur or the melting feeling on the skin may be reduced.

[0025] Furthermore, conventional polyolefins blended with additives for lubricating oils may have reduced lubricity after being subjected to a temperature cycle of -20°C to 90°C, which is assumed for use in winter.

[0026] An object of the present invention is to provide a polyolefin which can be used as a plasticizer capable of suppressing the precipitation of an additive blended in a plasticizer for electronic materials even after a temperature cycle of -20°C to 90°C assumed for use in winter.

[0027] Another object of the present invention is to provide a polyolefin which can be used as a cosmetic base having excellent transepidermal water loss suppressing effect and crystallization suppressing effect and having less stickiness.

[0028] Furthermore, the present invention aims to provide a cosmetic which, even if containing a large amount of ingredients that are solid at room temperature (e.g., waxes, oils, and higher alcohols), has excellent stability under temperature cycle conditions of -20°C to 50°C, a thick texture, and a melting feeling on the skin, and has little stickiness.

[0029] Another object of the present invention is to provide a polyolefin that can be used as a lubricant that exhibits excellent lubricity even after a temperature cycle of -20°C to 90°C assumed for use in winter.

[0030] Means for solving problems

[0031] The present inventors have conducted intensive studies in view of the above circumstances and have found that a novel polyolefin having a number average molecular weight and a side chain ratio of carbon atoms of n-3 or less within a specific range can solve the above problems. The present invention based on this finding is as follows.

[0032] [1] A polyolefin obtained from a linear olefin monomer having 8 to 20 carbon atoms and having a number average molecular weight of 250 to 10,000,

[0033] The side chain ratio of carbon atoms of n-3 or less calculated by formula (1) is 1 to 40%. The side chain ratio of carbon atoms of n-3 or less (%) = [Nx / (Nx+Ny)×2n-3] / 3×100···(1)

[0034] In formula (1),

[0035] n represents the average carbon number of the above olefin monomers,

[0036] Nx represents the 1 The integrated value of the signal at 0.75 to 0.95 ppm detected in the H-NMR measurement, and

[0037] Ny represents 1 The integrated value of the signal at 1.00 to 1.45 ppm detected in H-NMR measurement.

[0038] [1a] The polyolefin according to [1] above, wherein the linear olefin monomer having 8 to 20 carbon atoms is at least one selected from 1-decene, 1-dodecene and 1-tetradecene, more preferably 1-decene and / or 1-dodecene, and even more preferably 1-decene.

[0039] [1b] The polyolefin according to [1] or [1a] above, wherein the number average molecular weight is 300 to 5,000, more preferably 400 to 2,500, and even more preferably 400 to 1,800.

[0040] [1c] The polyolefin described in any one of [1] to [1b] above, wherein the ratio of side chains having a carbon number of n-3 or less is 1 to 30%, more preferably 1 to 20%, and even more preferably 5 to 20%.

[0041] [2] The method for producing a polyolefin according to any one of [1] to [1c] above, comprising polymerizing a linear olefin monomer having 8 to 20 carbon atoms in the presence of a Lewis acid catalyst.

[0042] [2a] The method according to [2] above, wherein the supply rate of the olefin monomer is switched at a time point when 35 to 75% by mass, more preferably 40 to 75% by mass, and even more preferably 50 to 75% by mass of the olefin monomer is supplied relative to the total supply amount of the olefin monomer; and

[0043] When the supply rate of the olefin monomer before switching is V1 and the supply rate of the olefin monomer after switching is V2, V1 / V2 is 0.1 or more and less than 1.0, more preferably 0.1 or more and less than 0.75, further preferably 0.1 or more and less than 0.6, and particularly preferably 0.5.

[0044] [2b] The method according to [2] or [2a], wherein the reaction temperature is increased by 1 to 20°C, more preferably 1 to 15°C, and even more preferably 1 to 10°C, at the time when 35 to 75% by mass of the olefin monomer is supplied relative to the total amount of the olefin monomer supplied.

[0045] [3] A plasticizer for electronic materials, comprising the polyolefin described in any one of [1] to [1c] above.

[0046] [3a] Use of the polyolefin according to any one of [1] to [1c] as a plasticizer for electronic materials.

[0047] [4] A cosmetic base comprising the polyolefin described in any one of [1] to [1c] above.

[0048] [4a] Use of the polyolefin described in any one of [1] to [1c] as a base for cosmetics.

[0049] [5] A cosmetic comprising the cosmetic base described in [4] above in an amount of 1 to 80% by mass based on the total mass of the cosmetic.

[0050] [6] A lubricant comprising the polyolefin described in any one of [1] to [1c] above.

[0051] [6a] Use of the polyolefin according to any one of [1] to [1c] above as a lubricant.

[0052] Effects of the Invention

[0053] According to the present invention, a polyolefin can be obtained which can be used as a plasticizer capable of suppressing the precipitation of an additive blended in a plasticizer for electronic materials even after a temperature cycle of -20°C to 90°C assumed for use in winter.

[0054] Furthermore, according to the present invention, a polyolefin can be obtained which can be used as a cosmetic base having excellent transepidermal water loss suppressing effect and crystallization suppressing effect and having less stickiness.

[0055] Furthermore, according to the present invention, a cosmetic can be obtained which, even if it contains a large amount of ingredients that are solid at room temperature (for example, waxes, oils, and higher alcohols), has excellent stability under temperature cycle conditions of -20°C to 50°C, a thick feeling, and a melting feeling on the skin, and has little stickiness.

[0056] Furthermore, according to the present invention, a polyolefin can be obtained which can be used as a lubricant showing excellent lubricity even after a temperature cycle of -20°C to 90°C assumed for use in winter. DETAILED DESCRIPTION

[0057] The various records in this specification can be combined with each other except for the cases where they are clearly not combined. In addition, the numerical range specified by the symbol "to" in this specification includes the numerical values ​​at both ends (upper and lower limits) of the "to". For example, "2 to 5" means more than 2 and less than 5.

[0058] (Polyolefin)

[0059] The polyolefin of the present invention is a polyolefin obtained from a linear olefin monomer having 8 to 20 carbon atoms. The above-mentioned olefin monomer may be used alone or in combination of two or more. Examples of the above-mentioned olefin monomer include 1-octene, 1-nonene, 1-decene, 2-decene, 3-decene, 4-decene, 5-decene, 1-undecene, 1-dodecene, 1-tridecene, 1-tetradecene, 1-pentadecene, 1-hexadecene, butadiene, and the like. The number of carbon atoms of the above-mentioned olefin monomer is preferably 8 to 16, more preferably 10 to 15, further preferably 10 to 12, and particularly preferably 10.

[0060] The ratio of the α-olefin in the olefin monomer is not particularly limited, but is preferably 70 to 100% by mass, and more preferably 80 to 100% by mass.

[0061] The olefin monomer is preferably at least one selected from 1-decene, 1-dodecene and 1-tetradecene, more preferably 1-decene and / or 1-dodecene, and further preferably 1-decene.

[0062] The number average molecular weight (Mn) of the polyolefin of the present invention is obtained from a chromatogram obtained by using a differential refractometer in gel permeation chromatography (GPC) using polystyrene as a standard and tetrahydrofuran as a developing solvent, i.e., a graph showing the relationship between the refractive index intensity and the elution time. The number average molecular weight of the polyolefin of the present invention is 250 to 10,000, preferably 300 to 5,000, more preferably 400 to 2,500, and even more preferably 400 to 1,800. When the number average molecular weight of the polyolefin is less than 250, the effect of the polyolefin in suppressing the crystallization of the additive (hereinafter sometimes described as "crystallization suppression effect") and the rich thickness of the obtained cosmetic are reduced. When the number average molecular weight exceeds 10,000, the handleability of the polyolefin is deteriorated, and the obtained cosmetic has a sticky feeling, which is not preferred.

[0063] One of the characteristics of the polyolefin of the present invention is that the side chain rate of carbon atoms of n-3 or less is 1 to 40%. Here, "n" refers to the average carbon number of the above-mentioned olefin monomer (that is, the arithmetic mean of the carbon number of the above-mentioned olefin monomer), and the "side chain rate of carbon atoms of n-3 or less" refers to the ratio (%) of the number of side chains of carbon atoms of n-3 or less to the total number of side chains in the polyolefin (=100×the number of side chains of carbon atoms of n-3 or less / the total number of side chains). For example, when n is 10, the "side chain rate of carbon atoms of n-3 or less" refers to the "side chain rate of carbon atoms of 7 or less".

[0064] The side chain ratio of polyolefins with carbon atoms of n-3 or less is calculated by formula (1):

[0065] Side chain ratio with carbon number of n-3 or less (%) = [Nx / (Nx+Ny)×2n-3] / 3×100···(1)

[0066] In formula (1),

[0067] n represents the average carbon number of the above olefin monomers,

[0068] Nx represents the 1 The integrated value of the signal at 0.75 to 0.95 ppm detected in the H-NMR measurement, and

[0069] Ny represents 1 The integrated value of the signal at 1.00 to 1.45 ppm detected in H-NMR measurement.

[0070] The side chain ratio of polyolefins with carbon atoms of n-3 or less can be calculated, for example, by the following procedure. Specifically, a 600 Hz NMR measuring apparatus (JNM-ECA600) manufactured by JEOL Ltd. is used to load a mixed solution of analysis sample: deuterated chloroform = 1:45 (mass ratio) into an NMR sample tube with an inner diameter of 5 mm, and a measurement sample is prepared. 1 H-NMR measurement was performed under the conditions of a relaxation delay time of 5 seconds and a free induction decay collection time of 1.8 seconds. 1 In the H-NMR spectrum, the signal of trimethylsilane (TMS) is taken as 0 ppm, and the integral value (Nx) of the signal of 0.75 to 0.95 ppm and the integral value (Ny) of the signal of 1.00 to 1.45 ppm are calculated. It should be noted that Nx is the integral value of the signal of CH3, and Ny is the integral value of the signal of CH2 and CH. In the case where the polyolefin has a side chain with a carbon number of n-3 or less, the proton from the terminal methyl group in the constituent unit of the polyolefin increases by 3 compared to the case where this is not the case. Therefore, the side chain rate with a carbon number of n-3 or less can be calculated by the above formula (1) using the obtained Nx and Ny and the average carbon number (n) of the linear olefin monomer.

[0071] When the ratio of side chains with carbon numbers of n-3 or less is less than 1%, the crystallization inhibition effect is reduced. In addition, even if the ratio of side chains with carbon numbers of n-3 or less exceeds 40%, the crystallization inhibition effect is reduced, and the melting feeling of the obtained cosmetics on the skin is reduced. The ratio of side chains with carbon numbers of n-3 or less is preferably 1 to 30%, more preferably 1 to 20%, and further preferably 5 to 20%.

[0072] (Production method of polyolefin)

[0073] The polyolefin of the present invention is preferably obtained by a production method comprising polymerizing a linear olefin monomer having 8 to 20 carbon atoms in the presence of a Lewis acid catalyst. The above-mentioned polymerization can be carried out using an organic solvent or in the absence of a solvent. Specifically, the polyolefin of the present invention can be obtained by a production method comprising the following steps: an initiator and an organic solvent based on needs are loaded into a reaction vessel, followed by supplying a Lewis acid catalyst, preferably under an inert gas atmosphere while stirring a mixture of an organic solvent, an initiator and a Lewis acid catalyst, while continuously or intermittently adding the above-mentioned olefin monomer to carry out addition polymerization. The olefin monomer can be added under pressure or under atmospheric pressure.

[0074] It is further preferred to switch the supply rate of the olefin monomer at a time point when 35 to 75% by mass, more preferably 40 to 75% by mass, and more preferably 50 to 75% by mass of the olefin monomer is supplied relative to the total supply amount of the olefin monomer. When the supply rate (supply amount per unit time) of the olefin monomer before the switch is V1 and the supply rate of the olefin monomer after the switch is V2, V1 / V2 is preferably 0.1 or more and less than 1.0, more preferably 0.1 or more and less than 0.75, further preferably 0.1 or more and less than 0.6, and particularly preferably 0.5.

[0075] The reaction temperature during the polyolefin polymerization is, for example, -10°C to 100°C, preferably -10°C to 50°C, and more preferably -10°C to 30°C.

[0076] It is desirable that the reaction temperature be raised by preferably 1 to 20°C, more preferably 1 to 15°C, and even more preferably 1 to 10°C when 35 to 75% by mass of the olefin monomer is supplied relative to the total amount of the olefin monomer supplied.

[0077] The reaction pressure during the polyolefin polymerization is not particularly limited, but is, for example, 0 to 2.0 MPa, and preferably 0.1 to 1.0 MPa.

[0078] Lewis acid catalysts for the polymerization of olefin monomers include, for example, metal halides or organometallic halides such as SnCl4, TiCl4, TiCl3, TiBr4, TiBr3, VCl5, FeCl3, ZrCl3, ZrCl4, ZnBr2, BF3, BCl3, and AlCl3. From the viewpoint of reactivity, preferred Lewis acid catalysts are aluminum compounds, and more preferably AlCl3. It should be noted that the "metal" in the above-mentioned "metal halide or organometallic halide" also includes "semimetal".

[0079] The amount of the Lewis acid catalyst relative to the olefin monomer (ie, 100×the amount of Lewis acid catalyst used (mol) / the amount of olefin monomer used (mol)) is, for example, 0.01 to 10 mol%, preferably 0.01 to 5 mol%, and more preferably 0.1 to 5 mol%.

[0080] As the initiator used for the polymerization of the olefin monomer, for example, water, alcohols, etc. are mentioned, and water is preferably used. The amount of the initiator relative to the Lewis acid catalyst (i.e., 100×the amount of the initiator used (mol) / the amount of the Lewis acid catalyst used (mol)) is, for example, 0.01 to 200 mol%, preferably 1 to 200 mol%, more preferably 10 to 150 mol%, and further preferably 10 to 100 mol%.

[0081] As organic solvents for the polymerization of olefin monomers, for example, hydrocarbons such as hexane, heptane, octane, decane, and liquid paraffin; aromatic hydrocarbons such as toluene and xylene; amides such as dimethyl sulfoxide, N,N-dimethylformamide, dimethylacetamide, and acetanilide; ketones such as acetone, butanone, methyl isobutyl ketone, and cyclohexanone; halogenated hydrocarbons such as dichloroethane and dichloromethane; acetates such as methyl acetate, ethyl acetate, propyl acetate, butyl acetate, and methyl butyrate. These can be used alone or in combination of two or more. From the viewpoint of reactivity, the dielectric constant of the organic solvent at 25°C is preferably 1 to 50, more preferably 1 to 30, further preferably 1 to 10, and particularly preferably 1 to 5. It should be noted that the dielectric constant of the organic solvent at 25°C can be measured using a liquid dielectric constant meter 871 (manufactured by Rufuto Co., Ltd., Japan).

[0082] The amount of the organic solvent relative to the olefin monomer (ie, 100×the amount of organic solvent used (g) / the amount of olefin monomer used (g)) is preferably 50 to 10,000 mass %, more preferably 50 to 500 mass %, and further preferably 50 to 200 mass %.

[0083] It is necessary to add a deactivating agent to the reaction solution taken out from the reactor to deactivate the Lewis acid catalyst. As the deactivating agent, for example, water, alcohols, ethers, amines, acetonitrile, ammonia, sodium hydroxide aqueous solution, potassium hydroxide aqueous solution, etc. can be used, and among these, water or sodium hydroxide aqueous solution can be preferably used.

[0084] (Lubricant)

[0085] The polyolefin of the present invention is preferably used as a lubricant. Therefore, the present invention also provides: a lubricant composed of the polyolefin of the present invention. It should be noted that the use of the lubricant composed of the polyolefin of the present invention is not particularly limited, and the lubricant can be suitably used as, for example, gear oil, engine oil (engine oil), industrial lubricant, working oil, and grease.

[0086] The lubricant composed of the polyolefin of the present invention can be used in combination with other base oils and lubricant additives. Examples of other base oils include mineral oils and synthetic oils. Examples of mineral oils include hydrogenated purified oils and paraffin-based mineral oils. Examples of synthetic oils include oils synthesized by Fischer-Tropsch reaction using methane and other gases as raw materials, poly-α-olefin oligomers, polybutene, alkylbenzenes, monoesters, polyol esters, polyethylene glycol esters, polyethylene propylene, hindered esters, dibasic acid esters, and the like.

[0087] Examples of lubricant additives include antioxidants, oiliness improvers, anti-wear agents, extreme pressure agents, metal deactivators, defoamers, rust inhibitors, pour point depressants, viscosity index improvers, anti-hydrolysis agents, and the like. Examples of antioxidants include zinc dialkyl dithiophosphates, organic sulfur compounds, hindered phenols, and aromatic amines. Examples of oiliness improvers include higher fatty acids (e.g., fatty acids having 13 to 21 carbon atoms), fatty acid esters, higher alcohols, and alkylamines. Examples of anti-wear agents include phosphate esters. Examples of extreme pressure agents include organic sulfur, phosphorus compounds, and organic halogen compounds. Examples of metal deactivators include benzotriazole, N,N'-disalicylidene-1,2-diaminopropane, and the like. Examples of defoamers include polymethylsiloxanes, organic fluorine compounds, metal soaps, fatty acid esters, phosphoric acid esters, higher alcohols, and polyalkylene glycol compounds. The lubricant additive is preferably an oiliness improver, more preferably a higher fatty acid, and still more preferably a fatty acid having 13 to 21 carbon atoms.

[0088] When the lubricant of the present invention is used as a motor oil, the precipitation of the lubricant additive can be suppressed, so that good lubrication performance can be exhibited even after temperature cycling at -20°C to 90°C. That is, the lubricant composition containing the lubricant additive and the lubricant of the present invention (i.e., the polyolefin of the present invention) can exhibit good lubrication performance.

[0089] As lubricant additives that can be used in the lubricant composition, the above substances can be cited. In addition, the lubricant composition may also contain the above-mentioned other base oils. The content of the lubricant of the present invention (i.e., the polyolefin of the present invention) in the lubricant composition is preferably 40 to 99.9% by mass, more preferably 70 to 99.9% by mass, and even more preferably 80 to 99.8% by mass relative to the entire lubricant composition.

[0090] In the lubricant composition, the lubricant additive and the lubricant of the present invention (ie, the polyolefin of the present invention), and any other base oil may be used alone or in combination of two or more.

[0091] (Plasticizers for electronic materials)

[0092] The polyolefin of the present invention is preferably used as a plasticizer for electronic materials. Therefore, the present invention also provides: a plasticizer for electronic materials composed of the polyolefin of the present invention. There is no particular limitation on the use of the plasticizer for electronic materials of the present invention. For example, the plasticizer for electronic materials of the present invention can be suitably used as a plasticizer for sealing materials for flexible electronic devices, semiconductors, etc. The plasticizer for electronic materials of the present invention can be used in combination with other components (for example, other plasticizers).

[0093] In particular, when the plasticizer for electronic materials of the present invention is used as the plasticizer for the sealing material, the precipitation of additives used together with the plasticizer can be suppressed, so that good plasticization can be exhibited even after temperature cycling at -20°C to 90°C. That is, the electronic material composition containing the electronic material and the polyolefin of the present invention can exhibit good plasticization.

[0094] The content of the electronic material plasticizer of the present invention (i.e., the polyolefin of the present invention) in the electronic material composition is preferably 1 to 50 parts by mass, more preferably 5 to 25 parts by mass, relative to 100 parts by mass of the electronic material. The electronic material composition may contain the electronic material and additives other than the electronic material plasticizer of the present invention.

[0095] As the electronic material, a thermoplastic resin is preferred, and a polyolefin obtained from an olefin monomer having 2 to 7 carbon atoms is preferred.

[0096] In the electronic material composition, the electronic material and the plasticizer for electronic material of the present invention (ie, the polyolefin of the present invention), and any additives may be used alone or in combination of two or more.

[0097] (Base for cosmetics)

[0098] The polyolefin of the present invention is preferably used as a cosmetic base. Therefore, the present invention also provides: a cosmetic base composed of the polyolefin of the present invention. The use of the cosmetic base of the present invention is not particularly limited, and the cosmetic base of the present invention can be suitably used as a cosmetic base having excellent transepidermal water loss inhibition effect and crystallization inhibition effect and less stickiness. The cosmetic base of the present invention can be used in combination with other ingredients (for example, other base materials, cosmetic additives).

[0099] Examples of cosmetics containing the cosmetic base of the present invention include creams (e.g., facial creams, body creams, sunscreens, moisturizing creams, hand creams, body creams, foot creams, and massage creams), lotions, foundations (e.g., liquid foundations), oily beauty serums, massage oils, hair oils, cleansing oils, sunscreens, spot makeup removers, treatments, mascara, and lipsticks.

[0100] In particular, the cosmetic containing the cosmetic base of the present invention exhibits good stability even after temperature cycling at -20°C to 40°C, and although it has a thick feel when applied, it does not feel sticky and can create a melting feeling as if it melts on the skin.

[0101] (cosmetic)

[0102] The present invention also provides cosmetics, wherein the cosmetic base of the present invention is included in an amount of 1 to 80% by mass relative to the whole cosmetics. That is, the present invention also provides cosmetics, wherein, relative to the whole cosmetics, 1 to 80% by mass of the cosmetic base of the present invention (i.e., the polyolefin of the present invention) and 20 to 99% by mass of other cosmetic ingredients are included. It should be noted that, in this specification, "other cosmetic ingredients" refer to cosmetic ingredients different from the cosmetic base of the present invention. When the content of the cosmetic base of the present invention is less than 1% by mass, its effect cannot be fully exerted. When the content of the cosmetic base of the present invention is higher than 80% by mass, the stability of the cosmetics may deteriorate. The content of the cosmetic base of the present invention relative to the whole cosmetics is preferably 1 to 50% by mass, more preferably 1 to 30% by mass.

[0103] Examples of cosmetics are as described above. Other cosmetic ingredients include, for example, solvents, oils and fats, higher fatty acids (e.g., fatty acids with 13 to 21 carbon atoms), higher alcohols, silicones, esters, surfactants, moisturizers, thickeners, antioxidants, stabilizers, preservatives, pearlescent agents, pH adjusters, ultraviolet absorbers, hydrotropes, pigments, dyes, bactericides, anti-inflammatory drugs, astringents, cooling agents, fragrances, plant extracts, etc. Examples of solvents include water, ethanol, 1,3-butylene glycol, dipropylene glycol, propylene glycol, glycerin, etc.

[0104] In the cosmetic of the present invention, other cosmetic ingredients and the cosmetic base of the present invention (ie, the polyolefin of the present invention) may be used alone or in combination of two or more.

[0105] Example

[0106] Hereinafter, the present invention will be described in detail with reference to Examples and Comparative Examples.

[0107] <Example 1: Synthesis of polyolefin 1>

[0108] A four-necked flask with an internal volume of 3 L was charged with 750 ml of heptane and 1.8 g of deionized water, and 35 mmol of aluminum chloride was supplied to 1 mol of 1-dodecene at 40°C. Thereafter, 1-dodecene was introduced at a flow rate of 0.4 L / hour until 375 ml was added while the reactor was maintained at 40°C. After 375 ml, the polymerization reaction was carried out while the reactor was maintained at 60°C and introduced at a flow rate of 0.4 L / hour. Next, the steps of adding 750 ml of a 20% by mass sodium hydroxide aqueous solution to the reaction solution to deactivate the Lewis acid catalyst and neutralize and wash were repeated twice at 80°C, and the organic layer was washed 6 times with 750 ml of deionized water. After desolventization and dehydration were carried out at 100°C and 6.7 kPa or less, adsorption treatment was carried out at 80°C using an adsorbent ("KW-700" and "KW-1000" manufactured by Kyowa Chemical Co., Ltd.), and polyolefin 1 was recovered. By 1 The ratio of side chains having carbon atoms of n-3 or less in the polyolefin 1 calculated by H-NMR and GPC was 28%.

[0109] <Example 2: Synthesis of polyolefin 2>

[0110] A four-necked flask with an internal volume of 3 L was charged with 750 ml of heptane and 0.9 g of deionized water, and 17.5 mmol of aluminum chloride was supplied to 1 mol of 1-decene at 10°C. After that, 1-decene was introduced at a flow rate of 0.3 L / hour until 375 ml was added while the temperature in the reactor was maintained at 10°C. After 375 ml, the temperature in the reactor was maintained at 20°C while the temperature was maintained at 0.6 L / hour, and a polymerization reaction was carried out. Next, the steps of adding 750 ml of a 20% by mass sodium hydroxide aqueous solution to the reaction solution to deactivate and neutralize the Lewis acid catalyst were repeated twice at 80°C, and the organic layer was washed 6 times with 750 ml of deionized water. After desolventization and dehydration were carried out at 100°C and 6.7 kPa or less, an adsorbent ("KW-700" and "KW-1000" manufactured by Kyowa Chemical Co., Ltd.) was used for adsorption treatment at 80°C to recover polyolefin 2. By 1 The ratio of side chains having carbon atoms of n-3 or less in the polyolefin 2 calculated by H-NMR and GPC was 11%.

[0111] <Example 3: Synthesis of polyolefin 3>

[0112] A four-necked flask with an internal volume of 3 L was charged with 750 ml of hexane and 1.8 g of deionized water, and 35 mmol of aluminum chloride was supplied to 1 mol of an olefin monomer mixture (1-decene (45 mass %) and 1-dodecene (55 mass %)) at 50° C. Thereafter, the olefin monomer mixture was fed at a flow rate of 0.2 L / hour until 300 ml was reached while the temperature in the reactor was maintained at 50° C., and after 300 ml, the polymerization reaction was carried out while the temperature in the reactor was maintained at 55° C. while the temperature was fed at a flow rate of 1 L / hour. Next, the steps of adding 750 ml of a 20 mass % sodium hydroxide aqueous solution to the reaction solution at 80° C. to deactivate the Lewis acid catalyst and neutralize and wash were repeated twice, and the organic layer was washed 6 times with 750 ml of deionized water, and the solvent and water were removed while reducing the pressure at 100° C. and 6.7 kPa or less. Then, an adsorption treatment was performed at 80° C. using an adsorbent ("KW-700" and "KW-1000" manufactured by Kyowa Chemical Co., Ltd.) to recover polyolefin 3. 1 The ratio of side chains having carbon atoms of n-3 or less in the polyolefin 3 calculated by H-NMR and GPC was 20%.

[0113] <Example 4: Synthesis of polyolefin 4>

[0114] A four-necked flask with an internal volume of 3 L was charged with 750 ml of heptane and 4.5 g of deionized water, and 35 mmol of aluminum chloride was supplied to 1 mol of 1-decene at 40°C. After that, 1-decene was introduced at a flow rate of 0.3 L / hour until 150 ml was reached while the temperature in the reactor was maintained at 40°C. After 150 ml, the temperature in the reactor was maintained at 40°C while the temperature was maintained at 0.4 L / hour, and a polymerization reaction was carried out. Next, the steps of adding 750 ml of a 20% by mass sodium hydroxide aqueous solution to the reaction solution to deactivate and neutralize the Lewis acid catalyst were repeated twice at 80°C, and the organic layer was washed 6 times with 750 ml of deionized water. After desolventization and dehydration were carried out at 100°C and 6.7 kPa or less, an adsorbent ("KW-700" and "KW-1000" manufactured by Kyowa Chemical Co., Ltd.) was used for adsorption treatment at 80°C to recover polyolefin 4. By 1 The ratio of side chains having carbon atoms of n-3 or less in the polyolefin 4 calculated by H-NMR and GPC was 25%.

[0115] <Example 5: Synthesis of polyolefin 5>

[0116] In a 5-liter (internal volume 4,890 ml) stainless steel pressure-resistant reactor, 1-tetradecene was introduced at a flow rate of 0.4 L / hour until 750 ml was added while the reactor was maintained at 80°C, and 74 mmol of boron trifluoride (BF3) was supplied at 40°C for each 1 mol of 1-tetradecene. Diethyl ether and ethanol were added so that the molar ratios relative to boron trifluoride were 1.00 and 0.03, respectively, and the polymerization reaction was carried out while maintaining the temperature at 40°C. Next, the steps of adding 750 ml of a 20% sodium hydroxide aqueous solution to the reaction solution to deactivate and neutralize the Lewis acid catalyst were repeated twice at 80°C, and the organic layer was washed 6 times with 750 ml of deionized water. After desolventization and dehydration were carried out at 100°C and a reduced pressure of less than 6.7 kPa, adsorption treatment was carried out at 80°C using an adsorbent ("KW-700" and "KW-1000" manufactured by Kyowa Chemical Co., Ltd.) to recover polyolefin 5. By 1 The ratio of side chains having carbon atoms of n-3 or less in the polyolefin 5 calculated by H-NMR and GPC was 38%.

[0117] <Comparative Example 1: Synthesis of polyolefin C1>

[0118] Into a four-necked flask with an internal volume of 5 L, 750 ml of ethylene dichloride and 1.8 g of deionized water were placed, and 74 mmol of aluminum chloride was added to 1 mol of 1-decene at 15°C. After that, 7500 ml of 1-decene was inserted at a flow rate of 0.4 L / hour, and a polymerization reaction was carried out at a reaction temperature of 50°C. Next, the steps of adding 750 ml of a 20% by mass sodium hydroxide aqueous solution to the reaction solution to deactivate and neutralize the Lewis acid catalyst were repeated twice at 80°C, and then the organic layer was washed 6 times with 750 ml of deionized water. After desolventization and dehydration were carried out at 100°C and 6.7 kPa or less, an adsorbent ("KW-700" and "KW-1000" manufactured by Kyowa Chemical Co., Ltd.) was used for adsorption treatment at 80°C to recover polyolefin C1. By 1 The ratio of side chains having carbon atoms of n-3 or less in the polyolefin C1 calculated by H-NMR and GPC was 31%.

[0119] <Comparative Example 2: Synthesis of polyolefin C2>

[0120] Into a four-necked flask with an internal volume of 5 L, 325 ml of heptane and 1.8 g of deionized water were placed, and 74 mmol of aluminum chloride was added to 1 mol of 1-decene at 15°C. After that, 325 ml of 1-decene was inserted at a flow rate of 0.4 L / hour, and a polymerization reaction was carried out at a reaction temperature of 130°C. Next, the steps of adding 325 ml of a 20 mass % sodium hydroxide aqueous solution to the reaction solution to deactivate and neutralize the Lewis acid catalyst were repeated twice at 80°C, and then the organic layer was washed 6 times with 325 ml of deionized water. After desolventization and dehydration were carried out at 100°C and a pressure reduction of less than 6.7 kPa, an adsorbent ("KW-700" and "KW-1000" manufactured by Kyowa Chemical Co., Ltd.) was used for adsorption treatment at 80°C to recover polyolefin C2. By 1 The ratio of side chains having carbon atoms of n-3 or less in the polyolefin C2 calculated by H-NMR and GPC was 52%.

[0121] The number average molecular weight of each polyolefin obtained in Examples 1 to 5 and Comparative Examples 1 and 2 was measured by gel permeation chromatography (GPC).

[0122] Table 1 shows the olefin monomers used in Examples 1 to 5 and Comparative Examples 1 and 2, and the number average molecular weight and the ratio of side chains having a carbon number of n-3 or less of the obtained polyolefins.

[0123]

[0124] <Evaluation of properties as a plasticizer for electronic materials>

[0125] The properties (plasticizing properties) of the polyolefins obtained in Examples 1 to 5 and Comparative Example 1 or 2 as plasticizers for electronic materials were evaluated by the following method.

[0126] Evaluation of plasticity

[0127] A mixture of 10 g of a toluene solution of polybutene (polybutene concentration: 30% by mass), 0.3 g of polyolefin (plasticizer for electronic materials) (amount relative to polybutene: 10% by mass), and 0.015 g of oleic acid (amount relative to polybutene: 0.5% by mass) was prepared. It should be noted that the above "amount of each component relative to polybutene" is calculated by the formula "100×amount of each component used (g) / amount of polybutene used (g)".

[0128] The prepared mixture was coated on a polyethylene terephthalate (PET) film at a speed of 50 mm / sec using an automatic coating device, dried at 60°C for 5 minutes, and then left to stand at room temperature overnight to produce a thin sheet with a film thickness of about 30 μm. After the produced thin sheet was stored in a storage warehouse at -20°C for 12 hours and then stored in a storage warehouse at 90°C for 12 hours, such a temperature cycle (1 cycle: 1 day) was repeated for 30 cycles (30 days), the thin sheet was cut off and a dumbbell-shaped test piece (JISK6251-1) was produced. The elongation of the dumbbell-shaped test piece was measured by a tensile test using a tensile testing machine. Using the obtained elongation, the plasticization of the polyolefin was evaluated according to the following criteria. Polyolefins evaluated as "○" or "◎" were judged to be plasticizers with excellent plasticization.

[0129] (Benchmark)

[0130] ◎: Elongation is more than 120%;

[0131] ○: Elongation is 110% or more and less than 120%;

[0132] △: Elongation is less than 110%.

[0133]

[0134] As shown in Table 2, compared with the polyolefins C1 and C2 obtained in Comparative Examples 1 and 2, the polyolefins 1 to 5 obtained in Examples 1 to 5 were superior in plasticity even after temperature cycling at -20°C to 90°C.

[0135] <Evaluation of properties as a base for cosmetics>

[0136] The properties of the polyolefins obtained in Examples 1 to 5 and Comparative Example 1 or 2 as a cosmetic base (transepidermal water loss inhibition effect, stickiness, and crystallization inhibition effect) were evaluated by the following methods. The results are shown in Table 3.

[0137] Evaluation of the effect of inhibiting transepidermal water loss

[0138] Ten women (aged 22 to 40) were selected as panelists to measure the transepidermal water loss before and after applying polyolefin (cosmetic base) on the inner side of the forearm using an evaporator EP1 (manufactured by Yayoi Co., Ltd.). The rate of change in transepidermal water loss was calculated using the following formula:

[0139] The change rate of transepidermal water loss (%) = [(transepidermal water loss after polyolefin application - transepidermal water loss before polyolefin application) / transepidermal water loss before polyolefin application] × 100.

[0140] In order to stabilize the body temperature, the panelists were asked to stand in a constant temperature and humidity room at 25°C and 40% humidity for more than 30 minutes, and then the transepidermal water loss was measured in the constant temperature and humidity room.

[0141] The average value of the transepidermal water loss change rate of all the panelists was calculated for each polyolefin, and the transepidermal water loss suppressing effect was evaluated according to the following criteria: The smaller the average value, the better the transepidermal water loss suppressing effect.

[0142] (Benchmark)

[0143] ◎: The above average value is less than -15%;

[0144] ○: The above average value is -15% or more and less than -5%;

[0145] △: The above average value is -5% or more and less than 0%;

[0146] ×: The above average value is 0% or more.

[0147] Evaluation of stickiness

[0148] Twenty female panelists (22 to 40 years old) were used to evaluate the stickiness of the obtained polyolefin (cosmetic base, about 1 g) after blending it into the skin according to the following scoring and criteria. Polyolefins rated "○" or "◎" were judged to be cosmetic bases without stickiness.

[0149] (score)

[0150] 2 points: After blending into the skin, there is no sticky feeling;

[0151] 1 point: After blending into the skin, it feels slightly sticky;

[0152] 0 points: After blending into the skin, it feels sticky.

[0153] (Benchmark)

[0154] ◎: The total score is 35 points or more;

[0155] ○: The total score is 30 points or more and 34 points or less;

[0156] △: The total score is 20 points or more and 29 points or less;

[0157] ×: The total score is 19 points or less.

[0158] Evaluation of crystallization inhibition effect

[0159] 0.1 g of palmitic acid was added to 50 g of each polyolefin, and the mixture was thoroughly mixed and stirred. The mixture was then placed in a glass container and sealed. The container was stored in a storage room at 50°C for 12 hours and then in a storage room at -20°C for 12 hours. This temperature cycle (1 cycle: 1 day) was repeated 30 times (30 days), and the crystallization inhibition effect was evaluated according to the following criteria.

[0160] (Benchmark)

[0161] ◎: Crystallization of the mixture is suppressed at -20°C, and the mixture has fluidity;

[0162] ○: Crystallization of the mixture was slightly suppressed at -20°C, and the mixture had a slight fluidity;

[0163] ×: The mixture was crystallized at -20°C and had no fluidity at all.

[0164]

[0165] As shown in Table 3, Polyolefins 1 to 5 were excellent in the transepidermal water loss suppressing effect and the crystallization suppressing effect and had no sticky feeling.

[0166] On the other hand, polyolefin C1 or C2 is inferior in the transepidermal water loss suppressing effect, the absence of stickiness, and the crystallization suppressing effect.

[0167] <Evaluation of properties as a lubricant>

[0168] The lubricant properties (lubricity) of the polyolefins obtained in Examples 1 to 5 and Comparative Example 1 or 2 were evaluated by the following method.

[0169] Preparation of lubricant composition

[0170] 0.1 g of palmitic acid (lubricant additive) was added to 50 g of each polyolefin (lubricant), and the mixture was sufficiently mixed and stirred to completely dissolve the palmitic acid, thereby preparing a lubricant composition.

[0171] Evaluation of lubricity before cycle testing

[0172] Each lubricant composition was placed on a metal disk (SUJ-2), and the static friction coefficient and dynamic friction coefficient before the cycle test were measured using a Bowden tester under the following conditions, and the respective average values ​​were calculated to evaluate the lubricity according to the following criteria. The lower the average value, the better the lubricity.

[0173] (condition)

[0174] Contact (steel ball, diameter 3mm);

[0175] Load: 500g;

[0176] Temperature: 25℃;

[0177] Speed: 2.5mm / sec;

[0178] Measuring distance: 10mm;

[0179] Number of trials: 100.

[0180] (Benchmark)

[0181] ◎: The average value of the static friction coefficient or the dynamic friction coefficient is less than 0.100;

[0182] ○: The average value of the static friction coefficient or the dynamic friction coefficient is 0.100 or more and less than 0.150;

[0183] △: The average value of the static friction coefficient or the dynamic friction coefficient is 0.150 or more and less than 0.200;

[0184] ×: The average value of the static friction coefficient or the dynamic friction coefficient is 0.200 or more.

[0185] Evaluation of crystallization inhibition effect

[0186] 50 g of each lubricant composition was placed in a sealed glass container, and the container was stored in a 90°C storage room for 12 hours and then stored in a -20°C storage room for 12 hours. After repeating 30 cycles (30 days) of temperature cycling (1 cycle: 1 day), the crystallization suppression effect was evaluated according to the following criteria.

[0187] (Benchmark)

[0188] ◎: Crystallization of the lubricant composition is suppressed at -20°C, and the lubricant composition has fluidity;

[0189] ○: Crystallization of the lubricant composition is slightly suppressed at -20°C, and the lubricant composition has a slight fluidity;

[0190] ×: The lubricant composition was crystallized at -20°C and had no fluidity at all.

[0191] Evaluation of lubricity after cycle test

[0192] After the cycle test, the lubricant composition was left to stand until the temperature reached 25°C, and the static friction coefficient and dynamic friction coefficient after the cycle test were measured in the same manner as the lubricity evaluation before the cycle test, and the average values ​​of each were calculated to evaluate the lubricity according to the above criteria. The lower the average value, the better the lubricity.

[0193]

[0194] As shown in Table 4, compared with the polyolefins C1 and C2 obtained in Comparative Examples 1 and 2, the polyolefins 1 to 5 obtained in Examples 1 to 5 were superior in lubricity and crystallization suppression effect.

[0195] <Examples 6 to 12, Comparative Examples 3 and 4: Production of Cosmetics>

[0196] The polyolefin (cosmetic base) obtained in Examples 1 to 5 and Comparative Example 1 or 2 and general additives (wax solid at room temperature, etc.) were mixed in the amounts shown in Table 5 to produce cosmetics. The obtained cosmetics were evaluated by the following method. The results are shown in Table 5. In addition, the composition of general additives is shown in Table 6.

[0197] Evaluation of temperature cycle stability

[0198] 50 g of the obtained cosmetic was placed in a sealed glass container, and a temperature cycle of storing in a 50°C storage room for 12 hours and then storing in a -20°C storage room for 12 hours was repeated (1 cycle: 1 day), and evaluated according to the following criteria.

[0199] (Benchmark)

[0200] ◎: The appearance and properties of the cosmetics did not change significantly after 28 cycles;

[0201] ○: Although the appearance and properties of the cosmetics changed slightly after 28 cycles, there was no significant change in the appearance and properties of the cosmetics after 14 cycles;

[0202] △: Although the appearance and properties of the cosmetics changed slightly after 14 cycles, there was no significant change in the appearance and properties of the cosmetics after 7 cycles;

[0203] ×: The appearance and properties of the cosmetics changed significantly after 7 cycles.

[0204] Evaluation of the thick feeling when applied

[0205] Twenty females (22 to 40 years old) were selected as panelists to evaluate the thick feeling of the obtained cosmetics (about 1 g) when applied to the skin according to the following scoring and criteria. Cosmetics rated "○" or "◎" were judged to have a thick feeling when applied.

[0206] (score)

[0207] 2 points: When applied to the skin, it feels thick and thick;

[0208] 1 point: When applied to the skin, it feels slightly thick;

[0209] 0 points: No thick feeling when applied on the skin.

[0210] (Benchmark)

[0211] ◎: The total score is 35 points or more;

[0212] ○: The total score is 30 points or more and 34 points or less;

[0213] △: The total score is 20 points or more and 29 points or less;

[0214] ×: The total score is 19 points or less.

[0215] Evaluation of the melting feeling on the skin

[0216] Twenty females (22 to 40 years old) were selected as panelists to evaluate the melting sensation on the skin when the obtained cosmetics (about 1 g) were applied to the skin and blended in according to the following scoring and criteria. Cosmetics evaluated as "○" or "◎" were judged to have a melting sensation on the skin.

[0217] (score)

[0218] 2 points: When applied to the skin and blended, it feels like melting on the skin;

[0219] 1 point: When applied to the skin and blended, the skin feels slightly melted;

[0220] 0 points: When applied and blended, there is no melting feeling on the skin.

[0221] (Benchmark)

[0222] ◎: The total score is 35 points or more;

[0223] ○: The total score is 30 points or more and 34 points or less;

[0224] △: The total score is 20 points or more and 29 points or less;

[0225] ×: The total score is 19 points or less.

[0226] Evaluation of stickiness

[0227] Twenty female panelists (aged 22 to 40) applied the obtained cosmetics (about 1 g) to the skin and blended them, and then evaluated the stickiness according to the following scoring and criteria. Cosmetics rated "○" or "◎" were judged to be cosmetics without stickiness.

[0228] (score)

[0229] 2 points: After applying to the skin and blending it, there is no sticky feeling;

[0230] 1 point: After applying it on the skin and blending it, it feels slightly sticky;

[0231] 0 points: After applying and blending into the skin, it feels sticky.

[0232] (Benchmark)

[0233] ◎: The total score is 35 points or more;

[0234] ○: The total score is 30 points or more and 34 points or less;

[0235] △: The total score is 20 points or more and 29 points or less;

[0236] ×: The total score is 19 points or less.

[0237]

[0238] [Table 6]

[0239]

[0240] As shown in Table 5, the cosmetics of Examples 6 to 12 containing polyolefins 1 to 5 (cosmetic base materials) and a large amount of general-purpose additives (waxes that are solid at room temperature, etc.) showed good stability even under severe conditions such as a temperature cycle of -20°C to 50°C, which assumes the temperature of a bathroom in winter. In addition, the cosmetics of Examples 6 to 12 were excellent in a thick feeling and a melting feeling on the skin when applied, and had no sticky feeling.

[0241] On the other hand, the cosmetics of Comparative Example 3 or 4 containing polyolefin C1 or C2 were inferior in temperature cycle stability, melting feeling on the skin, and stickiness.

[0242] <Example 13: Production of emulsion>

[0243] Each component was mixed according to the composition described in Table 6 below to obtain an emulsion (cosmetics).

[0244] [Table 7]

[0245] Example 13: Emulsion

[0246]

[0247]

[0248] "%" = "mass %"

[0249] <Example 14: Production of cream>

[0250] By mixing the components according to the composition described in Table 8 below, a cream (cosmetics) was obtained.

[0251] [Table 8]

[0252] Example 14: Cream

[0253] composition Polyolefin 2 (Example 2) 3% (C9-12)Alkanes 2% Squalane 2% Olive Oil 2% Ethylhexyl palmitate 2% glycerin 5% Propylene glycol 3% 1,3-Butanediol 2% Cetyl Alcohol 2% Docosanol 2% beeswax 1% Polyglyceryl-5-laurate 3% PEG / PPG / polybutylene glycol-8 / 5 / 3 glycerol 0.5% Polyquaternium-51 0.1% Sodium hyaluronate (1% aqueous solution) 0.01% Tocopherol 0.05% Niacinamide 3% Phenoxyethanol 0.2% Ethylhexylglycerin 0.1% Citric Acid Moderate Sodium Citrate Moderate water margin total 100%

[0254] "%" = "mass %"

[0255] <Example 15: Production of sunscreen>

[0256] The components were mixed according to the composition described in Table 9 below to obtain a sunscreen (cosmetics).

[0257] [Table 9]

[0258] Example 15: Sunscreen

[0259] composition Polyolefin 2 (Example 2) 3% (C9-12)Alkanes 2% Squalane 2% Dimethicone 1% Olive Oil 2% Ethylhexyl palmitate 2% Disteardimethylammonium hectorite 2% Acrylates / C10-30 Alkyl Acrylate Crosspolymer 0.1% Hydrogenated polyisobutylene 5% Titanium oxide 6% Zinc Oxide 5% Octyl Methoxycinnamate 2.8% Diethylamino Hydroxybenzoyl Hexyl Benzoate 2.2% PEG / PPG / polybutylene glycol-8 / 5 / 3 glycerol 0.5% Polyquaternium-51 0.1% glycerin 5% 1,3-Butanediol 2% Sodium hyaluronate (1% aqueous solution) 0.01% Phenoxyethanol 0.2% Ethylhexylglycerin 0.1% Arginine Moderate water margin total 100%

[0260] "%" = "mass %"

[0261] <Example 16: Production of topical makeup remover>

[0262] The components were mixed according to the composition described in Table 10 below to obtain a topical cleansing cream (cosmetics).

[0263] [Table 10]

[0264] Example 16: Local makeup remover

[0265]

[0266]

[0267] "%" = "mass %"

[0268] <Example 17: Production of makeup remover oil>

[0269] The components were mixed according to the composition described in Table 11 below to obtain a cleansing oil (cosmetics).

[0270] [Table 11]

[0271] Example 17: Makeup remover oil

[0272] composition Polyolefin 2 (Example 2) 2% (C9-12)Alkanes 18% Cetyl Ethylhexanoate 20% Squalane 5% Olive Oil 10% Sorbitol Tetraisostearate 15% Polyglyceryl-10 Diisostearate 6% Sorbitan oleate 4% Glyceryl Laurate 3% Polysorbate 20 7% Ethyl oleate 6% Tocopherol 0.05% spices 0.3% water margin total 100%

[0273] "%" = "mass %"

[0274] <Example 18: Production of hair oil>

[0275] The respective components were mixed according to the composition described in Table 12 below to obtain a hair oil (cosmetic product).

[0276] [Table 12]

[0277] Example 18: Hair Oil

[0278] composition Polyolefin 2 (Example 2) 5% (C9-12)Alkanes 10% (C13-15)Alkanes 10% Dimethicone 65% Olive Oil 10% AMINOPROPYL DIMETHICONE 5% Tocopherol 0.05% spices 0.3% water margin total 100%

[0279] "%" = "mass %"

[0280] <Example 19: Production of Hair Cream>

[0281] The respective components were mixed according to the composition described in Table 13 below to obtain a hair treatment cream (cosmetics).

[0282] [Table 13]

[0283] Example 19: Hair Treatment Cream

[0284]

[0285]

[0286] "%" = "mass %"

[0287] <Example 20: Production of Mascara>

[0288] By mixing the components according to the composition described in Table 14 below, a mascara was obtained.

[0289] [Table 14]

[0290] Example 20: Mascara

[0291] composition Polyolefin 2 (Example 2) 3% (C13-15)Alkanes 20% Iron Oxide 15% Microcrystalline wax 10% Candelilla wax 1.5% Ethanol 1% talc 1% Trimethylsiloxysilicate 10% Disteardimethylammonium hectorite 2% Dextrin palmitate 1% Propylparaben 0.05% Tocopherol 0.05% Hydrogenated polyisobutylene margin total 100%

[0292] "%" = "mass %"

[0293] <Example 21: Production of liquid foundation>

[0294] By mixing the components according to the composition described in Table 15 below, a liquid foundation (cosmetics) was obtained.

[0295] [Table 15]

[0296] Example 21: Liquid foundation

[0297]

[0298]

[0299] "%" = "mass %"

[0300] <Example 22: Production of lipstick>

[0301] The components were mixed according to the composition described in Table 16 below to obtain lipstick (cosmetics).

[0302] [Table 16]

[0303] Example 22: Lipstick

[0304] composition Polyolefin 2 (Example 2) 5% (C13-15)Alkanes 2% Hydrogenated polyisobutylene margin castor oil 5% Jojoba Oil 5% olive oil 5% Carnauba wax 2% Polyethylene wax 9% Silicone resin 18% Dimethyl polysiloxane (SH100) 5% Aluminum hydroxide Moderate Red No. 201 1% Titanium oxide 2% Pearlescent Pigments 5% total 100%

[0305] "%" = "mass %"

[0306] Industrial Applicability

[0307] The polyolefin of the present invention can be used as a plasticizer for electronic materials, a base for cosmetics, a lubricant, and the like.

[0308] This application is based on Japanese Patent Application No. 2022-066549 filed in Japan, the entire contents of which are incorporated herein by reference.

Claims

1. A polyolefin obtained from a linear olefin monomer having 8 to 20 carbon atoms and having a number average molecular weight of 250 to 10,000, The side chain ratio of carbon atoms n-3 or less calculated by formula (1) is 1 to 40%. The side chain ratio of carbon atoms n-3 or less (%) = [Nx / (Nx+Ny)×2n-3] / 3×100···(1) In formula (1), n represents the average number of carbon atoms of the above olefin monomers, Nx represents the 1 The integrated value of the signal at 0.75 to 0.95 ppm detected in the H-NMR measurement, and Ny represents 1 The integrated value of the signal at 1.00 to 1.45 ppm detected in H-NMR measurement.

2. The method for producing a polyolefin according to claim 1, comprising: A linear olefin monomer having 8 to 20 carbon atoms is polymerized in the presence of a Lewis acid catalyst.

3. A plasticizer for electronic materials, comprising the polyolefin according to claim 1.

4. A cosmetic base comprising the polyolefin according to claim 1.

5. A cosmetic comprising the cosmetic base according to claim 4 in an amount of 1 to 80% by mass based on the entire cosmetic.

6. A lubricant consisting of the polyolefin according to claim 1.

Citation Information

Cited By

  • Synergistic thickening moisturizing composition and application thereof in cosmetics

    CN121196956A